Magnesium alloy and preparation method thereof
By using specific induction frequency and stirring direction control in the induction melting furnace, the problems of uneven composition and element segregation of magnesium alloys are solved, efficient preparation of magnesium alloys is achieved, and the formability and corrosion resistance of magnesium alloys are improved.
Patent Information
- Application Number
- CN202211101158.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-09
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-09-09
AI Technical Summary
During the preparation process of traditional magnesium alloys, rare earth oxides and hydrides are difficult to suspend or sink, resulting in uneven magnesium alloy composition and serious element segregation, which reduces the formability and corrosion resistance of magnesium alloys.
An induction melting furnace is used to prepare magnesium alloys under medium and high frequency induction conditions. Through specific induction frequency and stirring direction control, the uniform mixing of magnesium alloy components and the separation of impurities are achieved, reducing element segregation and improving melt purity.
It effectively reduces the degree of segregation of elements in magnesium alloys, improves the composition uniformity and purity of magnesium alloys, and improves the formability and corrosion resistance of magnesium alloys.
Smart Images

Figure CN116287813B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of metal material preparation, and in particular to a magnesium alloy and a preparation method thereof. Background Art
[0002] Among the commonly used structural metal materials, magnesium has the smallest density, which is only 1.74×10 3 kg / m 3 , which is 1 / 3 and 3 / 4 smaller than aluminum and steel respectively, and is the lightest metal structural material in engineering applications. At the same time, magnesium alloy has become one of the hot spots in alloy research due to its high specific strength, specific stiffness, good thermal conductivity, excellent damping performance, good electromagnetic shielding performance, easy forming and processing, and easy recycling.
[0003] Compared with traditional magnesium alloys, rare earth magnesium alloys have better performance in strength and heat resistance, and have therefore been widely studied and applied. However, in the traditional magnesium alloy preparation process, rare earth oxides and hydrides will be suspended in the melt due to their structure, density, melt viscosity and other reasons, making it difficult to completely float or sink. In addition, when the liquid melt is standing and sinking for purification, rare earth elements are prone to gravity segregation, which seriously reduces the uniformity of the composition of the obtained magnesium alloy. The internal impurities and component segregation of magnesium alloys not only limit the potential of magnesium alloys, but also greatly reduce the formability and corrosion resistance of magnesium alloys.
[0004] Therefore, the prior art still needs to be improved. Summary of the invention
[0005] Based on this, the present application provides a magnesium alloy and a preparation method thereof, which can effectively reduce the segregation degree of elements in the magnesium alloy and improve the purity of the melt.
[0006] The technical solution of this application to solve the above technical problems is as follows:
[0007] In one aspect of the present application, a method for preparing a magnesium alloy is provided, comprising the following steps:
[0008] (1) Providing raw materials for magnesium alloy, including: metallic magnesium and other raw materials, wherein the other raw materials contain elements other than magnesium in the magnesium alloy;
[0009] (2) melting the metal magnesium in an induction melting furnace under high-frequency induction conditions to obtain molten metal magnesium;
[0010] (3) Mixing and melting the molten metal magnesium and the other raw materials under medium frequency induction conditions to obtain a first melt;
[0011] (4) subjecting the first melt to induction stirring treatment under medium frequency induction conditions to obtain a second melt;
[0012] (5) mixing the second melt with a refining agent under medium frequency induction conditions for refining to obtain a third melt;
[0013] (6) Under high-frequency induction conditions, the third melt is allowed to stand for a period of time and cast to obtain the magnesium alloy;
[0014] Wherein, the induction frequency under the medium frequency induction condition is 100 Hz to 1200 Hz, and the induction frequency under the high frequency induction condition is 2000 Hz to 3000 Hz.
[0015] In some embodiments, the induction stirring treatment includes a first stirring treatment, a second stirring treatment, and a third stirring treatment that are performed alternately in sequence; wherein, during the second stirring treatment and the third stirring treatment, the flow direction of the first melt is opposite, and during the first stirring treatment, the flow direction of the first melt is different from the flow directions during the other two stirring treatments.
[0016] In some embodiments, the induction stirring process satisfies at least one of (a) to (b):
[0017] (a) When performing the first stirring treatment, the power of the induction melting furnace is 25 kW to 60 kW, and the first melt is divided into two flow sections, an upper section and an lower section, and each flow section includes two flow areas;
[0018] (b) When the second stirring treatment and the third stirring treatment are performed, the power of the induction melting furnace is 65kW-80kW and 35kW-65kW respectively; when the second stirring treatment is performed, the flow direction of the first melt is: converging flow from the side wall of the induction melting furnace to the center; when the third stirring treatment is performed, the flow direction of the first melt is: diffusing flow from the center of the induction melting furnace to the side wall.
