A kind of aluminum alloy material without heat treatment and preparation method thereof

By preparing heat-free aluminum alloy materials containing zirconium, nitrogen, titanium, boron, rhenium, cerium and strontium, the problem of deformation and quality risks of aluminum alloy during heat treatment is solved, and high-performance aluminum alloy materials are realized, suitable for large-scale The production of integrated die castings has excellent mechanical properties and anti-microbial properties.

CN116287876BActive Publication Date: 2024-11-29HAIAN HONGYU ALLOY MATERIAL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310187990.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-02
Publication Date
2024-11-29
Estimated Expiration
2043-03-02

AI Technical Summary

Technical Problem

Aluminum alloys are prone to quality risks such as deformation and foaming during heat treatment, and are not economical and environmentally friendly, making it difficult to meet the dimensional stability and surface perfection requirements of large integrated die castings, especially in the promotion of integrated die casting technology. In application.

Method used

Using heat-free aluminum alloy materials including aluminum, zirconium, nitrogen, titanium, boron, rhenium, cerium and strontium, a high elastic modulus, tensile strength, yield strength and hardness are prepared through specific melting and die-casting process parameters. Aluminum alloy materials avoid stress release and dimensional deformation during heat treatment.

Benefits of technology

It achieves high performance performance of aluminum alloy materials, including extremely high elastic modulus, tensile strength, yield strength and elongation, and has excellent anti-corrosion, antibacterial and anti-mold properties, which can meet the die-casting needs at room temperature, avoiding The quality risks and economic costs of heat treatment.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a heat-treatment-free high-performance aluminum alloy material and a preparation method thereof. By introducing nitrogen and boron into a high-temperature aluminum alloy melt, the aluminum alloy performance is greatly improved, especially the elastic modulus is increased by more than three times, and high strength and elongation are obtained, and the aluminum alloy can be used for casting without heat treatment. The introduced nitrogen element is dispersed at the grain boundary of the aluminum alloy, playing multiple roles such as grain boundary strengthening, preventing grain growth, and refining grains. In addition, the aluminum alloy also obtains excellent anti-corrosion, antibacterial and anti-mildew properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of new materials, and specifically relates to a heat treatment-free aluminum alloy material and a preparation method thereof. Background Art

[0002] Aluminum alloy has low density. It has high specific stiffness, high specific strength, good thermal and electrical conductivity, good plasticity, and small expansion coefficient, and is widely used in many fields. However, aluminum alloy has disadvantages such as low hardness, poor wear resistance, and low friction coefficient. There are many factors that determine the performance of materials, and the performance of metal materials is mainly affected by the organizational structure. Aluminum alloy is widely used because of its light weight, easy processing and excellent economy. Aluminum itself has the characteristics of high elongation. In order to meet the die-casting process, it must have demoulding and fluidity, and all mechanical properties must meet the standards. At present, mainstream die-casting aluminum alloys need to be heat treated to increase the elongation to more than 10%. The purpose of heat treatment is to improve the strength, hardness and corrosion resistance of aluminum alloys.

[0003] Aluminum alloy heat treatment technology is a technology that selects a certain heat treatment specification, controls the heating speed to a certain corresponding temperature, keeps the temperature for a certain period of time, and cools at a certain speed when heat treating aluminum alloy products, so as to change the structural organization of the alloy. The specific process and mechanism include annealing, quenching and aging treatment, among which annealing is to remove the internal stress of the casting, promote the spheroidization of some silicon crystals of Al-Si alloy, and effectively improve the plasticity of the alloy. Quenching is a solid solution treatment and rapid cooling treatment, the purpose of which is to fix the strengthening phase. Solid solution treatment can fully dissolve various phases in the alloy, strengthen the solid solution, and improve the toughness and corrosion resistance of the alloy. Aging treatment is divided into natural aging and artificial aging, which refers to the process of storing the material at room temperature or higher temperature for a long time. Generally speaking, after aging treatment, the hardness and strength of the aluminum alloy are increased, but the plasticity, toughness and internal stress are reduced.

[0004] Aluminum alloy die-castings are not suitable for heat treatment. During the heat treatment process, stress release, dead weight and quenching can easily cause castings to deform, blister and other quality risks. It is also not economical and does not meet the country's advocacy of energy conservation and emission reduction.

