A fluorine-doped lithium-rich manganese-based positive electrode material and its preparation method and application

By uniformly doping fluorine elements on the surface of lithium-rich manganese-based positive electrode materials, using high-temperature and high-speed stirring and microwave reactions of polytetrafluoroethylene micropowder and titanium carbide powder, the oxygen release and structure of lithium-rich manganese-based positive electrode materials during charging and discharging are solved. The problem of easy collapse significantly improves its cycle stability and electrochemical properties, and extends the service life of lithium-ion batteries.

CN116282227BActive Publication Date: 2024-11-15HEBEI UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310301499.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-11-15
Estimated Expiration
2043-03-24

AI Technical Summary

Technical Problem

During the charging and discharging process of lithium-rich manganese-based positive electrode materials, there are problems such as oxygen release, easy structure collapse and poor cycle stability, and traditional doping methods cannot uniformly incorporate fluorine elements, resulting in poor electrochemical performance.

Method used

Use polytetrafluoroethylene micropowder and titanium carbide powder as fluorine-containing materials, and through high-temperature and high-speed stirring and microwave reaction, uniformly dopant fluorine elements on the surface of lithium-rich manganese-based positive electrode material, enhancing the combination of fluorine elements and materials, and inhibiting the transition metal ions. Migration and oxygen release to improve structural stability.

Benefits of technology

It effectively improves the cycle stability and structural stability of lithium-rich manganese-based positive electrode materials, extends the service cycle of lithium-ion batteries, improves battery performance, and avoids structural collapse and power attenuation caused by uneven distribution of fluorine elements in traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116282227B_ABST
    Figure CN116282227B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of electrode materials, and specifically discloses a fluorine-doped lithium-rich manganese-based positive electrode material and a preparation method and application thereof. The present invention uses lithium hydroxide, manganese dioxide, cobalt oxide and nickel oxide as precursors, and adds an organic fluorine-containing material prepared from polytetrafluoroethylene and titanium carbide as raw materials, and prepares the fluorine-doped lithium-rich manganese-based positive electrode material in a simple and economical method, which not only prevents the formation of oxygen molecules on the surface of the positive electrode material, but also greatly improves the cycle stability of the positive electrode material, effectively improves the battery performance of the positive electrode material, especially its cycle stability and structural stability, and increases the service life of the lithium ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of lithium ion electrode materials, and specifically discloses the preparation and application of a fluorine-doped lithium-rich manganese-based positive electrode material. Background Art

[0002] Lithium-ion batteries play a vital role in our daily lives. They are indispensable portable energy storage units in electronic devices, such as mobile phones and laptops. Today, consumers' pursuit of a better experience with modern devices has promoted the development of lithium-ion batteries with higher energy density and greater safety. Compared with other traditional positive electrode materials (lithium manganese oxide, lithium iron phosphate, etc.), layered lithium-rich manganese-based positive electrode materials have high reversible capacity (>250mAh / g), high energy density (>900Wh / kg) and wide operating voltage (>4.5V). Therefore, lithium-rich manganese-based positive electrode materials are considered to be the most valuable positive electrode materials for the next generation of lithium-ion batteries.

[0003] However, due to its inherent problems, the process of commercial promotion of lithium-rich manganese-based positive electrode materials has been hindered. For example, lithium-rich manganese-based positive electrode materials always show obvious defects during the charge and discharge process, such as too fast capacity and voltage decay, poor cycle performance, etc. The prior art has found that after fluorine is doped on the surface of the lithium-rich manganese-based positive electrode material, the fluorine replaces the oxygen position, which will increase the binding force between the transition metal ions and the lattice oxygen, and will inhibit the migration of the transition metal ions and the occurrence of phase change, thereby improving the structural stability and cycle stability of the positive electrode material. However, the traditional doping method cannot evenly incorporate the fluorine element into the surface of the lithium-rich manganese-based positive electrode material. Therefore, the development of a method that can evenly incorporate fluorine into the surface of the material, thereby improving the electrochemical properties and structural stability of the lithium-rich manganese-based positive electrode material, is still a difficult problem that the prior art needs to overcome. Summary of the invention