[0019] In some embodiments, the induction stirring process satisfies at least one of (c) to (d):
[0020] (c) the induction stirring treatment time is 15min to 40min;
[0021] (d) the time of the first stirring treatment, the second stirring treatment and the third stirring treatment are independently selected from 4 min to 10 min; and / or
[0022] The static treatment satisfies at least one of the conditions (e) to (f):
[0023] (e) the standing treatment time is 10 min to 40 min;
[0024] (f) The temperature of the static treatment is 720°C to 740°C.
[0025] In some embodiments, in the refining treatment step, the refining agent is added to the second melt by a refining agent adding device;
[0026] The refining agent adding device includes a cylinder for placing the refining agent and a handle connected to the cylinder. The side wall of the cylinder has an opening. During the process of adding the refining agent to the second melt, the refining agent enters the second melt through the opening on the side wall of the cylinder.
[0027] In some embodiments, the refining agent adding device satisfies at least one of the conditions (g) to (h):
[0028] (g) the aperture of the opening is 3 mm to 10 mm;
[0029] (h) The cylinder comprises a cylindrical body and a protective layer arranged on the outer surface of the body, and the body is made of stainless steel or graphite.
[0030] In some embodiments, the gas in the induction melting furnace is a protective gas, and the protective gas includes at least one of CO2 and SF6; and / or
[0031] Before the step of melting the metal magnesium, the method further includes preheating the raw material of the magnesium alloy to 180° C. to 220° C.
[0032] In some embodiments, the other raw materials satisfy at least one of the conditions (i) to (j):
[0033] (i) the other raw materials contain rare earth elements;
[0034] (j) The other raw materials include at least one of Mg-Gd alloy, Mg-Y alloy, Mg-Sm alloy and Mg-Zr alloy.
[0035] In some of the embodiments, after the step of induction stirring treatment and before the step of refining treatment, the step of skimming the second melt is also included; and / or
[0036] After the refining step and before the static treatment step, the method further includes performing a slagging treatment and a degassing step on the third melt; and / or
[0037] After the step of static treatment and before the step of casting, the method further includes a step of filtering the melt after the static treatment.
[0038] Another aspect of the present application provides a magnesium alloy product prepared by the above-mentioned method for preparing the magnesium alloy.
[0039] Compared with the prior art, the method for preparing magnesium alloy in the present application has the following beneficial effects:
[0040] In the above-mentioned method for preparing magnesium alloy, the raw materials of magnesium alloy are first melted in an induction melting furnace, and then the molten metal magnesium and other raw materials are mixed and melted under medium frequency induction conditions, and then the second melt is mixed with a refining agent under medium frequency induction conditions for refining treatment, and then it is left to stand under high frequency induction conditions. Through the control of specific induction frequency conditions, while ensuring the uniform mixing of the components of magnesium alloy, the impurity components included in the melt are separated. In this way, the segregation degree of elements in the magnesium alloy can be effectively reduced and the purity of the melt can be improved.
[0041] Furthermore, by controlling the specific stirring direction during the stirring process, the uniform mixing of the magnesium alloy components can be greatly promoted without destroying the oxide layer on the surface of the melt, thereby avoiding the secondary pollution problem introduced by external mechanical stirring. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 This is a schematic diagram of the stirring method of the induction melting furnace of Example 1;
[0043] Figure 2 It is a front view of the refining agent adding device of Example 1;
[0044] Figure 3 It is a cross-sectional view of the refining agent adding device of Example 1 at line AA;
[0045] Figure 4 This is a microscopic image of the magnesium alloy sample prepared in Example 1;
[0046] Figure 5 This is a microscopic image of the magnesium alloy sample prepared in Comparative Example 1.
[0047] Description of reference numerals:
[0048] 1. Refining agent adding device; 10. Cylinder body; 11. Opening; 20. Handle. DETAILED DESCRIPTION
[0049] In order to facilitate the understanding of the present application, the present application will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present application are given in the drawings. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.
[0050] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0051] An embodiment of the present application provides a method for preparing a magnesium alloy. The present application provides the following technical solution, including steps (1) to (6).
[0052] (1) Providing raw materials for magnesium alloys, including metallic magnesium and other raw materials, where the other raw materials contain elements other than magnesium in magnesium alloys.
[0053] (2) In an induction melting furnace, the metallic magnesium in step (1) is melted under high-frequency induction conditions to obtain molten metallic magnesium.
[0054] (3) In an induction melting furnace, the molten magnesium metal in step (2) and the other raw materials in step (1) are mixed and melted under medium frequency induction conditions to obtain a first melt.
[0055] (4) Under medium frequency induction conditions, the first melt in step (3) is subjected to induction stirring treatment to obtain a second melt.
[0056] (5) Under medium frequency induction conditions, the second melt in step (4) is mixed with a refining agent for refining treatment to obtain a third melt.
