A reinforcing agent for organic terrazzo and preparation method thereof

By using the reinforcing additives of polycarboxylic acid dehydration mother liquor, polyethylene glycol monomethyl ether and emulsifier in organic terrazzo, the problems of insufficient strength of organic terrazzo and high cost of epoxy resin are solved, and performance improvement and cost reduction are achieved. effect.

CN116283029BActive Publication Date: 2024-10-18GUANGZHOU CONCRETE QIJIE BUILDING MATERIALS TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310315024.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-18
Estimated Expiration
2043-03-29

AI Technical Summary

Technical Problem

Existing organic terrazzo products are too brittle, easy to break, lack strength and hardness, and the price of epoxy resin is high, resulting in high costs and there is room for improvement.

Method used

Polycarboxylic acid water-reducing mother liquor, polyethylene glycol monomethyl ether and emulsifier are used as reinforcing additives, and the polycarboxylic acid water-reducing mother liquor is synthesized and mixed with polyethylene glycol monomethyl ether and emulsifier as a blending agent for epoxy resin. Adding it in an appropriate amount can improve the compressive strength and Mohs hardness of organic terrazzo and reduce the amount of epoxy resin.

Benefits of technology

It effectively improves the compressive strength and Mohs hardness of organic terrazzo, reduces the amount of epoxy resin, lowers costs, improves environmental protection, and saves resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004149938580000081
    Figure BDA0004149938580000081
Patent Text Reader

Abstract

The present invention provides a reinforcing aid for organic terrazzo, and its raw materials for preparation include the following components by mass percentage: 18-28% polycarboxylic acid water reducing mother liquor, 70-80% polyethylene glycol monomethyl ether, and 2-3% emulsifier; by adding polycarboxylic acid water reducing mother liquor, it is beneficial to improve compressive strength and Mohs hardness, and polyethylene glycol monomethyl ether is added as a viscosity modifier, so that the amount of epoxy resin can be reduced when making organic terrazzo; adding an emulsifier can reduce the surface tension of the system, thereby reducing its interfacial energy, improving the stability of the solution, and making the obtained reinforcing aid added to the organic terrazzo production at an amount of 5-8% of the epoxy resin dosage, which can improve the compressive strength and Mohs hardness of organic terrazzo, reduce the amount of epoxy resin, low cost, good environmental protection, and save resources. The present invention also provides a preparation method of the reinforcing aid for organic terrazzo.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of organic terrazzo, and more particularly to a reinforcing auxiliary agent for organic terrazzo and a preparation method thereof. Background Art

[0002] Organic terrazzo is made of aggregate and organic materials, and the most common one is epoxy terrazzo. Epoxy terrazzo uses epoxy resin as a gelling material and adhesive. After mixing various colored stones, glass, shells, metals, etc., a curing agent is added to solidify, and finally professional grinding and polishing equipment is used for grinding and polishing. Among them, epoxy resin, also known as artificial resin, is a type of organic high molecular polymer with more than two epoxy groups in its molecular structure, and is a thermosetting plastic. Organic terrazzo occupies a huge market in major high-end buildings because of its unlimited colors and patterns, bright colors, and high gloss.

[0003] However, existing organic terrazzo products are generally too brittle, easy to break, and their strength and hardness need to be improved, and the price of epoxy resin remains high.

[0004] Therefore, the prior art has a large room for improvement. Summary of the invention

[0005] The purpose of the present invention is to make up for the deficiencies of the prior art and to propose a reinforcing agent for organic terrazzo, which optimizes the performance of organic terrazzo and adapts to the market demand for organic terrazzo, has low cost and good environmental protection.

[0006] In order to achieve the above object, the present invention is implemented by the following technical solutions:

[0007] A reinforcing auxiliary agent for organic terrazzo, wherein the raw materials for preparing the reinforcing auxiliary agent include the following components by mass percentage: 18-28% of polycarboxylic acid water reducing mother liquid, 70-80% of polyethylene glycol monomethyl ether, and 2-3% of emulsifier.

