A method for preparing diamond based on graphite under normal pressure

By depositing tantalum atoms using an HFCVD system under normal pressure and performing annealing treatment, the high-temperature, high-pressure, and high-power problems associated with the existing graphite diamond preparation method are solved, enabling the preparation of large-size, large-quantity diamonds and reducing costs and equipment. requirements, improving production efficiency.

CN116282002BActive Publication Date: 2024-10-18ZHEJIANG UNIV OF TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310059001.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-18
Publication Date
2024-10-18
Estimated Expiration
2043-01-18

AI Technical Summary

Technical Problem

The existing high-temperature and high-pressure method and detonation method used to prepare diamond from graphite have harsh production conditions, high equipment requirements, high cost and low production efficiency. Moreover, the chemical vapor deposition method has high power and low growth rate, making it difficult to obtain large-size, multi-layer diamond. number of diamond particles.

Method used

The HFCVD system is used to deposit the monodispersed tantalum atoms escaped from the metal tantalum wire onto the graphite surface under normal pressure, and the transformation of graphite into diamond is achieved through annealing treatment, which reduces the power and time of tantalum wire processing and reduces the generation of TaC. Promotes the phase transformation of graphite under normal pressure.

Benefits of technology

It realizes the preparation of large-sized and large-number diamond particles under normal pressure, reduces the preparation cost, simplifies the process, improves production efficiency, and has low equipment requirements and relatively simple operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004060944890000011
    Figure HDA0004060944890000011
  • Figure HDA0004060944890000012
    Figure HDA0004060944890000012
  • Figure HDA0004060944890000021
    Figure HDA0004060944890000021
Patent Text Reader

Abstract

The present invention provides a method for preparing diamond based on graphite under normal pressure, wherein metal tantalum atoms released when a tantalum wire in an HFCVD system is heated are deposited on a graphite sheet, thereby converting graphite into diamond under normal pressure, and the method has the advantages of low cost, energy saving and environmental protection; the method has low requirements on equipment, simple process and easy operation.
Need to check novelty before this filing date? Find Prior Art

Description

(I) Technical field

[0001] The invention relates to a new method for preparing diamond based on graphite under normal pressure. (II) Background technology

[0002] Diamond has extremely excellent physical and chemical properties, such as high hardness, high thermal conductivity, wide bandgap, strong chemical corrosion resistance, etc., and has extremely broad application prospects in industrial processing, electronic devices, electrochemical electrodes, etc. In particular, as a typical representative of wide bandgap semiconductor materials, diamond is considered to be the most promising material for preparing the next generation of high-power, high-frequency, high-temperature and low-power loss electronic devices, which has a significant impact on the future comprehensive national strength and national defense security.

[0003] Graphite, also a carbon material, is the most commonly used raw material for preparing diamonds. At present, the high temperature and high pressure method and the detonation method are commonly used in the industry to prepare diamonds from graphite. The high temperature and high pressure method completely simulates the natural mechanism of natural diamond growth underground. It generally requires pressure and temperature above 10GPa and 3000℃ to allow the carbon atoms in graphite to recombine into the structure of diamond. The single diamond particles prepared by this method are relatively small in size. The detonation method uses the instantaneous high temperature and high pressure environment generated by the explosion of high explosives to produce nano diamond particles. The nano diamonds obtained by this method have a large output, but the diamond particles are small in size and mixed with the raw materials, making post-processing very difficult and the purification process very complicated. The production conditions of these two methods are extremely harsh. The pressure required for phase change is as high as several thousand megapascals or even higher, and the temperature conditions are also as high as several thousand degrees Celsius. The equipment requirements are extremely high, and the production efficiency is low, the preparation cost is high, and the difficulty is great. Some researchers also use the chemical vapor deposition (CVD) method to prepare diamonds with graphite as a solid carbon source instead of gaseous carbon sources such as methane and acetone. However, this method requires high power and low diamond growth rate. Therefore, it is of great value to develop new methods for preparing diamond based on graphite.