[0004] In view of the technical problems in the prior art that the lithium-rich manganese-based positive electrode material has poor rate performance, easy structural collapse and poor cycle stability due to the release of oxygen during the charge and discharge process, and the fluorine element doped into the positive electrode material is random and cannot be doped evenly, the present invention provides a preparation and application of a fluorine-doped lithium-rich manganese-based positive electrode material. The surface of the fluorine-doped lithium-rich manganese-based positive electrode material provided by the present invention is uniformly doped with fluorine element, which effectively improves the electrochemical properties of the positive electrode material, especially its cycle stability and structural stability, and increases the service life of the lithium-ion battery.

[0005] To further illustrate the technical solution of the present invention, the specific contents are as follows:

[0006] The first aspect of the present invention provides a method for preparing a fluorine-doped lithium-rich manganese-based positive electrode material, comprising at least the following steps:

[0007] Step 1: Using lithium hydroxide, manganese dioxide, cobalt oxide and nickel oxide as raw materials, ball milling and calcining in batches to prepare a lithium-rich manganese-based positive electrode material;

[0008] Step 2: uniformly mix polytetrafluoroethylene powder and titanium carbide powder, sinter at a temperature of 400°C-500°C, add superconductive carbon black to the sintered product, mix uniformly, press into tablets, and react with microwaves in an inert atmosphere to obtain a fluorine-containing material;

[0009] Step 3: Evenly mix the lithium-rich manganese-based positive electrode material and the fluorine-containing material, stir at 80° C.-100° C. and a stirring speed greater than 5000 r / min, dry, and sinter to obtain a lithium-rich manganese-based positive electrode material with fluorine evenly doped on the surface.

[0010] Compared with the prior art, the present invention uses a simple and economical method to prepare a lithium-rich manganese-based positive electrode material with uniform fluorine doping on the surface, which not only prevents the formation of surface oxygen molecules, but also greatly improves the cycle stability and structural stability of the lithium-rich manganese-based positive electrode material. The present invention uses polytetrafluoroethylene micropowder and titanium carbide powder as raw materials for fluorine-containing materials, combines polytetrafluoroethylene with two-dimensional material titanium carbide, allows polytetrafluoroethylene, a flexible material, to completely open the chain, and high-temperature and high-speed stirring further increases the bonding surface between the fluorine-containing material and the lithium-rich manganese-based positive electrode material, so that the doped fluorine element can evenly cover the positive electrode material, avoiding the problem that the traditional doped fluorine element cannot be evenly distributed, resulting in oxygen exposure in some areas of the surface of the lithium-rich manganese-based positive electrode material, causing serious fragmentation of sample particles and leading to structural collapse and battery capacity attenuation. In addition, the incorporation of an appropriate amount of organic fluorine elements increases the binding force between transition metal ions and lattice oxygen, inhibits the migration of transition metals and the release of oxygen, inhibits cation mixing, and improves structural stability, thereby inhibiting the capacity decay of the battery positive electrode material, improving the cycle stability, effectively improving the battery performance of the positive electrode material, and increasing the battery's service life.

[0011] Preferably, in step 1, the mass ratio of lithium hydroxide, manganese dioxide, cobalt oxide and nickel oxide is 4.5-6.2:4-5.4:1-1.1:1-1.1.

[0012] Preferably, in step 2, the mass ratio of the polytetrafluoroethylene powder to titanium carbide is 1-1.1:1-1.2.

[0013] Preferably, in step three, the mass ratio of the fluorine-containing material to the lithium-rich manganese-based positive electrode material is 1-1.5:2.5-4.

[0014] Preferably, in step 1, the ball milling speed is 100 r / min-200 r / min, and the ball milling time is 8 h-15 h.