[0008] Adding polycarboxylic acid water reducing concentrate is helpful to improve compressive strength and Mohs hardness; adding polyethylene glycol monomethyl ether as a viscosity regulator can reduce the amount of epoxy resin used in the production of organic terrazzo; adding an emulsifier can reduce the surface tension of the system, thereby reducing its interfacial energy and improving the stability of the solution. Adding this product to the production of organic terrazzo at a dosage of 5-8% of the amount of epoxy resin can improve the compressive strength and Mohs hardness of the organic terrazzo, and can reduce the amount of epoxy resin used, with low cost, good environmental protection, and resource saving.

[0009] According to the above scheme, the polycarboxylic acid water-reducing concentrate includes the following components in parts by weight: 1 part of isopentyl polyoxyethylene ether macromonomer, 0.08-0.15 parts of sodium propylene sulfonate, 0.1-0.2 parts of general monomers, 0.003-0.004 parts of thiol compounds, 0.001-0.002 parts of E51 reducing agent, 0.004-0.006 parts of hydrogen peroxide, and 0.005-0.007 parts of persulfate.

[0010] According to the above scheme, the general monomer is one of acrylic acid and methacrylic acid.

[0011] According to the above scheme, the molecular weight of the polyethylene glycol monomethyl ether is 400-750.

[0012] The viscosity of the product can be changed by selecting polyethylene glycol monomethyl ether with different molecular weights, and it has good water solubility, wettability and lubricity.

[0013] According to the above scheme, the thiol compound includes at least one of mercaptopropionic acid, thioglycolic acid and mercaptoethanol. The thiol compound can be used as a chain transfer agent to adjust the molecular weight.

[0014] According to the above scheme, the persulfate includes at least one of ammonium persulfate, potassium persulfate, and sodium persulfate.

[0015] According to the above scheme, the molecular weight of the isopentenyl polyoxyethylene ether macromonomer is 3,000.

[0016] The present invention also provides a method for preparing the reinforcing agent for organic terrazzo, comprising the following steps:

[0017] Step 1: Synthesize polycarboxylate water-reducing mother liquor:

[0018] a. Prepare material A: weigh acrylic acid, mercapto compound and deionized water and mix them evenly;

[0019] b. Prepare material B: weigh E51 reducing agent and deionized water and mix them evenly;

[0020] c. Add deionized water at a temperature of 5-15°C into the reaction kettle, then add isopentenyl polyoxyethylene ether macromonomer and sodium propylene sulfonate in sequence, and start the stirrer to stir and dissolve for 30 minutes;

[0021] d. Add persulfate and hydrogen peroxide to the reactor and stir for 3 minutes;

[0022] e. Add material A and material B to the reactor at the same time, the addition time of material A is 120 minutes, and the addition time of material B is 150 minutes. The temperature of the reactor is controlled at 15-25° C., and the temperature is kept warm for 60 minutes after the addition is completed; after the insulation is completed, a sodium hydroxide solution with a mass concentration of 30% is added to adjust the pH value to between 6 and 8.5, and the solid content of the mother liquor is adjusted to 40%, so as to obtain a polycarboxylic acid water-reducing mother liquor;

[0023] Step 2: Mix the polycarboxylic acid water-reducing concentrate described in step 1 with polyethylene glycol monomethyl ether and an emulsifier to obtain a reinforcing agent for organic terrazzo.

[0024] According to the above scheme, the deionized water in step a is equal to the acrylic acid; the deionized water in step b is 15-20% of the isopentenyl polyoxyethylene ether macromonomer; and the deionized water in step c is 66% of the isopentenyl polyoxyethylene ether macromonomer.