[0004] The inventor previously used an HFCVD system to deposit the Ta atoms that escaped from the tantalum wire onto a graphite substrate, and then combined it with vacuum annealing to convert graphite into diamond at low pressure (see patent 202210305804.7). In this patent, the HFCVD system was used to treat the graphite substrate with Ta wire at powers of 2000W and 2200W, respectively. The selected tantalum wire had a higher power and a longer treatment time. The Ta atoms reacted with the carbon in the graphite sheet to generate a large amount of TaC, resulting in a reduction in the number of monodisperse Ta atoms, which limited the phase transformation of graphite into diamond. Therefore, in this patent, the inventor reduced the power and treatment time of the Ta wire treatment, optimized the annealing process, reduced the generation of TaC, obtained more monodisperse Ta atoms, and promoted the graphite / diamond phase transition under normal pressure caused by monodisperse Ta atoms, so as to obtain larger size and more diamonds. (III) Summary of the invention

[0005] The present invention develops a new method for preparing diamond from graphite under normal pressure. The method uses a HFCVD system to deposit monodisperse tantalum atoms released from metal tantalum wire onto the graphite surface at a relatively low power, and then performs annealing treatment to achieve the transformation of graphite into diamond under normal pressure.

[0006] To achieve the above object, the present invention adopts the following technical solution:

[0007] The present invention provides a method for preparing diamond based on graphite under normal pressure, the method comprising the following steps:

[0008] (1) Pretreatment of graphite sheets: The graphite sheets (prepared by Beijing Electric Carbon Factory, purity 99.9%) were successively ground (using 2000 mesh and 4000 mesh sandpaper), polished (using polishing flannel), ultrasonically cleaned in an organic solvent, cleaned with deionized water, and dried (dried with a nitrogen gun) to obtain pretreated graphite sheets; the above pretreatment is to obtain graphite sheets with a smooth and clean surface;

[0009] (2) Ta wire treatment: the pretreated graphite sheet in step (1) is placed as a substrate in a hot wire chemical vapor deposition (HFCVD) device for tantalum deposition (no carbon source is required, and chemical vapor deposition is not performed, but the Ta wire in the device is used as a heat source and a tantalum source), the pretreated graphite sheet is located directly below the tantalum wire, the hydrogen flow rate is adjusted to 10-350 sccm (preferably 100 sccm), the power is controlled to 300-800 W (preferably 400 W), and the gas pressure is 3-5 kPa (preferably 3.5 kPa). After treating for 1-60 min (preferably 5 min-15 min, more preferably 15 min), the power is reduced to 0 at a rate of 1 V / min in a hydrogen atmosphere to obtain a graphite sheet treated with Ta wire;

[0010] (3) Annealing: The graphite sheet treated with Ta wire in step (2) is sealed in a quartz tube and placed in a muffle furnace for annealing at 400-1300° C. for 10-180 min (preferably 500-1200° C. for 30-120 min, more preferably 1100° C. for 120 min) to obtain diamond.

[0011] Furthermore, the graphite sheet in step (1) is a polycrystalline graphite sheet with a size of 10×10×2 mm and a purity of 99.9%. Furthermore, the organic solvent in step (1) is ethanol or acetone, preferably ethanol.

[0012] In the step (1) of the embodiment of the present invention, the ultrasonic cleaning equipment is manufactured by Kunshan Ultrasonic Instrument Co., Ltd., model KQ5200DE, and the condition is 100W-200W ultrasound for 15 minutes, preferably 140W.

[0013] Preferably, the hot wire chemical vapor deposition equipment in step (2) is purchased from Shanghai Jiaoyou Diamond Coating Company, model number JUHFCVD001.

[0014] Compared with the existing process of converting graphite into diamond under high temperature and high pressure, the beneficial effects of the present invention are reflected in: (1) the metallic tantalum atoms escaped when the tantalum wire in the HFCVD system is heated are deposited on the graphite sheet, and the graphite is converted into diamond under normal pressure, which has the advantages of low cost, energy saving and environmental protection; (2) this method has low equipment requirements, simple process and easy operation; (3) compared with the inventor's previous process of converting graphite into diamond under low pressure (see patent 202210305804.7), the process of the present invention is simpler and has a shorter cycle, while obtaining a larger number and larger size of diamonds, providing a more feasible solution for the preparation of diamond based on phase change of graphite at normal pressure. (IV) Description of the drawings

[0015] Figure 1 This is a scanning electron microscope (SEM) image of the intrinsic graphite substrate after pretreatment.

[0016] Figure 2 This is a transmission electron microscope (TEM) image of the intrinsic graphite substrate after pretreatment.

[0017] Figure 3 SEM image of Example 1 (power 400 W - tantalum wire treatment 15 min - 500° C. annealing - 30 min).

