A kind of heat-resistant and corrosion-resistant coating on aluminum alloy surface and preparation method thereof

By forming a combined technology of nano-silica film and epoxy resin base coating on the surface of aluminum alloy, the problem of low adhesion of existing aluminum alloy surface coatings is solved, and the high-temperature and high-corrosion performance of aluminum alloy is improved and extended. product life.

CN116285602BActive Publication Date: 2024-10-08HUZHOU BAOYUN LEISURE PROD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310310317.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-08
Estimated Expiration
2043-03-28

AI Technical Summary

Technical Problem

The existing aluminum alloy surface coating has low adhesion and is difficult to maintain in corrosive media, resulting in poor anti-corrosion effect. It is prone to pitting corrosion at high temperatures and shortens product life.

Method used

A coupling agent mixture and nano-silica powder are used to form a temperature-resistant coating, and the surface is coated with a corrosion-resistant coating composed of epoxy resin, polyethylene glycol, diluent and boron trifluoride ether. Specific process steps and treatments improve adhesion and insulation.

Benefits of technology

Significantly improves the temperature and corrosion resistance of aluminum alloys, ensuring strong adhesion of the coating under high temperatures and corrosive environments, preventing oxidation weight loss and corrosion, and extending product life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a heat-resistant and corrosion-resistant coating on the surface of an aluminum alloy and a preparation method thereof. The coating comprises a heat-resistant coating and a corrosion-resistant coating sequentially attached to the surface of the aluminum alloy; the heat-resistant coating comprises the following raw materials in parts by weight: 100 parts of a coupling agent mixture, 3 to 5 parts of nano-silicon dioxide powder, and 1 to 3 parts of an active agent; the corrosion-resistant coating comprises the following raw materials in parts by weight: 100 to 120 parts of a water-based epoxy resin, 20 to 25 parts of polyethylene glycol powder, 5.5 to 12 parts of boron trifluoride etherate, and 100 to 160 parts of a diluent. The preparation method comprises: immersing the pretreated aluminum alloy in a heat-resistant coating liquid, curing, forming a heat-resistant coating, and then coating the corrosion-resistant coating liquid on the surface of the heat-resistant coating, curing, and obtaining a heat-resistant and corrosion-resistant coating attached to the surface of the aluminum alloy. The heat-resistant and corrosion-resistant coating prepared by the invention has strong adhesion to the surface of the aluminum alloy, and can significantly improve the heat resistance and corrosion resistance of the aluminum alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings, and in particular relates to a heat-resistant and corrosion-resistant coating on the surface of an aluminum alloy and a preparation method thereof. Background Art

[0002] When aluminum alloy is in the air, an aluminum oxide protective film will form on its surface. Under normal atmospheric conditions, this protective film can effectively protect the aluminum alloy substrate. However, under certain temperature and ambient humidity, pitting corrosion will occur on the aluminum alloy surface, seriously damaging the product's appearance and shortening the product's service life.

[0003] In order to improve the corrosion resistance of aluminum alloy products, modern processes often use organic coatings on the surface of aluminum alloys. Invention patent application: Metal surface treatment agent and method for treating metal surface (publication number CN101139500A), it is proposed that silane coupling agent, organic metal compound, silicate, phosphoric acid and other components are evenly scraped on the metal surface by using a wire rod, and heated and dried to form a coating to improve the appearance and physical and chemical properties of aluminum alloy; Invention patent application: A metal surface treatment liquid and its use method (publication number CN1341775A), it is proposed that the metal surface treatment liquid is composed of nine raw materials such as sodium dodecyl sulfate, sodium hydroxide, citric acid, etc., and the coating is formed by immersion on the metal surface. However, the coating formed by the above method has low adhesion to the metal surface, the coating is easy to fall off in the corrosive medium, and the anti-corrosion effect is poor. Summary of the invention

[0004] The purpose of the present invention is to overcome the deficiencies in the prior art and to provide a heat-resistant and corrosion-resistant coating on the surface of an aluminum alloy and a preparation method thereof. The prepared heat-resistant and corrosion-resistant coating has strong adhesion to the surface of the aluminum alloy and can significantly improve the heat resistance and corrosion resistance of the aluminum alloy.