[0025] The synthesis reaction mechanism of polycarboxylic acid water-reducing mother liquor is to use the redox reaction of the initiator to generate free radicals, which are used to initiate the polymerization reaction of the chain growth free radicals. Using olefin monomers containing unsaturated double bonds as raw materials, the double bonds in the monomer molecules are opened, and repeated addition reactions are carried out between molecules to connect many monomers to form macromolecules. Sodium propylene sulfonate is used as a functional monomer in the synthesis to improve the strength. Thiol compounds can play a role in regulating molecular weight as chain transfer agents; hydrogen peroxide and persulfate are used as oxidants together, and the three together with the E51 reducing agent in material B promote the initiator.

[0026] The beneficial effects of the present invention are:

[0027] The present invention sets the raw material components of the reinforcing auxiliary agent, and the addition of polycarboxylic acid water reducing mother liquor is beneficial to improving the compressive strength and Mohs hardness; the addition of polyethylene glycol monomethyl ether as a viscosity regulator can reduce the amount of epoxy resin used when preparing organic terrazzo; the addition of an emulsifier can reduce the surface tension of the system, thereby reducing its interfacial energy and improving the stability of the solution, so that the obtained reinforcing auxiliary agent is added to the organic terrazzo in an amount of 5-8% of the amount of epoxy resin used, which can improve the compressive strength and Mohs hardness of the organic terrazzo, reduce the amount of epoxy resin used, have low cost, good environmental protection, and save resources. DETAILED DESCRIPTION

[0028] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the present invention is not limited to the following embodiments.

[0029] Example 1

[0030] A reinforcing additive for organic terrazzo, wherein the raw materials for its preparation include the following components by weight percentage: 18% polycarboxylic acid water reducing solution, 80% polyethylene glycol monomethyl ether, and 2% emulsifier. The polycarboxylic acid water reducing solution includes the following components by weight: 1 part of isopentyl polyoxyethylene ether macromonomer, 0.08 part of sodium propylene sulfonate, 0.1 part of general monomer, 0.003 part of mercapto compound, 0.001 part of E51 reducing agent, 0.004 part of hydrogen peroxide, and 0.005 part of persulfate.

[0031] Specifically, the general monomer is acrylic acid, the molecular weight of the polyethylene glycol monomethyl ether is 400, the thiol compound is mercaptopropionic acid, the persulfate is ammonium persulfate, and the molecular weight of the isopentenyl polyoxyethylene ether macromonomer is 3000.

[0032] The method for preparing the reinforcing agent for organic terrazzo comprises the following steps:

[0033] Step 1: Synthesize polycarboxylate water-reducing mother liquor:

[0034] a. Prepare material A: weigh general monomer, thiol compound and deionized water, and mix them evenly;

[0035] b. Prepare material B: weigh E51 reducing agent and deionized water and mix them evenly;

[0036] c. Add deionized water at a temperature of 5°C into the reactor, then add isopentenyl polyoxyethylene ether macromonomer and sodium propylene sulfonate in sequence, and start the stirrer to stir and dissolve for 30 minutes;

[0037] d. Add persulfate and hydrogen peroxide to the reactor and stir for 3 minutes;

[0038] e. Add material A and material B to the reactor at the same time, the addition time of material A is 120 minutes, and the addition time of material B is 150 minutes. The temperature of the reactor is controlled at 15°C. After the addition is completed, the temperature is kept warm for 60 minutes; after the insulation is completed, a sodium hydroxide solution with a mass concentration of 30% is added to adjust the pH value to 6, and the solid content of the mother liquor is adjusted to 40%, that is, the polycarboxylic acid water-reducing mother liquor is obtained;

[0039] Step 2: Mix the polycarboxylic acid water-reducing concentrate described in step 1 with polyethylene glycol monomethyl ether and an emulsifier to obtain a reinforcing agent for organic terrazzo.

[0040] Specifically, the amount of deionized water in step a is equal to that of general monomers; the amount of deionized water in step b is 15% of the isopentenyl polyoxyethylene ether macromonomer; and the amount of deionized water in step c is 66% of the isopentenyl polyoxyethylene ether macromonomer.

