A kind of filler material for converter bottom and preparation method thereof
By adjusting the component proportions and particle sizes of forsterite, magnesium spinel bricks, modified asphalt and spherical asphalt, and combining metal aluminum powder as a binding agent, the poor spreading performance and sintering time of the existing converter bottom patching materials are solved long problem, achieving the effects of efficient spreading, short sintering time and long service life.
Patent Information
- Application Number
- CN202211088419.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-07
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-09-07
AI Technical Summary
The existing converter bottom patching materials have poor spreading performance, long sintering time, and low service life, which affects the smelting rhythm of the steel plant and the bottom blowing effect of the furnace bottom.
Use 20-30% forsterite, 45-55% post-consumer magnesium spinel bricks, 15-20% modified asphalt, 3-6% spherical asphalt, and 0.5-1.5% metal aluminum powder as the Binder, by adjusting raw material particle size and component ratio, improves spreading performance, shortens sintering time, enhances erosion resistance and service life.
It achieves efficient spreading, short sintering time, good erosion resistance and long service life, and improves the smelting efficiency of steel plants and the bottom blowing effect of furnace bottom.
Smart Images

Figure BDA0003836120350000041 
Figure BDA0003836120350000051 
Figure BDA0003836120350000052
Abstract
Description
Technical Field
[0001] The invention relates to the field of refractory materials for steelmaking, and in particular to a filler material for a converter bottom and a preparation method thereof. Background Art
[0002] With the continuous advancement of steelmaking technology, steel mills have higher and higher requirements for the life of converter bottom blowing, which has caused serious damage to the bottom of the converter and requires continuous hot maintenance. At present, most steel mills still use carbon-containing repair materials with tar pitch or resin as binders for converter bottom maintenance, which have problems such as poor spreading performance, long sintering time and low service life, which will not only affect the smelting rhythm of the steel mill, but also affect the bottom blowing effect of the converter bottom. Summary of the invention
[0003] In order to overcome the above problems, the purpose of the present invention is to provide a repair material for converter bottom and a preparation method thereof, which has the characteristics of good spreading performance, short sintering time, good anti-scouring performance and long service life.
[0004] To achieve the above-mentioned purpose, the converter bottom filler designed in the present invention comprises the following components and weight percentages: 20-30% forsterite, 45-55% used magnesium spinel bricks, 15-20% modified asphalt, 3-6% spherical asphalt, 0.5-1.5% additives, and 0.5-1% combustion promoter; the additive is metallic aluminum powder with a particle size of -180 mesh; the combustion promoter is one of kerosene or diesel.
[0005] As a preferred solution, the modified asphalt has a softening point of 105-120°C, a coking value of ≥55%, and a particle size of ≤3mm and >0.088mm; the spherical asphalt has a softening point of ≥170°C, a residual carbon rate of ≥60%, and a particle size of ≤2mm and >0.088mm. The particle size of the two asphalts cannot be too large, if it is larger than 3mm, it cannot melt quickly and thus affect the sintering time. The asphalt particle size cannot be too small, if it is smaller than 0.088mm, it will affect the fluidity of the supplementary furnace charge.
[0006] As a preferred solution, the used magnesium spinel brick material has a MgO content of ≥88%, and is divided into three gradations according to the particle size: ≤3mm and >1mm, ≤1mm and >0.088mm, and ≤0.088, with weight percentages of 30-40%, 35-45%, and 20-30%, respectively. Selecting the used magnesium spinel brick material with small particles of the three gradations is beneficial to improving the corrosion resistance of the furnace filling material.
[0007] As a preferred embodiment, the method for preparing the used magnesium spinel brick material comprises the following steps:
[0008] 1) Select and use magnesium spinel bricks, remove surface impurities, and crush them into ≤5mm and >0.088mm;
[0009] 2) The spent magnesium spinel bricks are shaped for 30 to 50 minutes, and then vibrated and screened to obtain spent magnesium spinel brick materials with three particle sizes of ≥3mm, 3mm≤ and >1mm, and ≤1mm and >0.088mm; the specific shaping process is to put the crushed spent magnesium spinel bricks into a drum mill, and during the rotation of the drum mill, the spent magnesium spinel brick particles rub against each other to obtain spent magnesium spinel brick particles with a smooth appearance;
[0010] 3) grinding the used magnesium spinel brick material with a particle size of ≥3 mm to obtain used magnesium spinel brick material powder with a particle size of ≤0.088 mm;
[0011] 4) Three gradations of particle sizes of ≤3mm and >1mm, ≤1mm and >0.088mm, and ≤0.088 are mixed at weight percentages of 30-40%, 35-45%, and 20-30% respectively to obtain used magnesium spinel brick materials.