[0057] (6) Under high-frequency induction conditions, the third melt in step (5) is allowed to stand for a period of time and then cast to obtain a magnesium alloy.
[0058] Among them, the induction frequency under the medium frequency induction condition is 100Hz~1200Hz, and the induction frequency under the high frequency induction condition is 2000Hz~3000Hz.
[0059] In the above-mentioned method for preparing magnesium alloy, the raw materials of magnesium alloy are first melted in an induction melting furnace, and then the molten metal magnesium and other raw materials are mixed and melted under medium frequency induction conditions, and then the second melt is mixed with a refining agent under medium frequency induction conditions for refining treatment, and then it is left to stand under high frequency induction conditions. Through specific induction frequency control, while ensuring that the components of magnesium alloy are mixed evenly, the impurity components included in the melt are separated. In this way, the segregation degree of elements in magnesium alloy can be effectively reduced and the purity of the melt can be improved.
[0060] In some embodiments, the other raw materials contain rare earth elements; further, the rare earth elements include at least one of lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), promethium (Pm), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), lutetium (Lu), yttrium (Y) and scandium (Sc).
[0061] Specifically, the elements contained in the above other raw materials can be selected according to the actual required products.
[0062] In some specific examples, the other raw materials in step (1) include at least one of Mg-Gd alloy, Mg-Y alloy, Mg-Sm alloy and Mg-Zr alloy.
[0063] It should be noted that the induction melting furnace used above can be an induction melting furnace commonly used in the art, such as an alloy induction melting furnace equipment.
[0064] Here is a description of the working principle of the induction melting furnace, but it is not limited to this: a high-frequency high-frequency current flows through a heating coil (usually made of copper tube) that is wound into a ring or other shape. This generates a strong magnetic flux with instantaneous polarity changes in the coil. When a heated object such as a metal is placed in the coil, the magnetic flux will penetrate the entire heated object, and a corresponding large eddy current will be generated inside the heated object in the opposite direction to the heating current. Due to the existence of resistance in the heated object, a lot of Joule heat will be generated, causing the temperature of the object itself to rise rapidly, thereby achieving the purpose of heating the material.
[0065] It can be understood that the medium and high frequency induction conditions in the induction melting furnace can be switched, and the melting stirring method in the three stirring treatments is controlled by the induction circuit and coil of the induction furnace itself. Since the electromagnetic force borne by the melt is inversely proportional to the square root of the induction frequency, the stirring force under the medium frequency induction condition is greater than that under the high frequency induction condition. In other words, the induction stirring treatment of the present application refers to the flow stirring of the melt after it is melted by controlling the process conditions of the induction melting furnace, that is, stirring without external machinery.
[0066] Based on a large number of creative experimental studies, the technicians of this application found that when using an induction melting furnace to melt magnesium alloys, the frequency control of the induction conditions has an important influence on removing impurities in the alloy and homogenizing the components. After a large number of experimental investigations, they creatively separated the impurity components included in the melt while ensuring uniform mixing of the components of the magnesium alloy through the control of specific induction frequencies and stirring directions.
[0067] In some of the embodiments, the melting power of the induction melting furnace is 25 kW to 150 kW;
[0068] In some of the embodiments, the induction frequency under the medium frequency induction condition is 100 Hz to 1200 Hz;
[0069] In some of the embodiments, the induction frequency under the high-frequency induction condition is 2000 Hz to 3000 Hz.
[0070] In some of the embodiments, the temperature used when melting the metal magnesium in the above step (2) is 730°C to 760°C.
[0071] In some of the embodiments, in step (2), before the step of melting the metallic magnesium, the step further includes preheating the raw material of the magnesium alloy to 180° C. to 220° C.
[0072] Furthermore, the preheating step is performed in an induction melting furnace, specifically by placing the raw material of the magnesium alloy in a melting crucible of the induction melting furnace.
[0073] In some embodiments, the melting crucible includes at least one of a graphite crucible, a magnesia crucible and a corundum crucible; in a specific example, the melting crucible is a graphite crucible.
[0074] In some of the examples, the gas in the induction melting furnace is a protective gas, and the protective gas includes at least one of CO2 and SF6.
[0075] It can be understood that the introduction of protective gas can prevent the magnesium alloy melt from being oxidized at high temperature.
[0076] Optionally, the protective gas is a mixed gas with a volume fraction of 99% CO2 and 1% SF6.
[0077] In some of the examples, in step (3), Mg-Sm alloy, Mg-Y alloy, Mg-Gd alloy and Mg-Zr alloy are added in sequence to the molten metal magnesium, and the induction melting furnace is adjusted to a medium frequency state with a power of 50 kW to 60 kW and a frequency of 40 Hz to 160 Hz for melting.