[0015] Preferably, in step one, the calcination is performed in two steps, the first calcination temperature is 550°C-650°C, the sintering time is 4h-8h, and the heating rate is 3°C / min-6°C / min; the second calcination temperature is 850°C-950°C, the calcination time is 10h-15h, and the heating rate is 4°C / min-8°C / min.

[0016] In the present invention, high temperature calcination is used to remove impurity elements in the precursor powder, and then the lithium-rich manganese-based positive electrode material is prepared by staged high temperature calcination. The high temperature can make the generated lattice more stable, so that the positive electrode material exhibits a layered structure.

[0017] Preferably, the preparation of the titanium carbide powder comprises the following steps: dissolving titanium aluminum carbide in a hydrochloric acid solution of lithium fluoride, stirring for reaction, centrifuging, washing, collecting solid centrifuge, and drying to obtain titanium carbide powder.

[0018] Preferably, the mass volume ratio of the titanium aluminum carbide to the hydrochloric acid solution of lithium fluoride is 1:10-12.

[0019] Preferably, the mass concentration of lithium fluoride in the lithium fluoride hydrochloric acid solution is 0.07 g / mL-0.1 g / mL, and the concentration of HCl is 8 mol / L-10 mol / L.

[0020] Preferably, the stirring reaction temperature is 30°C-45°C, and the stirring reaction time is 18h-24h.

[0021] Preferably, the centrifugal speed is 3500r / min-4500r / min, the centrifugal time is 3min-5min each time, and the centrifugation is performed 3-5 times.

[0022] Preferably, in step 2, the sintering time is 4h-8h.

[0023] The present invention mixes polytetrafluoroethylene powder and titanium carbide and then sintering, so that the organic chain [CF2-CF2] in the polytetrafluoroethylene molecule is opened and stored in the gap between titanium carbide layers like a plane, so that the polytetrafluoroethylene and titanium carbide are tightly combined.

[0024] Preferably, in step 2, the amount of superconductive carbon black added is 1%-3% of the mass of the sintered material.

[0025] Preferably, in step 2, the temperature of the microwave reaction is 500° C.-600° C., and the time of the microwave reaction is 5 min-15 min.

[0026] Preferably, in step three, the uniform mixing is achieved by ultrasonic mixing, the ultrasonic frequency is 35kHz-40kHz, and the ultrasonic time is 8min-12min.

[0027] Preferably, in step three, the stirring time is 1h-2h.

[0028] Under high-speed and high-temperature conditions, the organic fluorine-containing material will be evenly coated on the surface of the lithium-rich manganese-based particles, but this effect cannot be achieved by the solid-solid contact between traditional inorganic salts and lithium-rich manganese-based positive electrode material particles.

[0029] Preferably, in step three, the sintering temperature is 700°C-800°C, the heating rate is 3°C / min-7°C / min, and the sintering time is 2h-6h.

[0030] The second aspect of the present invention provides a fluorine-doped lithium-rich manganese-based positive electrode material, which is prepared by the preparation method of the fluorine-doped lithium-rich manganese-based positive electrode material.

[0031] The third aspect of the present invention provides the use of the fluorine-doped lithium-rich manganese-based positive electrode material in a lithium-ion battery.

[0032] The present invention provides a fluorine-doped lithium-rich manganese-based positive electrode material and a preparation method and application thereof. The operation is simple, and the surface of the fluorine-doped lithium-rich manganese-based positive electrode material provided by the present invention is uniformly doped with fluorine element, which effectively improves the battery performance of the positive electrode material, especially its cycle stability and structural stability, and increases the service life of the lithium-ion battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Attached Figure 1 The SEM images of Comparative Example 2 and Example 1 after 100 cycles at a current density of 1C, wherein (a) is Comparative Example 2, and (b) is Example 1;

[0034] Attached Figure 2 The cycle performance diagram of the samples of Comparative Examples 2-3 and Example 1 after 150 charge and discharge cycles at a current density of 1C;

[0035] Attached Figure 3 The rate performance diagram of the samples of Comparative Examples 2-3 and Example 1 after 150 charge and discharge cycles at a current density of 1C;