[0012] As a preferred solution, the forsterite is divided into two gradations according to the particle size: ≤10mm and >5mm and ≤5mm and >3mm, and the weight percentages are 50-60% and 40-50% respectively. Selecting two gradations of large-particle olivine raw materials is beneficial to improving the sintering strength of the repairing furnace material without affecting the corrosion resistance of the repairing furnace material.
[0013] As a preferred solution, the forsterite has a MgO content of ≥40%, and SiO 2 The content is ≤40%.
[0014] A method for preparing a furnace filler material for a converter bottom comprises the following steps:
[0015] 1) Weigh forsterite, used magnesium spinel brick material, modified asphalt, spherical asphalt, additives, and combustion promoter for use;
[0016] 2) Mix forsterite, used magnesium spinel bricks, modified asphalt, spherical asphalt and additives in a stirrer for 3 to 5 minutes, then add a combustion promoter and stir for 10 to 15 minutes to obtain a high-efficiency furnace filler for the converter bottom.
[0017] In the present invention, 15-20% of modified asphalt and 3-6% of spherical asphalt are used as binders. The modified asphalt has a low softening point and a high coking value, while the spherical asphalt has a high softening point and a high residual carbon rate. Due to its spherical characteristics, it is easier to flow and spread during use. The combination of the two can not only improve the spreading performance of the repair charge at medium temperature and shorten the sintering time, but also improve the adhesion and strength of the repair charge at high temperature, thereby improving the anti-scouring performance and service life of the repair charge.
[0018] The additive metal aluminum powder is introduced in the present invention, which can improve the high-temperature strength of the furnace repair material on the one hand, and on the other hand, the aluminum powder releases heat at high temperature to promote the sintering of the furnace repair material, further shortening the sintering time.
[0019] In the present invention, large particles are made of forsterite, which has a low melting point and can produce a small amount of liquid phase at the use temperature, thereby promoting the sintering of the furnace repair charge at a high temperature; small particles and the matrix are made of shaped used magnesium spinel brick materials, the main components of which are large crystalline magnesia sand, magnesium spinel, and a small amount of magnesium aron whiskers and aluminum nitride whiskers. The used materials have large grains and high strength, and can improve the corrosion resistance and scouring resistance of the furnace repair charge. At the same time, by shaping them, particles with a smoother appearance can be obtained, which is useful for improving the spreadability of the furnace repair charge.
[0020] In addition, since the binder in the repair charge is modified asphalt and spherical asphalt, the addition of spherical asphalt can strengthen the network structure after carbonization of the asphalt and improve the high-temperature erosion resistance of the repair charge; the present invention introduces used magnesium spinel bricks and forsterite as main raw materials into the repair charge for the converter bottom, and strictly controls the addition amount of the two, which can stabilize the material composition, adjust the volume expansion of the repair charge during the spinelization reaction at high temperature, and improve the thermal stability of the material, thereby increasing the service life. DETAILED DESCRIPTION
[0021] In order to better understand the present invention, the invention will be described in detail below in conjunction with specific examples.
[0022] To avoid repetition, the particle sizes of the raw materials involved in this specific implementation are first described uniformly and will not be described in detail in the examples.
[0023] The preparation method of the converter bottom filling material is as follows: weigh 20-30% of forsterite, 45-55% of used magnesium spinel bricks, 15-20% of modified asphalt, 3-6% of spherical asphalt, and 0.5-1.5% of additives, mix them in a stirrer for 3-5 minutes, then add 0.5-1% of a combustion promoter and stir for 10-15 minutes to obtain a high-efficiency converter bottom filling material.
[0024] Among them, the additive is metal aluminum powder with a particle size of -180 mesh;
[0025] The combustion promoter is one of kerosene or diesel;
[0026] The modified asphalt has a softening point of 105-120°C, a coking value of ≥55%, and a particle size of ≤3mm and >0.088mm; the spherical asphalt has a softening point of ≥170°C, a residual carbon rate of ≥60%, and a particle size of ≤2mm and >0.088mm.
[0027] The used magnesium spinel brick material has a MgO content of ≥88%, and is divided into three gradations according to the particle size: ≤3mm and >1mm, ≤1mm and >0.088mm, and ≤0.088mm, and their weight percentages are 30-40%, 35-45%, and 20-30% respectively.
[0028] Forsterite is divided into two gradations according to particle size: ≤10mm and >5mm and ≤5mm and >3mm, and their weight percentages are 50-60% and 40-50% respectively.