[0005] The present invention provides the following technical solutions:

[0006] In a first aspect, a heat-resistant and corrosion-resistant coating on an aluminum alloy surface is provided, comprising a heat-resistant coating and a corrosion-resistant coating sequentially attached to the surface of the aluminum alloy;

[0007] The heat-resistant coating comprises the following raw materials in parts by weight: 100 parts of coupling agent mixture, 3-5 parts of nano silicon dioxide powder, and 1-3 parts of active agent;

[0008] The corrosion-resistant coating comprises the following raw materials in parts by weight: 100-120 parts of epoxy resin, 20-25 parts of polyethylene glycol powder, 5.5-12 parts of boron trifluoride ether, and 100-160 parts of diluent.

[0009] Furthermore, the coupling agent mixture is composed of KH-550 silane coupling agent, ethanol and deionized water in a volume ratio of 1-1.5:8-10:10-15.

[0010] Furthermore, the non-ionic surfactant is specifically one of polyoxyethylene oleyl alcohol ether type surfactant, ethoxylated methyl glucoside stearate type surfactant or Tween 20 type surfactant (polyoxyethylene sorbitan monolaurate), preferably polyoxyethylene oleyl alcohol ether type surfactant.

[0011] Furthermore, the epoxy equivalent of the epoxy resin is 185-200 g / eq, and the polyethylene glycol is PEG4000.

[0012] In a second aspect, a method for preparing a heat-resistant and corrosion-resistant coating on an aluminum alloy surface is provided, comprising the following steps:

[0013] Add 3-5 parts by weight of nano silicon dioxide powder to 100 parts of the coupling agent mixed solution, stir, and drop 1-3 parts of the activator to obtain a temperature-resistant coating solution;

[0014] 100-120 parts by weight of epoxy resin and 50-80 parts by weight of diluent are mixed, 20-25 parts of polyethylene glycol powder are added, the temperature is raised and stirred, and then 5.5-12 parts of boron trifluoride ether are added dropwise, and after continuous stirring to obtain a light yellow viscous polymer, 50-80 parts of diluent are added to obtain a corrosion-resistant coating liquid;

[0015] The pretreated aluminum alloy is immersed in the heat-resistant coating liquid, taken out, blown dry and cured to form a heat-resistant coating on the surface of the aluminum alloy, and then the corrosion-resistant coating liquid is coated on the surface of the heat-resistant coating and cured to obtain a heat-resistant and corrosion-resistant coating attached to the surface of the aluminum alloy.

[0016] Furthermore, the aluminum alloy pretreatment method includes: grinding the aluminum alloy surface with water sandpaper, then mechanically polishing it to a mirror surface, and washing it with deionized water, and blowing it dry with cold air; then alkaline etching in a 10% mass fraction sodium hydroxide solution at 60~70°C for 5 minutes, and washing it with deionized water; then deashing in a 30% volume fraction nitric acid solution, washing it with deionized water, and blowing it dry with cold air.

[0017] Furthermore, the specific preparation method of the temperature-resistant coating liquid includes: mixing KH-550 silane coupling agent, ethanol and deionized water in a volume ratio of 1~1.5:8~10:10~15 to prepare a coupling agent mixed liquid, adding 3~5 parts by weight of nano-silicon dioxide powder to 100 parts of the coupling agent mixed liquid, stirring with a magnetic stirrer, and simultaneously adding 1~3 parts of an activator to obtain the obtained product.

[0018] Furthermore, the specific preparation method of the corrosion-resistant coating liquid includes: mixing 100-120 parts by weight of epoxy resin and 50-80 parts of diluent, stirring for 30 minutes at a speed of 60-80 r / min using a stirrer, adding 20-25 parts of polyethylene glycol powder, heating to 75-90°C, stirring for 3-4 hours at a speed of 60-80 r / min using a stirrer under nitrogen protection, adding 5.5-12 parts of boron trifluoride ether after mixing evenly, observing the reaction process, adjusting the stirring rate to 300-500 r / min, obtaining a light yellow viscous polymer, and then adding 50-80 parts of diluent, stirring and shaking for 5 minutes.