[0036] Attached Figure 4 It is the EDS analysis diagram of oxygen element and fluorine element in comparative example 2 and embodiment 1. DETAILED DESCRIPTION

[0037] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] Example 1

[0039] This embodiment provides a method for preparing a fluorine-doped lithium-rich manganese-based positive electrode material, the specific contents of which are as follows:

[0040] Step 1: Mix 9.31 g of lithium hydroxide, 8.25 g of manganese dioxide, 1.71 g of cobalt oxide and 1.71 g of nickel oxide, add 30 mL of anhydrous ethanol, pour into a ball mill, add ball milling beads at a ball-to-material ratio of 1:3, place the ball mill on a ball mill, ball mill at a speed of 150 rpm for 10 h, and then dry at 120 ° C for 6 h to obtain a precursor powder;

[0041] Step 2, manually grinding the precursor powder in an agate mortar for 30 minutes, then heating the precursor powder to 600°C at a heating rate of 5°C / min, sintering for 6 hours, cooling and then heating to 900°C at a heating rate of 6°C / min, performing secondary calcination for 12 hours, cooling after calcination, and obtaining a lithium-rich manganese-based positive electrode material;

[0042] Step 3, slowly dissolve 2g of titanium aluminum carbide in a 20mL volume, 0.08g / mL lithium fluoride hydrochloric acid solution (concentration is 9mol / L), stir and react at 40°C for 20h, after the reaction is completed, centrifuge the obtained product at a speed of 4000r / min for 3min each time, centrifuge 4 times, wash, collect the solid centrifuge, and dry to obtain titanium carbide powder;

[0043] Step 4: 0.1 g of polytetrafluoroethylene powder and 0.1 g of titanium carbide powder are mixed evenly, sintered at 450° C. for 6 h, and after cooling, the sintered mixture is weighed, and the sintered mixture is mixed evenly with 2% by mass of superconductive carbon black, and then pressed into tablets, and then subjected to microwave reaction in an inert atmosphere at a reaction temperature of 550° C. for 10 min to obtain a fluorine-containing material;

[0044] Step 5: Dissolve the fluorine-containing material in 10 mL of anhydrous ethanol, then add 0.5 g of lithium-rich manganese-based positive electrode material, ultrasonicate at a frequency of 40 kHz for 10 min, and after mixing evenly, heat and stir the mixed system at 90 ° C at a speed higher than 5000 r / min for 1 h, dry after stirring, and heat the dried mixture to 750 ° C at a heating rate of 5 ° C / min, sinter for 5 h, and cool to room temperature to obtain a fluorine-doped lithium-rich manganese-based positive electrode material.

[0045] Example 2

[0046] This embodiment provides a method for preparing a fluorine-doped lithium-rich manganese-based positive electrode material, the specific contents of which are as follows:

[0047] Step 1: Mix 9.31 g of lithium hydroxide, 8.25 g of manganese dioxide, 1.71 g of cobalt oxide and 1.71 g of nickel oxide, add 40 mL of anhydrous ethanol, pour into a ball mill, add ball milling beads at a ball-to-material ratio of 1:3, place the ball mill on a ball mill, ball mill at a speed of 150 rpm for 12 h, and then dry at 130 ° C for 8 h to obtain a precursor powder;

[0048] Step 2, manually grinding the precursor powder in an agate mortar for 30 minutes, then heating the precursor powder to 600°C at a heating rate of 4°C / min, sintering for 6 hours, cooling and then heating to 850°C at a heating rate of 5°C / min, performing secondary calcination for 13 hours, and cooling after calcination to obtain a lithium-rich manganese-based positive electrode material;

[0049] Step 3, slowly dissolve 1g of titanium aluminum carbide in a 12mL volume, 0.09g / mL mass concentration of lithium fluoride hydrochloric acid solution (concentration is 8mol / L), stir and react at 45°C for 20h, after the reaction is completed, centrifuge the obtained product at a speed of 4000r / min for 4min each time, centrifuge 3 times, wash, collect the solid centrifuge, and dry to obtain titanium carbide powder;