[0078] Specifically, the charging is carried out through a charging port on the top of the induction melting furnace.
[0079] In some of the embodiments, in step (3), the temperature used for mixing and melting the molten magnesium metal and other raw materials is 730° C. to 760° C.
[0080] In some of the embodiments, in step (4), the induction stirring treatment includes a first stirring treatment, a second stirring treatment and a third stirring treatment that are performed alternately in sequence to obtain a second melt; wherein, during the second stirring treatment and the third stirring treatment, the flow direction of the first melt is opposite, and during the first stirring treatment, the flow direction of the first melt is different from the flow directions during the other two stirring treatments.
[0081] Furthermore, by controlling the specific stirring direction during the induction stirring process, the uniform mixing of the magnesium alloy components can be greatly promoted without destroying the oxide layer on the surface of the melt, thereby avoiding the secondary pollution problem introduced by external mechanical stirring.
[0082] In some of the embodiments, in step (4), during the first stirring treatment, the first melt is divided into two flow sections, an upper section and an lower section, and each flow section includes two flow areas.
[0083] In some embodiments, the flow directions of the upper and lower flow portions of the first melt are opposite.
[0084] Please refer to Figure 1 As shown in (A) in the figure, taking the segmented horizontal lines of the upper and lower sections of the first melt as the reference, the direction away from the segmented horizontal lines is regarded as "up", and the direction close to the segmented horizontal lines is regarded as "down". As shown by the arrows in the figure, the upper section of the first melt flows from bottom to top, and the lower section flows from bottom to top.
[0085] In some of the embodiments, in step (4), when the second stirring treatment is performed, the flow direction of the first melt is: diffuse flow from the center of the induction melting furnace to the side wall.
[0086] Please refer to Figure 1 As shown in (C) in the figure, as shown by the arrows, the first melt diffuses and flows from the center to the side walls in the induction melting furnace. In other words, the melt height at the center of the induction melting furnace gradually decreases and diffuses to the surrounding side walls, that is, the melt height on the side walls gradually increases.
[0087] Specifically, the first melt is made to flow by controlling the induction conditions of the first melt induction melting furnace to achieve the purpose of stirring, and the flow direction of the first melt is controlled by adjusting the induction circuit and phase sequence, that is, the phase of the electromagnetic wave.
[0088] In some of the embodiments, in step (4), the flow direction of the first melt during the third stirring treatment is: flowing from the side wall of the induction melting furnace toward the center.
[0089] Please refer to Figure 1 As shown in (B), as shown by the arrows in the figure, the first melt flows from the side wall to the center in the induction melting furnace. In other words, the height of the melt on the side wall of the induction melting furnace gradually decreases and gathers toward the center, that is, the height of the melt in the center gradually increases.
[0090] In some of the embodiments, in step (4), during the first stirring treatment, the power of the induction melting furnace is 25 kW to 60 kW, and during the second stirring treatment and the third stirring treatment, the power of the induction melting furnace is 65 kW to 80 kW and 35 kW to 65 kW, respectively.
[0091] In some embodiments, in step (4), the induction stirring treatment time is 15 min to 40 min.
[0092] In some embodiments, in step (4), the time for the first stirring treatment, the second stirring treatment and the third stirring treatment are independently selected from 4 min to 10 min.
[0093] It can be understood that in the above step (4), the first stirring treatment, the second stirring treatment and the third stirring treatment are alternately performed in sequence as one cycle of alternating stirring, and the number of cyclic stirring can be multiple times, such as two or three times.
[0094] In some of the embodiments, in step (4), the temperature of the induction stirring treatment is 730°C to 760°C.
[0095] In some of the embodiments, in step (5), in the refining treatment step, a refining agent is added to the second melt by a refining agent adding device.
[0096] Please refer to the attached Figure 2 and Figure 3 , are respectively a front view and a cross-sectional view of the refining agent adding device. The refining agent adding device 1 comprises a barrel 10 for placing the refining agent, and a handle 20 connected to the barrel. The side wall of the barrel 10 has an opening 11. In the process of adding the refining agent to the second melt, the refining agent enters the second melt through the opening 11 on the side wall of the barrel 10.
[0097] It can be understood that the refining agent has a strong adsorption capacity for inclusions in the magnesium alloy melt, causing the inclusions to agglomerate and combine with the flux to form a precipitate, which can effectively remove inclusions in the magnesium alloy melt. However, the traditional refining agent addition is performed by direct pressing and manual stirring, which easily leads to the problem of refining agent agglomeration, resulting in insufficient refining agent addition, uneven distribution, and poor refining effect. During the refining agent addition process of the present application, the refining agent is gradually flushed into the melt through the openings on the side wall of the cylinder as the melt flows, which can avoid blockage and make the distribution of the refining agent in the melt more uniform, thereby improving the refining effect.