[0019] Furthermore, the preparation method of the heat-resistant coating includes: placing the pretreated aluminum alloy in the heat-resistant coating liquid and immersing it for 50 to 60 seconds, taking it out and blowing it dry, then curing it in an oven at a temperature of 100 to 130°C for 40 to 50 minutes, taking it out and cooling it to room temperature in the air to obtain the heat-resistant coating attached to the surface of the aluminum alloy.

[0020] Furthermore, the preparation method of the heat-resistant and corrosion-resistant coating includes: coating the corrosion-resistant coating liquid on the surface of the heat-resistant coating using a spin coater, and then curing it in an oven at a temperature of 80~100°C for 2~4h to obtain a heat-resistant and corrosion-resistant coating attached to the surface of the aluminum alloy.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The present invention forms a film containing nano silicon dioxide on the surface of the aluminum alloy through a coupling agent mixed liquid, that is, forms a heat-resistant coating on the surface of the aluminum alloy, thereby improving the heat resistance of the aluminum alloy; then, epoxy resin is used as a matrix, polyethylene glycol powder, boron trifluoride ether and a diluent are added to prepare a corrosion-resistant coating liquid, which is coated on the surface of the heat-resistant coating to form a corrosion-resistant coating with strong viscosity, strong adhesion and excellent isolation effect, and can effectively isolate the influence of the surrounding environment on the surface performance of the aluminum alloy, so that the aluminum alloy surface has good heat resistance and corrosion resistance. DETAILED DESCRIPTION

[0023] The following embodiments are only used to more clearly illustrate the technical solutions of the present invention, and are not intended to limit the protection scope of the present invention.

[0024] The epoxy resin in the following examples is selected from E51 (618) epoxy resin of Jinhong Glue Industry, with an epoxy equivalent of 185-200 g / eq; polyethylene glycol is selected from polyethylene glycol PEG4000 of Guangzhou Gaoyue Chemical Co., Ltd., and the diluent is selected from JH-5748 active diluent of Jinhong Glue Industry.

[0025] Example 1

[0026] This embodiment provides a method for preparing a heat-resistant and corrosion-resistant coating on the surface of an aluminum alloy, and the steps are as follows:

[0027] Step 1: Pretreatment of aluminum alloy.

[0028] The surface of the aluminum alloy was polished with water sandpaper and then mechanically polished to a mirror surface, washed with deionized water, and dried with cold air; then it was alkaline etched in a 10% mass fraction sodium hydroxide solution at 70°C for 5 minutes and washed with deionized water; then it was deashed in a 30% volume fraction nitric acid solution, washed with deionized water, and dried with cold air.

[0029] Step 2: Preparation of temperature-resistant coating liquid.

[0030] KH-550 silane coupling agent, ethanol and deionized water were mixed and stirred at a volume ratio of 1:8:10 for 1 hour to obtain a coupling agent mixture. 3 g of nano-silica powder was added to 100 g of the coupling agent mixture and stirred with a magnetic stirrer. At the same time, 1 g of ethoxylated methyl glucoside stearate type active agent was added dropwise to promote the dispersion of the nano-silica powder in the coupling agent mixture to obtain a temperature-resistant coating liquid.

[0031] Step 3: Preparation of corrosion-resistant coating liquid.

[0032] Mix 100g of epoxy resin and 50g of diluent, stir at 60r / min for 30min with a stirrer, pour the stirred resin solution into a four-necked flask with a thermometer, a stirring paddle and a nitrogen inlet, add 20g of polyethylene glycol powder, immerse the four-necked flask in a water bath, control the temperature at 75°C, fill the four-necked flask with nitrogen protection, stir at 60r / min for 3h with a stirrer, and after mixing evenly, slowly add 5ml of boron trifluoride ether through a dropping funnel, observe the reaction process, adjust the stirring rate to 300r / min, and obtain a light yellow viscous polymer. Then add 50g of diluent to the four-necked flask, stir and shake thoroughly for 5min to obtain a corrosion-resistant coating liquid.

[0033] Step 4: Preparation of heat-resistant and corrosion-resistant coating.