[0050] Step 4: 0.1 g of polytetrafluoroethylene powder and 0.1 g of titanium carbide powder are mixed evenly, sintered at 450° C. for 6 h, and after cooling, the sintered mixture is weighed, and the sintered mixture is mixed evenly with 3% of the mixture mass of superconductive carbon black and pressed into tablets, and then subjected to microwave reaction in an inert atmosphere at a reaction temperature of 500° C. for 15 min to obtain a fluorine-containing material;

[0051] Step 5: Dissolve the fluorine-containing material in 15 mL of anhydrous ethanol, then add 0.5 g of lithium-rich manganese-based positive electrode material, ultrasonicate at a frequency of 40 kHz for 10 min, and after mixing evenly, heat and stir the mixed system at 90 ° C at a speed higher than 5000 r / min for 1.5 h, dry after stirring, and heat the dried mixture to 700 ° C at a heating rate of 5 ° C / min, sinter for 6 h, and cool to room temperature to obtain a fluorine-doped lithium-rich manganese-based positive electrode material.

[0052] Example 3

[0053] This embodiment provides a method for preparing a fluorine-doped lithium-rich manganese-based positive electrode material, the specific contents of which are as follows:

[0054] Step 1: Mix 9.31 g of lithium hydroxide, 8.25 g of manganese dioxide, 1.71 g of cobalt oxide and 1.71 g of nickel oxide, add 30 mL of anhydrous ethanol, pour into a ball mill, add ball milling beads at a ball-to-material ratio of 1:3, place the ball mill on a ball mill, ball mill at a speed of 150 rpm for 10 h, and then dry at 120 ° C for 6 h to obtain a precursor powder;

[0055] Step 2, manually grinding the precursor powder in an agate mortar for 30 minutes, then heating the precursor powder to 600°C at a heating rate of 5°C / min, sintering for 6 hours, cooling and then heating to 900°C at a heating rate of 5°C / min, performing secondary calcination for 12 hours, cooling after calcination, and obtaining a lithium-rich manganese-based positive electrode material;

[0056] Step 3, slowly dissolve 2g of titanium aluminum carbide in a 25mL volume, 0.08g / mL lithium fluoride hydrochloric acid solution (concentration is 10mol / L), stir and react at 40°C for 20h, after the reaction is completed, centrifuge the obtained product at a speed of 4500r / min for 3min each time, centrifuge 4 times, wash, collect the solid centrifuge, and dry to obtain titanium carbide powder;

[0057] Step 4: 0.1 g of polytetrafluoroethylene powder and 0.1 g of titanium carbide powder are mixed evenly, sintered at 450° C. for 6 h, and after cooling, the sintered mixture is weighed, and the sintered mixture is mixed evenly with 2.5% of the mass of the mixture of superconductive carbon black and pressed into tablets, and then subjected to microwave reaction in an inert atmosphere at a reaction temperature of 600° C. for 8 min to obtain a fluorine-containing material;

[0058] Step 5: Dissolve the fluorine-containing material in 10 mL of anhydrous ethanol, then add 0.5 g of lithium-rich manganese-based positive electrode material, ultrasonicate at a frequency of 35 kHz for 12 min, and after mixing evenly, heat and stir the mixed system at 100 ° C at a speed higher than 5000 r / min for 1 h, dry after stirring, and heat the dried mixture to 800 ° C at a heating rate of 6 ° C / min, sinter for 4 h, and cool to room temperature to obtain a fluorine-doped lithium-rich manganese-based positive electrode material.