[0018] Figure 4 TEM image of Example 1 (400W-15min-500℃-30min).

[0019] Figure 5 SEM image of Example 2 (400W-15min-1100℃-30min).

[0020] Figure 6 TEM image of Example 2 (400W-15min-1100℃-30min).

[0021] Figure 7 SEM image of Example 3 (400W-15min-1100℃-120min).

[0022] Figure 8TEM image of Example 3 (400W-15min-1100℃-120min).

[0023] Fig. 9 SEM image of Example 4 (400W-15min-1200℃-30min).

[0024] Fig.10 TEM image of Example 4 (400W-15min-1200℃-30min).

[0025] Fig.11 SEM image of Example 5 (400W-5min-1100℃-30min).

[0026] Fig.12 TEM image of Example 5 (400 W-5 min-1100°C-30 min). (V) Specific implementation methods

[0027] The present invention is further described below by means of specific embodiments, but the protection scope of the present invention is not limited thereto.

[0028] Example 1

[0029] (1) A graphite sheet (prepared by Beijing Electric Carbon Factory, purity 99.9%) was ground (using 2000 mesh and 4000 mesh sandpaper successively), polished (using polishing flannel cloth), ultrasonically cleaned in ethanol (manufactured by Kunshan Ultrasonic Instrument Co., Ltd., model KQ5200DE, 140W ultrasonic for 15 minutes), cleaned with deionized water, and dried (dried with a nitrogen gun) to obtain a pretreated graphite sheet; the above pretreatment is to obtain a graphite sheet with a smooth and clean surface.

[0030] (2) The tantalum wire is tooled in the form of a double spiral. The graphite sheet pretreated in step (1) is placed in a hot wire chemical vapor deposition (HFCVD) device, and hydrogen is introduced at a flow rate of 100 sccm and a power of 400 W. The gas pressure is controlled to be stable at 3.5 kPa. After 15 minutes of treatment, the power is reduced to 0 at a rate of 1 V / min in a hydrogen atmosphere to complete the Ta deposition process.

[0031] (3) placing the graphite sheet treated in step (2) into a quartz tube and sealing the tube, placing the sealed quartz tube (with the sample inside) into a muffle furnace at 500° C., taking out the sample after annealing for 30 minutes, and completing the annealing process.

[0032] Field emission scanning electron microscopy (FESEM) and high resolution transmission electron microscopy (HRTEM) were used to observe the composition of the samples after the experiment.

[0033] Figure 1This is the SEM picture of the intrinsic graphite substrate after pretreatment. The graphite surface is very smooth after treatment.

[0034] Figure 2 This is a TEM image of the intrinsic graphite substrate after pretreatment, which mainly shows the crystal plane information of graphite (002)(100) etc.

[0035] Figure 3 This is the SEM picture of Example 1. After annealing, there are fewer nanoparticles on the surface of the sample.

[0036] Figure 4 This is the TEM image of Example 1. From the low-magnification image, it can be seen that there are a small amount of black nanoparticles on the thin area of ​​the sample. SAED-a mainly contains diffraction rings of the (002), (100), (101) and (110) crystal planes of graphite. Figure (b) shows a high-magnification image of the nanoparticles. In Figure (b), there is a granular area with clear lattice fringes inside the particles. The interplanar spacing is 0.210nm, which is the (111) plane of cubic diamond. The enlarged image (c) of particle c shows that there are lattice fringes with a spacing of 0.212nm inside the particles, which is close to the interplanar spacing of the (111) plane of cubic diamond. There are also lattice fringes of the (002) plane of graphite outside the particles. The previous analysis shows that there are nanodiamond particles of about 8-12nm in the sample.

[0037] Example 2

[0038] (1) A graphite sheet (prepared by Beijing Electric Carbon Factory, purity 99.9%) was ground (using 2000 mesh and 4000 mesh sandpaper successively), polished (using polishing flannel cloth), ultrasonically cleaned in ethanol (manufactured by Kunshan Ultrasonic Instrument Co., Ltd., model KQ5200DE, 140W ultrasonic for 15 minutes), cleaned with deionized water, and dried (dried with a nitrogen gun) to obtain a pretreated graphite sheet; the above pretreatment is to obtain a graphite sheet with a smooth and clean surface.