[0034] At room temperature, the pretreated aluminum alloy was immersed in the heat-resistant coating liquid for 50 seconds, taken out and blown dry, then cured in an oven at 130°C for 40 minutes, taken out and cooled to room temperature in air, and the heat-resistant coating attached to the surface of the aluminum alloy was obtained. The corrosion-resistant coating liquid was applied to the surface of the heat-resistant coating using a spin coater, and then cured in an oven at 80°C for 2 hours, and the heat-resistant and corrosion-resistant coating attached to the surface of the aluminum alloy was obtained.

[0035] Example 2

[0036] This embodiment provides a method for preparing a heat-resistant and corrosion-resistant coating on the surface of an aluminum alloy, and the steps are as follows:

[0037] Step 1: Pretreatment of aluminum alloy.

[0038] The surface of the aluminum alloy was polished with water sandpaper and then mechanically polished to a mirror surface, washed with deionized water, and dried with cold air; then it was alkaline etched in a 10% mass fraction sodium hydroxide solution at 70°C for 5 minutes and washed with deionized water; then it was deashed in a 30% volume fraction nitric acid solution, washed with deionized water, and dried with cold air.

[0039] Step 2: Preparation of temperature-resistant coating liquid.

[0040] KH-550 silane coupling agent, ethanol and deionized water were mixed and stirred at a volume ratio of 1:10:15 for 1 hour to obtain a coupling agent mixture. 5 g of nano-silica powder was added to 100 g of the coupling agent mixture, and the mixture was stirred with a magnetic stirrer. At the same time, 2 g of Tween 20 type active agent was added dropwise to promote the dispersion of the nano-silica powder in the coupling agent mixture to obtain a temperature-resistant coating liquid.

[0041] Step 3: Preparation of corrosion-resistant coating liquid.

[0042] Mix 120g of epoxy resin and 80g of diluent, stir at 80r / min for 30min with a stirrer, pour the stirred resin solution into a four-necked flask with a thermometer, a stirring paddle and a nitrogen inlet, add 25g of polyethylene glycol powder, immerse the four-necked flask in a water bath, control the temperature at 90°C, fill the four-necked flask with nitrogen protection, stir at 60r / min for 4h with a stirrer, and after mixing evenly, slowly add 10ml of boron trifluoride ether through a dropping funnel, observe the reaction process, adjust the stirring rate to 500r / min, and obtain a light yellow viscous polymer, then add 80g of diluent to the four-necked flask, stir and shake thoroughly for 5min to obtain a corrosion-resistant coating liquid.

[0043] Step 4: Preparation of heat-resistant and corrosion-resistant coating.

[0044] At room temperature, the pretreated aluminum alloy was immersed in the heat-resistant coating liquid for 60 seconds, taken out and blown dry, then cured in an oven at 100°C for 50 minutes, taken out and cooled to room temperature in air, and the heat-resistant coating attached to the surface of the aluminum alloy was obtained. The corrosion-resistant coating liquid was applied to the surface of the heat-resistant coating using a spin coater, and then cured in an oven at 80°C for 4 hours, and the heat-resistant and corrosion-resistant coating attached to the surface of the aluminum alloy was obtained.

[0045] Example 3

[0046] This embodiment provides a method for preparing a heat-resistant and corrosion-resistant coating on the surface of an aluminum alloy, and the steps are as follows:

[0047] Step 1: Pretreatment of aluminum alloy.

[0048] The surface of the aluminum alloy was polished with water sandpaper and then mechanically polished to a mirror surface, washed with deionized water, and dried with cold air; then it was alkaline etched in a 10% mass fraction sodium hydroxide solution at 65°C for 5 minutes and washed with deionized water; then it was deashed in a 30% volume fraction nitric acid solution, washed with deionized water, and dried with cold air.

[0049] Step 2: Preparation of temperature-resistant coating liquid.