[0059] Comparative Example 1

[0060] The difference between this comparative example and Example 1 is that step 3 is omitted, and other components and preparation methods remain unchanged. The specific contents are as follows:

[0061] This comparative example provides a method for preparing a fluorine-doped lithium-rich manganese-based positive electrode material, and the specific preparation method is as follows:

[0062] Step 1: Mix 9.31 g of lithium hydroxide, 8.25 g of manganese dioxide, 1.71 g of cobalt oxide and 1.71 g of nickel oxide, add 30 mL of anhydrous ethanol, pour into a ball mill, add ball milling beads at a ball-to-material ratio of 1:3, place the ball mill on a ball mill, ball mill at a speed of 150 rpm for 10 h, and then dry at 120 ° C for 6 h to obtain a precursor powder;

[0063] Step 2, manually grinding the precursor powder in an agate mortar for 30 minutes, then heating the precursor powder to 600°C at a heating rate of 5°C / min, sintering for 6 hours, cooling and then heating to 900°C at a heating rate of 6°C / min, performing secondary calcination for 12 hours, cooling after calcination, and obtaining a lithium-rich manganese-based positive electrode material;

[0064] Step 3, 0.1 g of polytetrafluoroethylene powder and 2% of superconductive carbon black by weight of the polytetrafluoroethylene powder are mixed evenly and pressed into tablets, and then subjected to microwave reaction under an inert atmosphere at a reaction temperature of 550° C. for 10 min to obtain a fluorine-containing material;

[0065] Step 4: dissolve the fluorine-containing material in 10 mL of anhydrous ethanol, then add 0.5 g of lithium-rich manganese-based positive electrode material, ultrasonicate at a frequency of 40 kHz for 10 min, and after mixing evenly, heat and stir the mixed system at 90 ° C at a speed higher than 5000 r / min for 1 h, dry after stirring, and heat the dried mixture to 750 ° C at a heating rate of 5 ° C / min, sinter for 5 h, and cool to room temperature to obtain a fluorine-doped lithium-rich manganese-based positive electrode material.

[0066] Comparative Example 2

[0067] This comparative example provides a method for preparing a conventional fluorine-doped lithium-rich manganese-based positive electrode material, the specific contents of which are as follows:

[0068] Step 1: Evenly mix 5.95 g of lithium hydroxide, 5.51 g of manganese dioxide, 1.14 g of cobalt oxide, 1.14 g of nickel oxide and 0.15 g of lithium fluoride, add 30 mL of anhydrous ethanol, pour into a ball mill, add ball milling beads at a ball-to-material ratio of 1:3, place the ball mill on a ball mill, ball mill at a speed of 150 rpm for 10 h, and then dry at 120 ° C for 6 h to obtain a precursor powder;

[0069] Step 2: Grind the precursor powder manually in an agate mortar for 30 minutes, then heat the precursor powder to 600°C at a heating rate of 5°C / min, sinter for 6 hours, and then heat it to 900°C at a heating rate of 6°C / min after cooling, and perform secondary calcination for 12 hours. After calcination, cool it to obtain a fluorine-doped lithium-rich manganese-based positive electrode material.

[0070] Comparative Example 3

[0071] This comparative example provides a method for preparing a lithium-rich manganese-based positive electrode material that is not doped with fluorine, and the specific contents are as follows:

[0072] Step 1: Mix 9.31 g of lithium hydroxide, 8.25 g of manganese dioxide, 1.71 g of cobalt oxide and 1.71 g of nickel oxide, add 30 mL of anhydrous ethanol, pour into a ball mill, add ball milling beads at a ball-to-material ratio of 1:3, place the ball mill on a ball mill, ball mill at a speed of 150 rpm for 10 h, and then dry at 120 ° C for 6 h to obtain a precursor powder;

[0073] Step 2: Grind the precursor powder manually in an agate mortar for 30 minutes, then heat the precursor powder to 600°C at a heating rate of 5°C / min, sinter for 6 hours, and then heat it to 900°C at a heating rate of 6°C / min after cooling, and perform secondary calcination for 12 hours. After calcination, cool it to obtain a lithium-rich manganese-based positive electrode material.