[0041] 5 parts by weight of the reinforcing agent obtained above were uniformly mixed with 100 parts by weight of epoxy resin, 20 parts by weight of aggregate, and 10 parts by weight of curing agent, and then cured to obtain an organic terrazzo, which was marked as A1.

[0042] 5 parts by weight of the reinforcing agent obtained above were uniformly mixed with 91 parts by weight of epoxy resin, 20 parts by weight of aggregate, and 10 parts by weight of curing agent, and then cured to obtain an organic terrazzo, which was marked as A2.

[0043] Example 2

[0044] A reinforcing agent for organic terrazzo, wherein the raw materials for its preparation include the following components by weight percentage: 22% polycarboxylic acid water reducing solution, 75% polyethylene glycol monomethyl ether, and 3% emulsifier. The polycarboxylic acid water reducing solution includes the following components by weight: 1 part of isopentyl polyoxyethylene ether macromonomer, 0.1 part of sodium propylene sulfonate, 0.15 part of general monomer, 0.0035 part of mercapto compound, 0.0015 part of E51 reducing agent, 0.005 part of hydrogen peroxide, and 0.006 part of persulfate.

[0045] Specifically, the general monomer is methacrylic acid, the molecular weight of the polyethylene glycol monomethyl ether is 600, the thiol compound is thioglycolic acid, the persulfate is potassium persulfate, and the molecular weight of the isopentenyl polyoxyethylene ether macromonomer is 3000.

[0046] The method for preparing the reinforcing agent for organic terrazzo comprises the following steps:

[0047] Step 1: Synthesize polycarboxylate water-reducing mother liquor:

[0048] a. Prepare material A: weigh general monomer, thiol compound and deionized water, and mix them evenly;

[0049] b. Prepare material B: weigh E51 reducing agent and deionized water and mix them evenly;

[0050] c. Add deionized water at a temperature of 10°C into the reactor, then add isopentenyl polyoxyethylene ether macromonomer and sodium propylene sulfonate in sequence, and start the stirrer to stir and dissolve for 30 minutes;

[0051] d. Add persulfate and hydrogen peroxide to the reactor and stir for 3 minutes;

[0052] e. Add material A and material B to the reactor at the same time, the addition time of material A is 120 minutes, and the addition time of material B is 150 minutes. The temperature of the reactor is controlled at 20°C. After the addition is completed, the temperature is kept warm for 60 minutes; after the insulation is completed, a sodium hydroxide solution with a mass concentration of 30% is added to adjust the pH value to 7, and the solid content of the mother liquor is adjusted to 40%, that is, the polycarboxylic acid water-reducing mother liquor is obtained;

[0053] Step 2: Mix the polycarboxylic acid water-reducing concentrate described in step 1 with polyethylene glycol monomethyl ether and an emulsifier to obtain a reinforcing agent for organic terrazzo.

[0054] Specifically, the amount of deionized water in step a is equal to that of general monomers; the amount of deionized water in step b is 18% of the isopentenyl polyoxyethylene ether macromonomer; and the amount of deionized water in step c is 66% of the isopentenyl polyoxyethylene ether macromonomer.

[0055] 5 parts by weight of the reinforcing agent obtained above were uniformly mixed with 100 parts by weight of epoxy resin, 20 parts by weight of aggregate, and 10 parts by weight of curing agent, and then cured to obtain an organic terrazzo, which was marked as B1.

[0056] 5 parts by weight of the reinforcing agent obtained above were uniformly mixed with 92 parts by weight of epoxy resin, 20 parts by weight of aggregate, and 10 parts by weight of curing agent, and then cured to obtain an organic terrazzo, which was marked as B2.