[0039] (2) The tantalum wire is tooled in the form of a double spiral. The graphite sheet pretreated in step (1) is placed in a hot wire chemical vapor deposition device, and hydrogen is introduced at a flow rate of 100 sccm and a power of 400 W. The gas pressure is controlled to be stable at 3.5 kPa. After 15 minutes of treatment, the power is reduced to 0 at a rate of 1 V / min in a hydrogen atmosphere to complete the Ta deposition process.

[0040] (3) placing the graphite sheet treated in step (2) into a quartz tube and sealing the tube, placing the sealed quartz tube (with the sample inside) into a muffle furnace at 1100° C., taking out the sample after annealing for 30 minutes, and completing the annealing process.

[0041] Field emission scanning electron microscopy (FESEM) and high resolution transmission electron microscopy (HRTEM) were used to observe the composition of the samples after the experiment.

[0042] Figure 5 This is the SEM picture of Example 2. After annealing, many spherical nanoparticles are generated on the surface of the sample. Compared with annealing at 500°C (Example 1), the number of nanoparticles on the surface of the sample increases significantly and the size becomes larger.

[0043] Figure 6 This is the TEM image of Example 2. From the low-magnification image, it can be seen that there are many nano-spherical particles in the thin area of ​​the sample. SAED-a mainly contains diffraction rings of the (002), (100) and (101) crystal planes of graphite. Figure (b) shows a high-magnification image of the nanoparticles. There are two pairs of diffraction points in FT-b corresponding to the positions of the two particles in Figure (b). The enlarged image b-1 of particle 1 shows that there are clear lattice fringes inside the particle, and the crystal plane spacing is 0.210nm, which is the (111) plane of cubic diamond. The enlarged image of particle 2 also shows that there are lattice fringes with a spacing of 0.206nm inside the particle, which is consistent with the crystal plane spacing of the (111) plane of cubic diamond. It can be seen that there are diamond nanoparticles in the sample, with a size of about 5nm.

[0044] Example 3

[0045] (1) A graphite sheet (prepared by Beijing Electric Carbon Factory, purity 99.9%) was ground (using 2000 mesh and 4000 mesh sandpaper successively), polished (using polishing flannel cloth), ultrasonically cleaned in ethanol (manufactured by Kunshan Ultrasonic Instrument Co., Ltd., model KQ5200DE, 140W ultrasonic for 15 minutes), cleaned with deionized water, and dried (dried with a nitrogen gun) to obtain a pretreated graphite sheet; the above pretreatment is to obtain a graphite sheet with a smooth and clean surface.

[0046] (2) The tantalum wire is tooled in the form of a double spiral. The graphite sheet pretreated in step (1) is placed in a hot wire chemical vapor deposition (HFCVD) device, and hydrogen is introduced at a flow rate of 100 sccm and a power of 400 W. The gas pressure is controlled to be stable at 3.5 kPa. After 15 minutes of treatment, the power is reduced to 0 at a rate of 1 V / min in a hydrogen atmosphere to complete the Ta deposition process.

[0047] (3) placing the graphite sheet treated in step (2) into a quartz tube and sealing the tube, placing the sealed quartz tube (with the sample inside) into a muffle furnace at 1100° C., taking out the sample after annealing for 120 min, and completing the annealing process.

[0048] Field emission scanning electron microscopy (FESEM) and high resolution transmission electron microscopy (HRTEM) were used to observe the composition of the samples after the experiment.

[0049] Figure 7 This is the SEM picture of Example 3. After annealing, spherical nanoparticles exist on the surface of the sample. Compared with the sample annealed for 30 minutes (Example 2), the number of particles on the surface is more and the size is larger.

[0050] Figure 8 This is the TEM image of Example 3. SAED-a shows the diffraction rings of the (111), (200), (220) and (311) crystal planes of diamond. Figure (b) is an enlarged view of area b in Figure (a). The corresponding FT image FT-b shows the diffraction information of the crystal plane with a spacing of 0.210nm. The FT image FT-b1 of area 1 in Figure (b) shows the diffraction information of the crystal plane spacing of 0.210nm and 0.126nm, corresponding to the (111) and (220) of diamond, and the angle between the (111) and (111) planes is 70°, and the angle between the (111) and (220) planes is 35°, which is consistent with the standard angle of the crystal plane angle. In Figure b-1, there are corresponding lattice fringes with spacings of 0.210nm and 0.126nm. The FT image FT-b2 of area 2 shows diffraction information with interplanar spacing of 0.206nm and 0.104nm, corresponding to the (111) and (222) planes of diamond. In the enlarged image b-2, there are corresponding lattice fringes with a spacing of 0.206nm, belonging to the (111) crystal plane of diamond. Analysis shows that more diamonds are obtained in this area, with a size between 10nm and 15nm.