[0029] The method for preparing the post-use magnesium spinel brick material comprises the following steps:
[0030] 1) Select and use magnesium spinel bricks, remove surface impurities, and crush them into ≤5mm and >0.088mm;
[0031] 2) The spent magnesium spinel bricks are shaped for 30 to 50 minutes, and then vibrated and screened to obtain spent magnesium spinel brick materials with three particle sizes of ≥3mm, 3mm≤ and >1mm, and ≤1mm and >0.088mm; the specific shaping process is to put the crushed spent magnesium spinel bricks into a drum mill, and during the rotation of the drum mill, the spent magnesium spinel brick particles rub against each other to obtain spent magnesium spinel brick particles with a smooth appearance;
[0032] 3) grinding the used magnesium spinel brick material with a diameter of ≥3 mm after shaping to obtain used magnesium spinel brick material powder with a diameter of ≤0.088;
[0033] 4) Three gradations of particle sizes of ≤3mm and >1mm, ≤1mm and >0.088mm, and ≤0.088 are mixed at weight percentages of 30-40%, 35-45%, and 20-30% respectively to obtain used magnesium spinel brick materials.
[0034] Table 1 Proportion of components of the filler material for the converter bottom in Examples 1 to 5
[0035]
[0036]
[0037] Table 2 Grading of magnesium spinel brick materials after use
[0038]
[0039] Table 3 Grading of forsterite
[0040]
[0041] Comparative Example 1
[0042] The traditional converter bottom filling material has the following components and contents: 50 parts of fused magnesia, 35 parts of sintered magnesia and 15 parts of tar pitch.
[0043] Comparative Example 2
[0044] The traditional converter bottom filling material has the following components and contents: 55 parts of sintered magnesia, 35 parts of fused magnesia and 10 parts of resin.
[0045] Comparative Example 3
[0046] The traditional converter bottom filling material has the following components and contents: 52 parts of sintered magnesia, 35 parts of fused skin sand, and 13 parts of tar pitch.
[0047] Table 4 Performance of the filler material for converter bottom
[0048]
[0049] As can be seen from Table 4, the converter bottom filling material of the present invention has the following advantages:
[0050] (1) Compared with the comparative example, the flow index at 1100°C of the embodiment of the present invention is significantly improved, indicating that the spreading performance of the embodiment is significantly improved.
[0051] (2) Compared with the comparative example, the sintering time at 1100° C. is significantly shortened in the embodiments of the present invention.
[0052] (3) Compared with the comparative example, the adhesion rate of the embodiment of the present invention is significantly improved after one furnace, indicating that the anti-scouring performance of the embodiment is significantly improved.
[0053] (4) Compared with the comparative example, the service life of the embodiments of the present invention is improved.
Claims
1. A filler material for converter bottom, characterized in that: Its components and weight percentage content are: 20-30% forsterite, 45-55% used magnesium spinel brick material, 15-20% modified asphalt, 3-6% spherical asphalt, 0.5-1.5% additives, and 0.5-1% sintering agent; The additive is aluminum powder with a particle size of -180 mesh; The combustion promoter is one of kerosene or diesel; The modified asphalt has a softening point of 105-120°C, a coking value of ≥55%, and a particle size of ≤3mm and >0.088mm; the spherical asphalt has a softening point of ≥170°C, a residual carbon rate of ≥60%, and a particle size of ≤2mm and >0.088mm; The used magnesium spinel brick material has a MgO content of ≥88%, and is divided into three gradations according to the particle size: ≤3mm and >1mm, ≤1mm and >0.088mm, and ≤0.088, and their weight percentages are 30-40%, 35-45%, and 20-30% respectively; The method for preparing the used magnesium spinel brick material comprises the following steps: 1) Select and use magnesium spinel bricks, remove surface impurities, and crush them into ≤5mm and >0.088mm; 2) shaping the used magnesium spinel brick for 30 to 50 minutes, and then vibrating and screening to obtain used magnesium spinel brick materials with three particle sizes of ≥3 mm, 3 mm ≤ and >1 mm, and ≤1 mm and >0.088 mm; 3) grinding the used magnesium spinel brick material with a diameter of ≥3 mm after shaping to obtain used magnesium spinel brick material powder with a diameter of ≤0.088; 4) Three gradations of particle sizes of ≤3 mm and >1 mm, ≤1 mm and >0.088 mm, and ≤0.088 are mixed at weight percentages of 30-40%, 35-45%, and 20-30% to obtain used magnesium spinel brick materials; The forsterite is divided into two gradations according to the particle size: ≤10mm and >5mm and ≤5mm and >3mm, and the weight percentages thereof are 50-60% and 40-50% respectively; The forsterite has a MgO content of ≥40% and a SiO2 content of ≤40%.
2. A method for preparing the converter bottom filler material as claimed in claim 1, characterized in that: The following steps are involved: 1) Weigh forsterite, used magnesium spinel brick material, modified asphalt, spherical asphalt, additives, and combustion promoter for use; 2) Mix forsterite, used magnesium spinel bricks, modified asphalt, spherical asphalt and additives in a stirrer for 3 to 5 minutes, then add a combustion promoter and stir for 10 to 15 minutes to obtain a high-efficiency furnace filler for the converter bottom.