[0057] Example 3

[0058] A reinforcing additive for organic terrazzo, wherein the raw materials for its preparation include the following components by weight percentage: 28% polycarboxylic acid water reducing solution, 70% polyethylene glycol monomethyl ether, and 2% emulsifier. The polycarboxylic acid water reducing solution includes the following components by weight: 1 part of isopentyl polyoxyethylene ether macromonomer, 0.2 part of sodium propylene sulfonate, 0.2 part of general monomer, 0.004 part of mercapto compound, 0.002 part of E51 reducing agent, 0.006 part of hydrogen peroxide, and 0.007 part of persulfate.

[0059] Specifically, the general monomer is acrylic acid, the molecular weight of the polyethylene glycol monomethyl ether is 750, the thiol compound is a mixture of thioglycolic acid and thioethanol, the persulfate is a mixture of potassium persulfate and sodium persulfate, and the molecular weight of the isopentenyl polyoxyethylene ether macromonomer is 3000.

[0060] The method for preparing the reinforcing agent for organic terrazzo comprises the following steps:

[0061] Step 1: Synthesize polycarboxylate water-reducing mother liquor:

[0062] a. Prepare material A: weigh general monomer, thiol compound and deionized water, and mix them evenly;

[0063] b. Prepare material B: weigh E51 reducing agent and deionized water and mix them evenly;

[0064] c. Add deionized water at a temperature of 15°C into the reactor, then add isopentenyl polyoxyethylene ether macromonomer and sodium propylene sulfonate in sequence, and start the stirrer to stir and dissolve for 30 minutes;

[0065] d. Add persulfate and hydrogen peroxide to the reactor and stir for 3 minutes;

[0066] e. Add material A and material B to the reactor at the same time, the addition time of material A is 120 minutes, and the addition time of material B is 150 minutes. The temperature of the reactor is controlled at 20°C. After the addition is completed, the temperature is kept warm for 60 minutes; after the insulation is completed, a sodium hydroxide solution with a mass concentration of 30% is added to adjust the pH value to 8.5, and the solid content of the mother liquor is adjusted to 40%, thereby obtaining a polycarboxylic acid water-reducing mother liquor;

[0067] Step 2: Mix the polycarboxylic acid water-reducing concentrate described in step 1 with polyethylene glycol monomethyl ether and an emulsifier to obtain a reinforcing agent for organic terrazzo.

[0068] Specifically, the amount of deionized water in step a is equal to that of general monomers; the amount of deionized water in step b is 20% of the isopentenyl polyoxyethylene ether macromonomer; and the amount of deionized water in step c is 66% of the isopentenyl polyoxyethylene ether macromonomer.

[0069] 5 parts by weight of the reinforcing agent obtained above were uniformly mixed with 100 parts by weight of epoxy resin, 20 parts by weight of aggregate, and 10 parts by weight of curing agent, and then cured to obtain an organic terrazzo, marked as C1.

[0070] 5 parts by weight of the reinforcing agent obtained above were uniformly mixed with 93 parts by weight of epoxy resin, 20 parts by weight of aggregate, and 10 parts by weight of curing agent, and then cured to obtain an organic terrazzo, marked as C2.

[0071] Comparative Example 1

[0072] 100 parts by weight of epoxy resin, 20 parts by weight of aggregate, and 10 parts by weight of curing agent are uniformly mixed and then cured to obtain an organic terrazzo, which is marked as D1.

[0073] The performance of the organic terrazzo obtained in Examples 1-3 and Comparative Example 1 was tested, and the test results are shown in Table 1:

[0074] Table 1

[0075]

[0076] As can be seen from Table 1 above, adding the reinforcing agent of the present invention to organic terrazzo can effectively improve the compressive strength and Mohs hardness of the organic terrazzo. Moreover, when it is necessary to obtain organic terrazzo with the same performance, adding the reinforcing agent of the present invention can help reduce the amount of epoxy resin used, which is low in cost, good in environmental protection, and saves resources.

[0077] The above description is only a preferred embodiment of the present invention, so all equivalent changes or modifications made according to the structure, characteristics and principles described in the scope of the patent application of the present invention are included in the scope of the patent application of the present invention.