[0074] Performance Testing

[0075] To further illustrate the electrochemical performance of the fluorine-doped lithium-rich manganese-based positive electrode material provided by the present invention, the lithium-rich manganese-based positive electrode material prepared in each embodiment and each comparative example is applied to a lithium-ion battery, and relevant electrochemical tests are performed. The specific preparation method is as follows:

[0076] Step 1: Evenly mix the obtained lithium-rich manganese-based positive electrode material with acetylene black and polyvinylidene fluoride (PVDF) at a mass ratio of 8:1:1, add 20 mL of N-methylpyrrolidone, and grind for 25 minutes to obtain a mixed slurry;

[0077] Step 2: evenly coat the obtained mixed slurry on aluminum foil with a coating thickness of 0.5 mm, dry at 80° C. for 10 h, and after drying, cut the obtained electrode sheet into a disc with a diameter of 1 cm, i.e., the electrode sheet;

[0078] Step 3: Use the obtained electrode sheet as the positive electrode sheet, the lithium sheet as the negative electrode sheet, an ultra-high molecular weight polyethylene diaphragm (PE diaphragm), and a high-voltage electrolyte to prepare a button battery in a glove box, and perform a charge and discharge test on a blue battery test system. The test voltage range is 2.0V-4.8V, and the test temperature is 25°C.

[0079] According to the test results, Figure 1-4 , as shown in Table 1 and Table 2.

[0080] Table 1 Cyclic discharge specific capacity of batteries prepared using lithium-rich manganese-based positive electrode materials of various embodiments and comparative examples

[0081]

[0082]

[0083] Table 2 Rate performance of batteries prepared using lithium-rich manganese-based positive electrode materials of various embodiments and comparative examples

[0084]

[0085] Figure 1 It shows that the structural stability of the positive electrode material is improved by the method of surface doping with fluorine. After 100 charge and discharge cycles, the fluorine element on the surface of the positive electrode material provided in Comparative Example 2 is not evenly distributed, resulting in oxygen exposure in some areas of the surface layer, so that the particles of the traditional doped sample are severely broken, and then the serious structural collapse may cause capacity decay. In contrast, after the oxygen on the surface of the positive electrode material provided in Example 1 is uniformly replaced by fluorine, the binding force between the transition metal ions and the lattice oxygen will be improved, which inhibits the migration of transition metals and the release of oxygen, thereby improving the structural stability and cycle stability.

[0086] Figure 2 It is confirmed that the cyclic stability of the material can be significantly improved after the surface of the positive electrode material particles is uniformly doped with fluorine. This is mainly attributed to the fact that the fluorine on the surface of the positive electrode material particles can promote the combination of lattice oxygen and transition metal ions, enhance covalency, inhibit cation mixing, and improve the structural stability of the material, thereby making the positive electrode material have stable cyclic performance. Among them, the capacity retention rate of the sample in Example 1 after 150 cycles is 98.5%.

[0087] from Figure 3 It can be seen that with the increase of current density, different samples have different degrees of attenuation. At a current density of 0.1C, the batteries prepared using the samples provided in Example 1, Comparative Example 2 and Comparative Example 3 have discharge specific capacities of 249.6mAh / g, 204mAh / g and 267.4mAh / g, respectively, at a current density of 0.1C; at a current density of 1C, the discharge specific capacities are 168.9mAh / g, 136.3mAh / g and 134.2mAh / g, respectively; at a current density of 5C, the discharge specific capacities are 121.7mAh / g, 88.1mAh / g and 71.8mAh / g, respectively. The above results show that the battery rate performance prepared by the fluorine-doped lithium-rich manganese-based positive electrode material of Example 1 is the best and most stable, which is mainly attributed to the fact that the incorporation of an appropriate amount of organic fluorine increases the binding force between lattice oxygen and transition metal ions, inhibits cation mixing, and improves structural stability, thereby inhibiting the capacity decay of the material.

[0088] Figure 4The EDS analysis diagrams of oxygen and fluorine in Comparative Example 2 and Example 1. In the same particle surface area, the presence ranges of oxygen and fluorine in the Comparative Example 2 sample are relatively inconsistent, the area of ​​oxygen is uniform and orderly, while the area of ​​fluorine is uneven and random. In contrast, the fluorine in the Example 1 sample is uniformly distributed on the surface of the material, and the presence range of oxygen is basically consistent with the presence range of fluorine, and the distribution of fluorine is uniform and orderly like the distribution of oxygen.