[0050] KH-550 silane coupling agent, ethanol and deionized water were mixed and stirred at a volume ratio of 1.5:9:13 for 1 hour to obtain a coupling agent mixture. 4 g of nano-silica powder was added to 100 g of the coupling agent mixture and stirred with a magnetic stirrer. At the same time, 3 g of polyoxyethylene oleyl alcohol ether type active agent was added dropwise to promote the dispersion of the nano-silica powder in the coupling agent mixture to obtain a temperature-resistant coating liquid.

[0051] Step 3: Preparation of corrosion-resistant coating liquid.

[0052] Mix 110g of epoxy resin and 60g of diluent, stir at 70r / min for 30min with a stirrer, pour the stirred resin solution into a four-necked flask with a thermometer, a stirring paddle and a nitrogen inlet, add 23g of polyethylene glycol powder, immerse the four-necked flask in a water bath, control the temperature at 80°C, fill the four-necked flask with nitrogen protection, stir at 80r / min for 3h with a stirrer, and after mixing evenly, slowly add 10ml of boron trifluoride ether through a dropping funnel, observe the reaction process, adjust the stirring rate to 400r / min, and obtain a light yellow viscous polymer. Then add 60g of diluent to the four-necked flask, stir and shake thoroughly for 5min to obtain a corrosion-resistant coating liquid.

[0053] Step 4: Preparation of heat-resistant and corrosion-resistant coating.

[0054] At room temperature, the pretreated aluminum alloy was immersed in the heat-resistant coating liquid for 55 seconds, taken out and blown dry, then cured in an oven at 120°C for 45 minutes, taken out and cooled to room temperature in air, and the heat-resistant coating attached to the surface of the aluminum alloy was obtained. The corrosion-resistant coating liquid was applied to the surface of the heat-resistant coating using a spin coater, and then cured in an oven at 100°C for 2 hours, and the heat-resistant and corrosion-resistant coating attached to the surface of the aluminum alloy was obtained.

[0055] Example 4

[0056] This embodiment provides a method for preparing a heat-resistant and corrosion-resistant coating on the surface of an aluminum alloy, and the steps are as follows:

[0057] Step 1: Pretreatment of aluminum alloy.

[0058] The surface of the aluminum alloy was polished with water sandpaper and then mechanically polished to a mirror surface, washed with deionized water, and dried with cold air; then it was alkaline etched in a 10% mass fraction sodium hydroxide solution at 65°C for 5 minutes and washed with deionized water; then it was deashed in a 30% volume fraction nitric acid solution, washed with deionized water, and dried with cold air.

[0059] Step 2: Preparation of temperature-resistant coating liquid.

[0060] KH-550 silane coupling agent, ethanol and deionized water were mixed and stirred at a volume ratio of 1.2:10:12 for 1 hour to obtain a coupling agent mixture. 4 g of nano-silica powder was added to 100 g of the coupling agent mixture, and the mixture was stirred with a magnetic stirrer. At the same time, 2 g of polyoxyethylene oleyl alcohol ether type active agent was added dropwise to promote the dispersion of the nano-silica powder in the coupling agent mixture to obtain a temperature-resistant coating liquid.

[0061] Step 3: Preparation of corrosion-resistant coating liquid.

[0062] Mix 110g of epoxy resin and 70g of diluent, stir at 80r / min for 30min with a stirrer, pour the stirred resin solution into a four-necked flask with a thermometer, a stirring paddle and a nitrogen inlet, add 25g of polyethylene glycol powder, immerse the four-necked flask in a water bath, control the temperature at 80°C, fill the four-necked flask with nitrogen protection, stir at 80r / min for 3.5h with a stirrer, and after mixing evenly, slowly add 8ml of boron trifluoride ether through a dropping funnel, observe the reaction process, adjust the stirring rate to 400r / min, and obtain a light yellow viscous polymer, then add 70g of diluent to the four-necked flask, stir and shake thoroughly for 5min to obtain a corrosion-resistant coating liquid.

[0063] Step 4: Preparation of heat-resistant and corrosion-resistant coating.

[0064] At room temperature, the pretreated aluminum alloy was immersed in the heat-resistant coating liquid for 60 seconds, taken out and blown dry, then cured in an oven at 110°C for 50 minutes, taken out and cooled to room temperature in air, and the heat-resistant coating attached to the surface of the aluminum alloy was obtained. The corrosion-resistant coating liquid was applied to the surface of the heat-resistant coating using a spin coater, and then cured in an oven at 90°C for 3.5 hours, and the heat-resistant and corrosion-resistant coating attached to the surface of the aluminum alloy was obtained.