[0098] There is no specific requirement for the shape of the openings, which may be rectangular, square or circular, and there is no specific requirement for the number of the openings, which may be multiple.
[0099] In a specific example, the opening is circular.
[0100] In some embodiments, the opening has a diameter of 3 mm to 10 mm.
[0101] In some of the embodiments, the cylinder includes a cylindrical body and a protective layer arranged on the outer surface of the body, and the body is made of stainless steel or graphite.
[0102] In some of the embodiments, the refining agent is pre-loaded into a refining barrel of the refining agent adding device, the refining barrel extends into the melt and rotates, and the refining agent enters the second melt through the openings on the side wall of the barrel.
[0103] In some of the embodiments, the refining agent may be a refining agent commonly used in the art. Further, the refining agent includes at least one of JDMJ, RJ2, RJ6 and Dow230.
[0104] In some embodiments, the mass of the refining agent is 0.8 wt % to 1.5 wt % of the total mass of the raw material for the magnesium alloy.
[0105] In a specific example, the mass of the refining agent is 1 wt % of the total mass of the raw material for the magnesium alloy.
[0106] In some embodiments, the total mass of the raw materials of the magnesium alloy is 10 kg to 50 kg.
[0107] In some of the embodiments, during the above refining treatment, the power of the induction melting furnace is 70 kW to 90 kW, the induction frequency is 2000 Hz to 2300 Hz, the temperature is 730° C. to 760° C., and the time is 3 min to 8 min.
[0108] In some of the embodiments, after the refining step, a heat preservation step is further performed under high-frequency induction conditions, and the heat preservation time is 10 minutes to 20 minutes.
[0109] In some embodiments, after the stirring step and before the refining step, a step of deslagging the second melt is further included. Further, the deslagging is performed under high frequency conditions.
[0110] In some embodiments, after the refining step and before the static treatment step, the third melt is further subjected to a slag removal and degassing step. Further, the slag removal is performed under high frequency conditions.
[0111] In some of the embodiments, the degassing step is as follows: high-purity argon gas is used for 3 minutes to 10 minutes.
[0112] Furthermore, after the degassing step and before the static treatment, the method further includes a step of skimming slag from the surface of the melt.
[0113] It can be understood that the purpose of introducing argon is to remove gas and non-metallic inclusions in the melt. During the degassing process, impurities included in the middle of the melt will be blown out to the surface to form slag, so slag removal is carried out again.
[0114] In some of the examples, in step (6), the standing time is 10 min to 40 min.
[0115] In some of the examples, in step (6), the temperature of the static treatment is 720° C. to 740° C. It can be understood that controlling the temperature of the induction melting furnace under high-frequency induction conditions further improves the purification effect.
[0116] In some of the embodiments, during the above-mentioned static treatment, the power of the induction melting furnace is 70 kW to 90 kW, and the induction frequency is 2000 Hz to 2300 Hz.
[0117] In some of the examples, step (6) further includes filtering the melt after the standing treatment step, after the standing treatment step and before the casting step.
[0118] It can be understood that the function of filtering is to block inclusion particles at each hole of the filter, and to filter, degas and remove slag from the melt.
[0119] In some of the embodiments, the filtering step is performed using a filtering device; specifically, the filtering device is a filter plate with a pore size of 1 μm to 20 μm, made of stainless steel or ceramic, and having a protective layer on the outer surface.
[0120] In some of the examples, step (6) further includes preheating the filtration device to 180° C. to 220° C. before the filtering step.
[0121] In some of the examples, after the filtering step and before casting, a step of skimming the filtered melt is further included.
[0122] In some of the examples, in step (6), the casting step is performed using a steel mold, and further, before casting, the step of preheating the steel mold is included, and the preheating temperature is 200°C to 250°C.
[0123] Specifically, during the casting process, the third melt is discharged from the side discharge port of the induction melting furnace after being allowed to stand, and enters the steel mold for casting using a fixed-point casting method, and a magnesium alloy is obtained after cooling.
[0124] In one embodiment of the present application, a magnesium alloy is provided. The magnesium alloy is prepared by the above method for preparing the magnesium alloy.
[0125] The magnesium alloy prepared by the preparation method of the magnesium alloy has low element segregation, uniform element distribution and few ingot inclusions.
[0126] The present application will be described below in conjunction with specific embodiments, but the present application is not limited to the following embodiments. It should be understood that the attached claims summarize the scope of the present application. Under the guidance of the concept of the present application, technical personnel in the field should realize that certain changes made to the various embodiments of the present application will be covered by the spirit and scope of the claims of the present application. Specific embodiments
[0128] The present application is further described below in conjunction with the accompanying drawings and embodiments, but the protection content of the present application is not limited to the scope described in the embodiments.