[0089] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a fluorine-doped lithium-rich manganese-based positive electrode material, characterized in that: At least the following steps are included: Step 1: Using lithium hydroxide, manganese dioxide, cobalt oxide and nickel oxide as raw materials, ball milling and calcining in batches to prepare a lithium-rich manganese-based positive electrode material; Step 2: uniformly mix polytetrafluoroethylene powder and titanium carbide powder, sinter at a temperature of 400°C-500°C, add superconductive carbon black to the sintered product, mix uniformly, press into tablets, and react with microwaves in an inert atmosphere to obtain a fluorine-containing material; Step 3: Evenly mix the lithium-rich manganese-based positive electrode material and the fluorine-containing material, stir at 80° C.-100° C. and a stirring speed greater than 5000 r / min, dry, and sinter to obtain a lithium-rich manganese-based positive electrode material with fluorine evenly doped on the surface.

2. The method for preparing the fluorine-doped lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: In step 1, the mass ratio of lithium hydroxide, manganese dioxide, cobalt oxide and nickel oxide is 4.5-6.2:4-5.4:1-1.1:1-1.1; and / or In step 2, the mass ratio of the polytetrafluoroethylene powder to titanium carbide is 1-1.1:1-1.2; and / or In step three, the mass ratio of the fluorine-containing material to the lithium-rich manganese-based positive electrode material is 1-1.5:2.5-4.

3. The method for preparing the fluorine-doped lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: In step 1, the ball milling speed is 100r / min-200r / min, and the ball milling time is 8h-15h; and / or In step one, the calcination is carried out in two steps, the first calcination temperature is 550°C-650°C, the sintering time is 4h-8h, and the heating rate is 3°C / min-6°C / min; the second calcination temperature is 850°C-950°C, the calcination time is 10h-15h, and the heating rate is 4°C / min-8°C / min.

4. The method for preparing the fluorine-doped lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: The preparation of the titanium carbide powder comprises the following steps: dissolving titanium aluminum carbide in a hydrochloric acid solution of lithium fluoride, stirring for reaction, centrifuging, washing, collecting solid centrifuge products, and drying to obtain the titanium carbide powder.

5. The method for preparing the fluorine-doped lithium-rich manganese-based positive electrode material according to claim 4, characterized in that: The mass volume ratio of the titanium aluminum carbide to the hydrochloric acid solution of lithium fluoride is 1:10-12; and / or The mass concentration of lithium fluoride in the lithium fluoride hydrochloric acid solution is 0.07 g / mL-0.1 g / mL, and the concentration of HCl is 8 mol / L-10 mol / L; and / or The stirring reaction temperature is 30°C-45°C, and the stirring reaction time is 18h-24h; and / or The centrifugal speed is 3500r / min-4500r / min, the centrifugal time is 3min-5min each time, and the centrifugation is performed 3-5 times.

6. The method for preparing the fluorine-doped lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: In step 2, the sintering time is 4h-8h; and / or In step 2, the amount of superconductive carbon black added is 1%-3% of the mass of the sintered material.

7. The method for preparing the fluorine-doped lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: In step 2, the temperature of the microwave reaction is 500° C.-600° C., and the time of the microwave reaction is 5 min-15 min.

8. The method for preparing the fluorine-doped lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: In step 3, the stirring time is 1h-2h; and / or In step three, the sintering temperature is 700°C-800°C, the heating rate is 3°C / min-7°C / min, and the sintering time is 2h-6h.

9. A fluorine-doped lithium-rich manganese-based positive electrode material, characterized in that: The positive electrode material is prepared by the method for preparing the fluorine-doped lithium-rich manganese-based positive electrode material according to any one of claims 1 to 8.

10. Use of the fluorine-doped lithium-rich manganese-based positive electrode material according to claim 9 in lithium-ion batteries.