[0065] Performance Characterization

[0066] 1. The aluminum alloy with the heat-resistant and corrosion-resistant coating and the uncoated aluminum alloy prepared in Example 1 were subjected to a temperature resistance test at 450-700°C, and the oxidation weight loss was calculated. The results are shown in Table 1 below.

[0067] Table 1 Oxidation weight loss test results

[0068]

[0069] It can be seen from Table 1 that the aluminum alloy surface with the heat-resistant and corrosion-resistant coating prepared in the present invention has good heat resistance, and the quality of the aluminum alloy remains basically unchanged under the heat treatment condition of 600°C.

[0070] 2. The performance tests were conducted on the aluminum alloys with heat-resistant and corrosion-resistant coatings and the aluminum alloys without coatings prepared in Examples 1 to 4. The results are shown in Table 2 below.

[0071] The test method for the acid corrosion resistance of the coating is: drop 2 ml of 40wt% sulfuric acid on the surface of the sample, keep it at 25℃ for 24 hours, and observe the blistering corrosion phenomenon on the surface of the film layer.

[0072] The test method for the alkaline corrosion resistance of the coating is: drop 0.1 standard concentration of sodium hydroxide on the surface of the sample, keep it at 25°C for 24 hours, and observe the blistering corrosion phenomenon on the surface of the film layer.

[0073] Table 2 Performance of heat-resistant and corrosion-resistant coatings

[0074]

[0075] As can be seen from Table 2, the surface of the uncoated aluminum alloy is severely corroded in an acid-base corrosive environment, and a large amount of corrosion impurities are generated. However, the aluminum alloy prepared by the present invention is kept at 25°C for 24 hours, and there is no surface change in the acid-base immersion experiment, which shows that the coating has good adhesion and corrosion resistance.

[0076] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A heat-resistant and corrosion-resistant coating on the surface of an aluminum alloy, characterized in that: It includes a temperature-resistant coating and a corrosion-resistant coating sequentially attached to the surface of the aluminum alloy; The heat-resistant coating comprises the following raw materials in parts by weight: 100 parts of coupling agent mixture, 3-5 parts of nano silicon dioxide powder, and 1-3 parts of active agent; The corrosion-resistant coating comprises the following raw materials in parts by weight: 100-120 parts of epoxy resin, 20-25 parts of polyethylene glycol powder, 5.5-12 parts of boron trifluoride etherate, and 100-160 parts of diluent; The coupling agent mixture is composed of KH-550 silane coupling agent, ethanol and deionized water in a volume ratio of 1-1.5:8-10:10-15; The active agent is one of a polyoxyethylene oleyl alcohol ether type active agent, an ethoxylated methyl glucoside stearate type active agent or a Tween 20 type active agent; The epoxy resin is E51 epoxy resin produced by Jinhong Glue Industry, and the epoxy equivalent is 185-200 g / eq; the diluent is JH-5748 active diluent produced by Jinhong Glue Industry; The method for preparing the heat-resistant and corrosion-resistant coating on the surface of the aluminum alloy comprises the following steps: Add 3-5 parts by weight of nano silicon dioxide powder to 100 parts of the coupling agent mixed solution, stir, and drop 1-3 parts of the activator to obtain a temperature-resistant coating solution; 100-120 parts by weight of epoxy resin and 50-80 parts by weight of diluent are mixed, 20-25 parts of polyethylene glycol powder are added, the temperature is raised and stirred, and then 5.5-12 parts of boron trifluoride ether are added dropwise, and after continuous stirring to obtain a light yellow viscous polymer, 50-80 parts of diluent are added to obtain a corrosion-resistant coating liquid; The pretreated aluminum alloy is immersed in the heat-resistant coating liquid, taken out, blown dry and cured to form a heat-resistant coating on the surface of the aluminum alloy, and then the corrosion-resistant coating liquid is coated on the surface of the heat-resistant coating and cured to obtain a heat-resistant and corrosion-resistant coating attached to the surface of the aluminum alloy.