[0129] Example 1
[0130] (1) The mass composition of the magnesium alloy is: 8.0wt% Gd, 3.0wt% Y, 2.0wt% Sm, 0.5wt% Zr, and the balance is Mg. The raw materials provided are formulated according to the mass composition of the magnesium alloy: metallic magnesium, Mg-Gd alloy, Mg-Y alloy, Mg-Sm alloy, and Mg-Zr alloy.
[0131] (2) Preheating metal magnesium, Mg-Gd alloy, Mg-Y alloy, Mg-Sm alloy, Mg-Zr alloy and a melting crucible to 200° C.; in a mixed atmosphere of 99% CO2 and 1% SF6, adjusting the induction melting furnace to high-frequency induction conditions with a melting furnace power of 90 kW and a frequency of 2000 Hz to 2300 Hz, adding metal Mg to the melting crucible and heating it to 740° C., then keeping the temperature to completely melt the metal Mg, to obtain molten metal magnesium;
[0132] (3) Under the condition of keeping warm at 740°C, Mg-Gd alloy, Mg-Y alloy, Mg-Sm alloy and Mg-Zr alloy are added to the molten metal magnesium in sequence through the charging port on the top of the induction melting furnace, and the induction melting furnace is adjusted to the medium frequency induction condition with the power of the melting furnace being 60 kW and the frequency being 140 Hz to 160 Hz. The mixed melting is carried out in the same stirring mode as the first stirring treatment, and the materials are added through the charging port on the top of the induction melting furnace to obtain a first melt.
[0133] (4) The first stirring treatment, the second stirring treatment and the third stirring treatment were carried out alternately under the condition of medium frequency induction at 740°C. The time of each stirring treatment was 4 minutes, and the alternating stirring treatment was 20 minutes. In the first stirring treatment, the first melt flowed from top to bottom in the upper part of the induction melting furnace and from bottom to top in the lower flow part. The power of the induction melting furnace was 60 kW, and the frequency of the medium frequency induction was 140 Hz to 160 Hz. The flow direction of the first melt in the second stirring treatment was: flowing from the side wall of the induction melting furnace to the center, that is, the first melt in the furnace flowed from the side wall of the induction melting furnace to the center. The melt flows upward from the side wall, gathers to the center, and flows downward from the center. The power of the induction melting furnace is 70kW, and the frequency of the medium frequency induction is 140Hz~160Hz. The flow direction of the first melt during the third treatment is: diffuse flow from the center of the induction melting furnace to the side wall, that is, the first melt in the furnace flows upward from the center, diffuses to the side wall, and flows downward from the side wall. The power of the induction melting furnace is 52kW, and the frequency of the medium frequency induction is 150Hz~180Hz to obtain the second melt. For the first stirring treatment, the second stirring treatment and the third stirring treatment, please refer to the attached flow direction of the melt. Figure 1 (A), (C) and (B) in the figure.
[0134] (5) Under high-frequency induction conditions (power of 85kW, frequency of 2000Hz~2300Hz), skim off the scum on the surface of the melt, then at 740°C, adjust the power of the smelting furnace to 50kW, adjust the induction frequency to 150Hz~180Hz, and use the same stirring method as the third stirring treatment to carry out refining treatment. The specific steps of the refining treatment are: pre-load a refining agent with a mass of 1% of the mass of the raw material into the barrel of the refining agent adding device, extend the barrel into the melt through the handle connected to the barrel and rotate it, and the refining agent enters the second melt through the opening on the side wall of the barrel, and refines for 4 minutes. After the refining is completed, adjust the power of the smelting furnace to 85kW, and the induction frequency to 2000Hz~2300Hz. After keeping warm for 10 minutes, skim off the scum on the surface of the melt and then degas. Degassing is carried out using high-purity argon gas, and the degassing time is 3 minutes. Then skim off the surface scum. Among them, the front view of the refining agent adding device is shown in the figure below. Figure 2 As shown, the cross-sectional view of the refining agent adding device on line AA is as follows Figure 3 shown.
[0135] (6) The power of the smelting furnace is maintained at 85 kW, the induction frequency is maintained at 2000 Hz to 2300 Hz, and the molten metal is allowed to stand for 30 minutes, with the temperature maintained at 730°C; the scum on the surface of the melt is skimmed off, and the melt is filtered through a filter preheated to 200°C; finally, a steel mold preheated to 200°C is used for casting, and a fixed-point casting method is used to obtain the Mg-8Gd-3Y-2Sm-0.5Zr alloy after cooling.
[0136] The prepared Mg-8Gd-3Y-2Sm-0.5Zr alloy was observed under an optical microscope, and the obtained structure picture is as follows: Figure 4 As shown, the tissue is evenly distributed with few internal inclusions.