[0051] Example 4

[0052] (1) A graphite sheet (prepared by Beijing Electric Carbon Factory, purity 99.9%) was ground (using 2000 mesh and 4000 mesh sandpaper successively), polished (using polishing flannel cloth), ultrasonically cleaned in ethanol (manufactured by Kunshan Ultrasonic Instrument Co., Ltd., model KQ5200DE, 140W ultrasonic for 15 minutes), cleaned with deionized water, and dried (dried with a nitrogen gun) to obtain a pretreated graphite sheet; the above pretreatment is to obtain a graphite sheet with a smooth and clean surface.

[0053] (2) The tantalum wire is tooled in the form of a double spiral. The graphite sheet pretreated in step (1) is placed in a hot wire chemical vapor deposition (HFCVD) device, and hydrogen is introduced at a flow rate of 100 sccm and a power of 400 W. The gas pressure is controlled to be stable at 3.5 kPa. After 15 minutes of treatment, the power is reduced to 0 at a rate of 1 V / min in a hydrogen atmosphere to complete the Ta deposition process.

[0054] (3) placing the graphite sheet treated in step (2) into a quartz tube and sealing the tube, placing the sealed quartz tube (with the sample inside) into a muffle furnace at 1200° C., taking out the sample after annealing for 30 minutes, and completing the annealing process.

[0055] Field emission scanning electron microscopy (FESEM) and high resolution transmission electron microscopy (HRTEM) were used to observe the composition of the samples after the experiment.

[0056] Fig. 9 This is the SEM picture of Example 4. After annealing, dense spherical nanoparticles exist on the surface of the sample. Compared with the sample annealed at 1100°C (Example 2), the number of nanoparticles on the surface is more and the size is larger.

[0057] Fig.10 The TEM image of Example 4, low-magnification TEM image (a) shows that there are many black particles in the sample. SAED-a mainly shows the diffraction rings of graphite (002), (100), (101), (110) and (112), and there are also diffraction points corresponding to the interplanar spacing of 0.170nm, 0.150nm, 0.140nm and 0.130nm. Figure (c) is an enlarged view of the b area in Figure (a), and the FT-b image shows the diffraction rings with an interplanar spacing of 0.210nm, where the diffraction point area corresponding to the arrow coincides with the particle position in Figure (b). From the enlarged view of the particle, it can be seen that the particle has clear lattice fringes inside, and the interplanar spacing is 0.210nm, which is the cubic diamond (111) plane. The FT diagram in Figure (c) shows diffraction information with interplanar spacings of 0.190nm, 0.150nm and 0.130nm, which are close to the (101), (102) and (110) of hexagonal diamond. By measuring the angles between the crystal planes, it was found that they were consistent with the standard crystal plane angles of the hexagonal diamond structure. The previous analysis showed that diamonds larger than 10nm were obtained in the sample.

[0058] Example 5

[0059] (1) A graphite sheet (prepared by Beijing Electric Carbon Factory, purity 99.9%) was ground (using 2000 mesh and 4000 mesh sandpaper successively), polished (using polishing flannel cloth), ultrasonically cleaned in ethanol (manufactured by Kunshan Ultrasonic Instrument Co., Ltd., model KQ5200DE, 140W ultrasonic for 15 minutes), cleaned with deionized water, and dried (dried with a nitrogen gun) to obtain a pretreated graphite sheet; the above pretreatment is to obtain a graphite sheet with a smooth and clean surface.

[0060] (2) The tantalum wire is tooled in the form of a double spiral. The graphite sheet pretreated in step (1) is placed in a hot wire chemical vapor deposition (HFCVD) device, and hydrogen is introduced at a flow rate of 100 sccm and a power of 400 W. The gas pressure is controlled to be stable at 3.5 kPa. After 5 minutes of treatment, the power is reduced to 0 at a speed of 1 V / min in a hydrogen atmosphere to complete the Ta deposition treatment.