2. A method for preparing the heat-resistant and corrosion-resistant coating on the surface of an aluminum alloy according to claim 1, characterized in that it comprises the following steps: Add 3-5 parts by weight of nano silicon dioxide powder to 100 parts of the coupling agent mixed solution, stir, and drop 1-3 parts of the activator to obtain a temperature-resistant coating solution; 100-120 parts by weight of epoxy resin and 50-80 parts by weight of diluent are mixed, 20-25 parts of polyethylene glycol powder are added, the temperature is raised and stirred, and then 5.5-12 parts of boron trifluoride ether are added dropwise, and after continuous stirring to obtain a light yellow viscous polymer, 50-80 parts of diluent are added to obtain a corrosion-resistant coating liquid; The pretreated aluminum alloy is immersed in the heat-resistant coating liquid, taken out, blown dry and cured to form a heat-resistant coating on the surface of the aluminum alloy, and then the corrosion-resistant coating liquid is coated on the surface of the heat-resistant coating and cured to obtain a heat-resistant and corrosion-resistant coating attached to the surface of the aluminum alloy.

3. The method for preparing a heat-resistant and corrosion-resistant coating on an aluminum alloy surface according to claim 2, characterized in that: The aluminum alloy pretreatment method comprises: grinding the aluminum alloy surface with water sandpaper, then mechanically polishing to a mirror surface, washing with deionized water, and drying with cold air; then alkaline etching in a sodium hydroxide solution at 60-70° C. for 5 minutes, washing with deionized water; then deashing in a nitric acid solution, washing with deionized water, and drying with cold air.

4. The method for preparing a heat-resistant and corrosion-resistant coating on an aluminum alloy surface according to claim 2, characterized in that: The specific preparation method of the temperature-resistant coating liquid comprises: mixing KH-550 silane coupling agent, ethanol and deionized water in a volume ratio of 1-1.5:8-10:10-15 to prepare a coupling agent mixed liquid, adding 3-5 parts by weight of nano silicon dioxide powder to 100 parts of the coupling agent mixed liquid, stirring with a magnetic stirrer, and simultaneously adding 1-3 parts of an activator to obtain the obtained coating liquid.

5. The method for preparing a heat-resistant and corrosion-resistant coating on an aluminum alloy surface according to claim 2, characterized in that: The specific preparation method of the corrosion-resistant coating liquid comprises: mixing 100-120 parts by weight of epoxy resin and 50-80 parts by weight of diluent, stirring at a speed of 60-80 r / min for 30 minutes with a stirrer, adding 20-25 parts of polyethylene glycol powder, heating to 75-90° C., stirring at a speed of 60-80 r / min for 3-4 hours with a stirrer under nitrogen protection, adding 5.5-12 parts of boron trifluoride ether after mixing evenly, observing the reaction process, adjusting the stirring rate to 300-500 r / min, obtaining a light yellow viscous polymer, and then adding 50-80 parts of diluent, stirring and shaking for 5 minutes to obtain the obtained product.

6. The method for preparing a heat-resistant and corrosion-resistant coating on an aluminum alloy surface according to claim 2, characterized in that: The preparation method of the heat-resistant coating comprises: placing the pretreated aluminum alloy in the heat-resistant coating liquid and soaking it for 50 to 60 seconds, taking it out and blowing it dry, then curing it in an oven at a temperature of 100 to 130° C. for 40 to 50 minutes, taking it out and cooling it to room temperature in the air, thereby obtaining the heat-resistant coating attached to the surface of the aluminum alloy.

7. The method for preparing a heat-resistant and corrosion-resistant coating on an aluminum alloy surface according to claim 2, characterized in that: The preparation method of the heat-resistant and corrosion-resistant coating comprises: coating the corrosion-resistant coating liquid on the surface of the heat-resistant coating by a spin coater, and then curing it in an oven at a temperature of 80-100° C. for 2-4 hours to obtain the heat-resistant and corrosion-resistant coating attached to the surface of the aluminum alloy.