[0137] Example 2
[0138] Example 2 is basically the same as Example 1, except that the stirring treatment in step (4) of Example 2 only adopts the first stirring treatment method, and the overall stirring time is the same as that of Example 1.
[0139] The remaining steps are the same as those in Example 1.
[0140] Example 3
[0141] Example 3 is basically the same as Example 1, except that in step (4) of Example 3, only the second stirring treatment method is used during the stirring treatment, and the overall stirring time is the same as that of Example 1.
[0142] The remaining steps are the same as those in Example 1.
[0143] Example 4
[0144] Example 4 is basically the same as Example 1, except that in step (4) of Example 4, only the third stirring treatment method is used during the stirring treatment, and the overall stirring time is the same as that of Example 1.
[0145] The remaining steps are the same as those in Example 1.
[0146] Example 5
[0147] Example 5 is basically the same as Example 1, except that the three stirring treatment times in step (4) of Example 5 are different from those in Example 1. The specific steps are as follows.
[0148] (4) At 740° C., the first stirring treatment, the second stirring treatment and the third stirring treatment were alternately performed in sequence under medium frequency induction conditions. The duration of each stirring treatment was 4 minutes, and the alternating stirring treatment was circulated for 15 minutes.
[0149] The remaining steps are the same as those in Example 1.
[0150] Example 6
[0151] Example 6 is basically the same as Example 1, except that the duration of the three stirrings in step (4) of Example 6 is different from that of Example 1. The specific steps are as follows.
[0152] (4) At 740° C., the first stirring treatment, the second stirring treatment and the third stirring treatment were alternately performed in sequence under medium frequency induction conditions. The duration of each stirring treatment was 4 minutes, and the alternating stirring treatment was 40 minutes.
[0153] The remaining steps are the same as those in Example 1.
[0154] Example 7
[0155] Example 7 is basically the same as Example 1, except that the standing treatment time in step (6) of Example 7 is different from that in Example 1. The specific steps are as follows:
[0156] (6) Under high-frequency induction conditions, the power of the melting furnace is 85 kW and the frequency is 2000 Hz to 2300 Hz. The melt is allowed to stand for 10 minutes and the standing temperature is maintained at 730°C. The scum on the surface of the melt is then skimmed off and the melt is filtered through a filter preheated to 200°C. Finally, the melt is cast using a steel mold preheated to 200°C by a fixed-point casting method. After cooling, the Mg-8Gd-3Y-2Sm-0.5Zr alloy is obtained.
[0157] The remaining steps are the same as those in Example 1.
[0158] Comparative Example 1
[0159] Comparative Example 1 is basically the same as Example 1, except that: Comparative Example 1 uses a pit-type resistance furnace to smelt the alloy, and the stirring treatment in step (4) uses external mechanical stirring for a stirring time of 20 minutes.
[0160] The prepared Mg-8Gd-3Y-2Sm-0.5Zr alloy was observed under an optical microscope, and the obtained structure picture is as follows: Figure 5 As shown, the tissue is unevenly distributed and has serious internal inclusions.
[0161] Comparative Example 2
[0162] Comparative Example 2 is basically the same as Example 2, except that: in Comparative Example 2, a traditional medium frequency induction furnace is used for smelting, i.e., there is no high frequency band, the stirring method in the stirring treatment in step (4) is the same as the first stirring treatment, the above steps (2) to (5) are all carried out under medium frequency induction conditions, step (6) is carried out under medium frequency low power, and the heat preservation and stirring are carried out for 20 minutes.
[0163] The composition deviation and inclusion volume fraction of the Mg-8Gd-3Y-2Sm-0.5Zr alloy obtained in each embodiment and comparative example were tested and calculated. The inclusion volume fraction was calculated as follows:
[0164] Inclusion size is expressed as inclusion equivalent diameter d avg express,
[0165] In the formula, A inclusion is the area of a single inclusion obtained by image analysis software, μm 2 .
[0166] The average volume fraction of inclusions F avg Calculated by the following formula:
[0167]
[0168] In the formula, A field is the area of the metallographic field of view, μm 2 .
[0169] The alloy composition deviation is calculated as follows:
[0170]
[0171]
[0172] In the formula, A max , A min , A avg They respectively represent the maximum, minimum and average values of the same element composition measured at different sampling locations of the same ingot.
[0173] The specific results of the composition deviation and impurity content of the alloy samples prepared in each embodiment and comparative example are shown in Table 1.
[0174] Table 1
[0175]
[0176]
[0177] Combined with the data in Table 1, it can be seen that compared with the preparation method of the magnesium alloy in the comparative example, the magnesium alloy prepared by the preparation method of the magnesium alloy of the present application has fewer alloy inclusions and a more uniform structure.
[0178] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0179] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.