[0061] (3) placing the graphite sheet treated in step (2) into a quartz tube and sealing the tube, placing the sealed quartz tube (with the sample inside) into a muffle furnace at 1100° C., taking out the sample after annealing for 30 minutes, and completing the annealing process.

[0062] Field emission scanning electron microscopy (FESEM) and high resolution transmission electron microscopy (HRTEM) were used to observe the composition of the samples after the experiment.

[0063] Fig.11 This is the SEM picture of Example 5. After annealing, a small amount of spherical nanoparticles are present on the surface of the sample. Compared with the sample treated with Ta wire for 15 minutes (Example 2), the number of nanoparticles on the surface is greatly reduced, and the particle size is more uniform.

[0064] Fig.12 This is the TEM image of Example 5. From the low-magnification image, it can be seen that there are many black nanoparticles in the thin area of ​​the sample. SAED-a mainly contains diffraction rings of the (002), (100) and (101) crystal planes of graphite. Figure (b) shows a high-magnification image of the nanoparticles. There are two pairs of diffraction points in FT-b corresponding to the positions of the two particles in Figure (b). The enlarged image b-1 of particle 1 shows that there are clear lattice fringes inside the particle, and the crystal plane spacing is 0.212nm, which is close to the (111) plane of cubic diamond. The enlarged image b-2 of particle 2 also shows that there are lattice fringes with a spacing of 0.202nm inside the particle, which is consistent with the crystal plane spacing of the (111) plane of cubic diamond. The outside of both particles is surrounded by lattice fringes of the (002) crystal plane of graphite. The previous analysis shows that there are nanodiamond particles of about 10nm in the sample.

Claims

1. A method for preparing diamond based on graphite under normal pressure, characterized in that The method comprises the following steps: (1) Pretreatment of graphite sheets: grinding, polishing, ultrasonic cleaning in an organic solvent, cleaning with deionized water, and drying the graphite sheets in sequence to obtain pretreated graphite sheets; (2) Ta wire treatment: the pretreated graphite sheet in step (1) is placed as a substrate in a hot wire chemical vapor deposition device for tantalum deposition, wherein the pretreated graphite sheet is located directly below the tantalum wire, the hydrogen flow rate is adjusted to 10-350 sccm, the power is controlled to 300-800 W, and the gas pressure is 3-5 kPa. After treatment for 1-60 min, the power is reduced to 0 at a rate of 1 V / min in a hydrogen atmosphere to obtain a graphite sheet treated with Ta wire; (3) Annealing treatment: The graphite sheet treated with Ta wire in step (2) is sealed in a quartz tube, placed in a muffle furnace and annealed at 400-1300° C. for 10-180 min to obtain diamond.

2. The method for preparing diamond based on graphite under normal pressure according to claim 1, characterized in that: The graphite sheet described in step (1) is a polycrystalline graphite sheet with a size of 10×10×2 mm and a purity of 99.9%.

3. The method for preparing diamond based on graphite under normal pressure according to claim 1, characterized in that: The organic solvent in step (1) is ethanol or acetone.

4. The method for preparing diamond based on graphite under normal pressure as claimed in claim 3, characterized in that: The organic solvent in step (1) is ethanol.

5. The method for preparing diamond based on graphite under normal pressure according to claim 1, characterized in that: The hydrogen flow rate in step (2) is 100 sccm.

6. The method for preparing diamond based on graphite under normal pressure according to claim 1, characterized in that: The power in step (2) is 400W.

7. The method for preparing diamond based on graphite under normal pressure according to claim 1, characterized in that: The air pressure in step (2) is 3.5 kPa.

8. The method for preparing diamond based on graphite under normal pressure according to claim 1, characterized in that: The treatment time in step (2) is 5 min to 15 min.

9. The method for preparing diamond based on graphite under normal pressure according to claim 1, characterized in that: The annealing temperature in step (3) is 500-1200° C. and the annealing time is 30-120 min.

10. The method for preparing diamond based on graphite under normal pressure according to claim 9, characterized in that: The annealing temperature in step (3) is 1100° C. and the annealing time is 120 min.

Citation Information

Patent Citations

  • A method for preparing diamond based on graphite under low pressure

    CN114751408B

  • Method for preparing diamond based on graphite under low pressure

    CN114751408A

  • Self-supporting ultra-fine nanocrystalline diamond thick film

    US20210140038A1