[0005] In addition, the large-scale integrated die-casting technology that emerged with Tesla has become one of the hottest development trends in the industry. The promotion and application of integrated die-casting technology requires matching equipment, molds, processes, materials, etc. Due to the large projection area of ​​integrated die-castings, heat treatment can easily cause dimensional deformation and surface defects of parts. For large integrated parts, there is a huge cost risk. Therefore, integrated die-castings tend to use aluminum alloy materials that do not require heat treatment. Summary of the invention

[0006] The purpose of the present invention is to address the problems in the above-mentioned background technology and disclose a heat-treatment-free aluminum alloy material and a preparation method thereof. A heat-treatment-free aluminum alloy material is characterized by comprising aluminum, nitrogen, zirconium, titanium, boron and rhenium, cerium and strontium, and the mass percentages of each group are: zirconium 7-12%, nitrogen 0.001-1.2%, titanium 0.4-0.7%, boron 0.0001-0.2%, rhenium, cerium, strontium 0.0001-0.2%, and the rest are aluminum and unavoidable impurities; wherein the mass percentage of the impurity content is less than 0.15%. Another object of the present invention is to provide a preparation method for the above-mentioned heat-treatment-free aluminum alloy material. The method comprises the following preparation steps: using 99.7% or more original aluminum A00 to heat and melt, the melting temperature is 650°C-720°C, after the A00 is melted, adding zirconium at a mass percentage of 7-12%, and heating to melt, the melting temperature is 730°C-800°C, introducing aluminum nitride fine powder into the melt after the zirconium is melted, and then adding boron at a mass percentage of 0.0001-0.2% and titanium at a mass percentage of 0.4-0.7% after the nitrogen element is introduced, and melting to obtain aluminum, nitrogen, zirconium, titanium and boron melts, adjusting the aluminum alloy solution to 690°C-720°C, adding aluminum master alloy at a mass percentage of 0.0001-0.2% of rhenium, cerium and strontium, and heating the mold to obtain an aluminum alloy ingot or casting. Due to the introduction of nitrogen and the mixing effect, the aluminum alloy material disclosed in the present invention has an extremely high elastic modulus, reaching 260GPa, a tensile strength ≥260MPa, a yield strength ≥120MPa, an elongation ≥10%, and a hardness ≥65HBW. It also has excellent anti-corrosion, anti-bacterial and anti-mildew properties. The antibacterial mechanism is that trace nitrogen precipitates to form ammonia gas and then becomes antibacterial. Due to its excellent performance, it can be exempted from heat treatment. DETAILED DESCRIPTION Example 1

[0007] In this embodiment, aluminum alloy A1 is provided, and the chemical composition is as follows: zirconium 7.0%, nitrogen 0.001%, boron 0.0001%, titanium 0.4%, rhenium, cerium, and strontium are all 0.0001%, and the rest is aluminum and inevitable impurities; wherein, the mass percentage of the impurity content is less than 0.15%, and the remainder is Al. The preparation method of the aluminum alloy is: 99.7% or more of the original aluminum A00 is heated and melted, and the melting temperature is 650°C. After the A00 is melted, 7.0% of the mass percentage of zirconium is added, and the melting temperature is 730°C. After the zirconium is melted, 0.001% of the mass percentage of nitrogen is introduced into the melt by adding aluminum nitride, and then 0.0001% of the mass percentage of boron is added, and 0.4% of the mass percentage of titanium is added. After melting, aluminum, zirconium, nitrogen, boron and titanium melts are obtained. The aluminum alloy solution is adjusted to 720°C, and aluminum master alloy is added according to the mass percentage of rhenium, cerium and strontium at 0.0001 respectively. The obtained aluminum alloy ingot of aluminum alloy A1 is sent to the side furnace of the die casting machine for melting and die casting production, wherein the die casting process parameters are: casting temperature 700°C, mold preheating temperature 260°C, casting boost pressure 300MPa, injection speed 4m / s. The die casting sample obtained in this example is a thin-walled casting (thickness 3mm), and the room temperature elastic modulus is measured to be 120GPa, the tensile strength is 272MPa, the yield strength is 129MPa, the elongation is 11%, and the hardness is 67HBW. Example 2