Claims

1. A reinforcing agent for organic terrazzo, characterized in that: The raw materials for its preparation include the following components by mass percentage: 18-28% of polycarboxylic acid water-reducing mother liquid, 70-80% of polyethylene glycol monomethyl ether, and 2-3% of emulsifier; The polycarboxylate water-reducing concentrate comprises the following components in parts by weight: 1 part of isopentenyl polyoxyethylene ether macromonomer, 0.08-0.15 parts of sodium propylene sulfonate, 0.1-0.2 parts of general monomers, 0.003-0.004 parts of thiol compounds, 0.001-0.002 parts of E51 reducing agent, 0.004-0.006 parts of hydrogen peroxide, and 0.005-0.007 parts of persulfate; The gelling material of the organic terrazzo is epoxy resin.

2. The reinforcing agent for organic terrazzo according to claim 1, characterized in that: The general monomer is one of acrylic acid and methacrylic acid.

3. The reinforcing agent for organic terrazzo according to claim 1, characterized in that: The molecular weight of the polyethylene glycol monomethyl ether is 400-750.

4. The reinforcing agent for organic terrazzo according to claim 1, characterized in that: The thiol compound includes at least one of mercaptopropionic acid, thioglycolic acid, and mercaptoethanol.

5. The reinforcing agent for organic terrazzo according to claim 1, characterized in that: The persulfate includes at least one of ammonium persulfate, potassium persulfate, and sodium persulfate.

6. The reinforcing agent for organic terrazzo according to claim 1, characterized in that: The molecular weight of the isopentenyl polyoxyethylene ether macromonomer is 3,000.

7. A method for preparing the reinforcing agent for organic terrazzo according to any one of claims 1 to 6, comprising the following steps: Step 1: Synthesize polycarboxylate water-reducing mother liquor: a. Prepare material A: weigh general monomer, thiol compound and deionized water, mix them evenly and set aside; b. Prepare material B: weigh E51 reducing agent and deionized water, mix them evenly and set aside; c. Add deionized water at a temperature of 5-15°C into the reactor, then add isopentenyl polyoxyethylene ether macromonomer and sodium propylene sulfonate in sequence, and start the stirrer to stir and dissolve for 30 minutes; d. Add persulfate and hydrogen peroxide to the reactor and stir for 3 minutes; e. Add material A and material B to the reactor at the same time, the addition time of material A is 120 minutes, and the addition time of material B is 150 minutes. The temperature of the reactor is controlled at 15-25° C., and the temperature is kept warm for 60 minutes after the addition is completed; after the insulation is completed, a sodium hydroxide solution with a mass concentration of 30% is added to adjust the pH value to between 6 and 8.5, and the solid content of the mother liquor is adjusted to 40%, so as to obtain a polycarboxylic acid water-reducing mother liquor; Step 2: Mix the polycarboxylic acid water-reducing concentrate described in step 1 with polyethylene glycol monomethyl ether and an emulsifier to obtain a reinforcing agent for organic terrazzo.

8. The method for preparing a reinforcing agent for organic terrazzo according to claim 7, characterized in that: The deionized water in step a is equal to the general monomer; the deionized water in step b is 15-20% of the isopentenyl polyoxyethylene ether macromonomer; and the deionized water in step c is 66% of the isopentenyl polyoxyethylene ether macromonomer.

Citation Information

Patent Citations

  • Polycarboxylic acid slump retaining agent with low bleeding rate and preparation method thereof

    CN104973816A

  • Non-ionic waterborne epoxy curing agent and preparation method thereof

    CN105482079A

  • Water-based epoxy resin emulsion prepared by utilizing emulsifying agent comprising single or double epoxy groups

    CN107151334A

  • Water reducing agent for tunnel concrete

    CN110436818A

  • Waterborne epoxy self-leveling mortar and preparation method thereof

    CN114105563A