Claims
1. A method for preparing a magnesium alloy, characterized in that: The following steps are involved: (1) Providing raw materials for magnesium alloy, including: metallic magnesium and other raw materials, wherein the other raw materials contain elements other than magnesium in the magnesium alloy; (2) melting the metal magnesium in an induction melting furnace under high-frequency induction conditions to obtain molten metal magnesium; (3) Mixing and melting the molten metal magnesium and the other raw materials in an induction melting furnace under medium frequency induction conditions to obtain a first melt; (4) subjecting the first melt to induction stirring treatment under medium frequency induction conditions to obtain a second melt; (5) mixing the second melt with a refining agent under medium frequency induction conditions for refining to obtain a third melt; (6) Under high-frequency induction conditions, the third melt is allowed to stand for a period of time and cast to obtain the magnesium alloy; After the induction stirring step and before the refining step, the method further includes performing a slag removal step on the second melt, wherein the slag removal step is performed under high frequency conditions; After the refining step and before the static treatment step, the method further includes performing a slag removal and degassing step on the third melt, wherein the slag removal is performed under high frequency conditions; Wherein, the induction frequency under the medium frequency induction condition is 100 Hz to 1200 Hz, and the induction frequency under the high frequency induction condition is 2000 Hz to 3000 Hz.
2. The method for preparing a magnesium alloy according to claim 1, characterized in that: The induction stirring process includes a first stirring process, a second stirring process and a third stirring process which are performed alternately in sequence; wherein, when the second stirring process and the third stirring process are performed, the flow direction of the first melt is opposite, and when the first stirring process is performed, the flow direction of the first melt is different from the flow directions of the other two stirring processes; When performing the first stirring treatment, the power of the induction melting furnace is 25 kW to 60 kW, the first melt is divided into two flow sections, each flow section is two flow areas; When the second stirring treatment and the third stirring treatment are performed, the power of the induction melting furnace is 65kW-80kW and 35kW-65kW respectively; when the second stirring treatment is performed, the flow direction of the first melt is: converging flow from the side wall of the induction melting furnace to the center; when the third stirring treatment is performed, the flow direction of the first melt is: diffusing flow from the center of the induction melting furnace to the side wall.
3. The method for preparing a magnesium alloy according to claim 2, characterized in that: The induction stirring treatment satisfies at least one of (a) to (b): (a) The induction stirring treatment time is 15min to 40min; (b) the time of the first stirring treatment, the second stirring treatment and the third stirring treatment are independently selected from 4 min to 10 min; and / or The static treatment satisfies at least one of the conditions (c) to (d): (c) the standing treatment time is 10 min to 40 min; (d) The temperature of the static treatment is 720°C to 740°C.
4. The method for preparing a magnesium alloy according to claim 2, characterized in that: The temperature of the induction stirring treatment is 730°C to 760°C.
5. The method for preparing a magnesium alloy according to any one of claims 1 to 4, characterized in that: In the refining treatment step, the refining agent is added to the second melt through a refining agent adding device; The refining agent adding device includes a cylinder for placing the refining agent and a handle connected to the cylinder. The side wall of the cylinder has an opening. During the process of adding the refining agent to the second melt, the refining agent enters the second melt through the opening on the side wall of the cylinder.
6. The method for preparing a magnesium alloy according to claim 5, characterized in that: The refining agent adding device satisfies at least one of the conditions (e) to (f): (e) The aperture of the opening is 3 mm to 10 mm; (f) The cylinder comprises a cylindrical body and a protective layer arranged on the outer surface of the body, and the body is made of stainless steel or graphite.
7. The method for preparing a magnesium alloy according to any one of claims 1 to 4, characterized in that: The gas in the induction melting furnace is a protective gas, and the protective gas includes at least one of CO2 and SF6; and / or before the step of melting the metallic magnesium, it also includes the step of preheating the raw material of the magnesium alloy to 180°C to 220°C.
8. The method for preparing a magnesium alloy according to any one of claims 1 to 4, characterized in that: The other raw materials meet at least one of the conditions (g) to (h): (g) the other raw materials contain rare earth elements; (h) The other raw materials include at least one of Mg-Gd alloy, Mg-Y alloy, Mg-Sm alloy and Mg-Zr alloy.
9. The method for preparing a magnesium alloy according to any one of claims 1 to 4, characterized in that: After the step of static treatment and before the step of casting, the method further includes a step of filtering the melt after the static treatment.
10. A magnesium alloy, characterized in that: The magnesium alloy is prepared by the method for preparing the magnesium alloy according to any one of claims 1 to 9.
Citation Information
Patent Citations
Novel Mg-Y-Nd-(La+Ce)-Zr biodegradable magnesium alloy and manufacturing method thereof
CN110468319A
Variable frequency induction heater
CN1300176A