[0008] In this embodiment, aluminum alloy A2 is provided, and the chemical composition is as follows: 9.6% zirconium, 0.1% nitrogen, 0.1% boron, 0.5% titanium, 0.1% rhenium, cerium, and strontium, and the rest is aluminum and unavoidable impurities; wherein the mass percentage of the impurity content is less than 0.15%, and the remainder is Al. The preparation method of the aluminum alloy is as follows: 99.7% or more of the original aluminum A00 is heated and melted, and the melting temperature is 680°C. After the A00 is melted, zirconium is added at a mass percentage of 9.6%, and the temperature is increased to melt, and the melting temperature is 750°C. After the zirconium is melted, 0.1% of nitrogen is introduced into the melt by adding aluminum nitride, and then 0.1% of boron is added at a mass percentage, and 0.5% of titanium is added at a mass percentage. After melting, aluminum, zirconium, nitrogen, boron and titanium melts are obtained. The aluminum alloy solution is adjusted to 700°C, and aluminum master alloy is added according to the mass percentage of rhenium, cerium and strontium by 0.1%, and the obtained aluminum alloy ingot of aluminum alloy A2 is sent to the side furnace of the die casting machine for melting and die casting production. The die casting process parameters are: casting temperature 700°C, mold preheating temperature 260°C, casting boost pressure 300MPa, and injection speed 4m / s. The die casting sample obtained in this example is a thin-walled casting (thickness 3mm), and the room temperature elastic modulus is measured to be 180GPa, the room temperature tensile strength is measured to be 281MPa, the yield strength is 220MPa, the elongation is 13%, and the hardness is 68HBW. Example 3

[0009] In this embodiment, aluminum alloy A3 is provided, and the chemical composition is as follows by mass percentage: zirconium 12.0%, nitrogen 1.2%, boron 0.2%, titanium 0.7%, rhenium, cerium, and strontium are all 0.2%, and the rest is aluminum and inevitable impurities; wherein, the mass percentage of the impurity content is less than 0.15%, and the remainder is Al. The preparation method of the aluminum alloy is: using 99.7% or more of the original aluminum A00 to heat and melt, the melting temperature is 720°C, after A00 is melted, zirconium is added at a mass percentage of 12.0%, and the temperature is increased to melt, the melting temperature is 800°C, after the zirconium is melted, 1.2% of the mass percentage of nitrogen is introduced into the melt, specifically, aluminum nitride powder is added to the high-temperature melt, and then boron is added at a mass percentage of 0.2%, and titanium is added at a mass percentage of 0.7%. After melting, aluminum, zirconium, nitrogen, boron, and titanium melts are obtained. The aluminum alloy solution is adjusted to 690°C, and aluminum master alloy is added according to the mass percentage of rhenium, cerium, and strontium by 0.2%, and the obtained aluminum alloy ingot of aluminum alloy A3 is sent to the side furnace of the die casting machine for melting and die casting production, wherein the die casting process parameters are: casting temperature 700°C, mold preheating temperature 260°C, casting boost pressure 300MPa, and injection speed 4m / s. The die casting sample obtained in this example is a thin-walled casting (thickness 3mm), and the room temperature elastic modulus is measured to be 260GPa, the tensile strength is 289MPa, the yield strength is 139MPa, the elongation is 11.5%, and the hardness is 71HBW.

Claims

1. A heat-treatment-free aluminum alloy material, characterized in that: Its components include aluminum, zirconium, titanium, boron, rhenium, cerium and strontium, and also contain nitrogen. The mass percentages of the components are: zirconium 7-12%, nitrogen 0.001-1.2%, titanium 0.4-0.7%, boron 0.0001-0.2%, rhenium, cerium and strontium are all 0.0001-0.2%, and the rest are aluminum and unavoidable impurities, wherein the mass percentage of the impurity content is less than 0.15%.

2. The method for preparing a heat-treatment-free aluminum alloy material according to claim 1, characterized in that: The method comprises the following steps: using 99.7% or more original aluminum A00 to heat and melt, the melting temperature is 650°C-720°C, after the A00 is melted, adding zirconium at a mass percentage of 7-12%, and heating to melt, the melting temperature is 730°C-800°C, introducing nitrogen into the melt after the zirconium is melted, then adding boron at a mass percentage of 0.0001-0.2%, adding titanium at a mass percentage of 0.4-0.7%, waiting for the melt to obtain aluminum, zirconium, nitrogen, titanium, and boron melts, adjusting the aluminum alloy solution to 690°C-720°C, adding aluminum master alloy at a mass percentage of 0.0001-0.2% of rhenium, cerium, and strontium, and heating the mold to obtain an aluminum alloy ingot or casting.

3. The preparation method according to claim 2, wherein the nitrogen element is introduced by adding aluminum nitride fine powder into the high-temperature melt.

4. According to the preparation method of claim 2, the aluminum alloy material prepared has an elastic modulus of up to 260GPa, a tensile strength ≥260MPa, a yield strength ≥120MPa, an elongation ≥10%, and a hardness ≥65HBW, and can be used for heat treatment-free casting.

5. According to the preparation method of claim 2, the aluminum alloy material prepared has the properties of corrosion resistance, antibacterial and mildew resistance.

Citation Information

Patent Citations

  • Musical instrument.

    US734262A