High stability and low yield strength ratio hot rolled welding bottle steel

By controlling the composition and production process of welding cylinder steel, especially the steel throwing speed and laminar flow cooling mode, the problem of large fluctuation and low hit rate of welding cylinder steel is solved, and high stability and low yield and strength ratio is achieved. The cylinder steel is produced, meeting the requirements of high strength and toughness.

CN116287971BActive Publication Date: 2024-11-22LIUZHOU IRON & STEEL CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202211385028.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-26
Publication Date
2024-11-22
Estimated Expiration
2041-10-26

AI Technical Summary

Technical Problem

The yield strength ratio fluctuates greatly and the yield strength ratio is lower than the hit rate of the existing hot-rolled welded cylinder steel, making it difficult to meet the high strength and toughness requirements during the production process.

Method used

By controlling the composition and production process of welded cylinder steel, including limiting the steel throwing speed, adjusting the laminar flow cooling mode and cooling speed, we ensure that the yield strength ratio is below 0.75, and adopting a production method with high stability and low yield strength ratio to ensure the yield strength ratio Hit rate reaches 100%.

Benefits of technology

The high stability and low yield-strength ratio of welded cylinder steel is achieved, with yield-strength ratio less than 0.75 and the hit rate reaches 100%, ensuring the high strength and toughness properties of welded cylinder steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116287971B_ABST
    Figure CN116287971B_ABST
Patent Text Reader

Abstract

The present invention provides a high-stability, low-yield ratio hot-rolled welding bottle steel, wherein the metallographic structure of the high-stability, low-yield ratio hot-rolled welding bottle steel is: ferrite + pearlite, grain size 11, and yield ratio less than 0.75. The present invention innovatively limits the increase in the speed of finishing rolling and steel throwing without significantly modifying the existing equipment of the rolling line. The structure of the obtained welding bottle steel is basically a normal equiaxed ferrite + pearlite structure, and the yield ratio hit rate is high.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application, the parent application is: Application Number: 2021112525602, Invention Name: High stability and low yield ratio hot-rolled welded bottle steel and its production method, Application date: 2021.10.26. Technical Field

[0002] The invention relates to the field of steel rolling, and in particular to a hot-rolled welded steel with high stability and low yield strength ratio. Background Art

[0003] Welding cylinder steel refers to the steel used to produce liquefied petroleum gas or dissolved acetylene gas. Because it contains flammable and explosive liquids or gases, the parent material of the welding cylinder must have higher strength and toughness indicators. The production process of welding gas cylinders mainly consists of drawing and welding. In order to ensure the smooth completion of the drawing process, the parent material welding cylinder steel must also have good cold forming properties. The yield strength ratio ReL / Rm value is an important technical indicator to measure the cold forming performance of steel plates. The national standard GB / T 6653 stipulates that the yield strength ratio ReL / Rm of welding cylinder steel is ≤0.80.

[0004] Existing research on the control of yield ratio of welding bottle steel often focuses on the cooling mode. The consensus has been formed that the two-stage cooling mode of hot rolling laminar cooling is conducive to obtaining welding bottle steel with low yield ratio. However, in actual production, even if the two-stage cooling mode is adopted, there is often a large fluctuation in the yield ratio of welding bottle steel and a low yield ratio hit rate, which is only about 80%.

[0005] In summary, the prior art has the following problems: the yield strength ratio of hot-rolled welded bottle steel fluctuates greatly and the yield strength ratio hit rate is low. Summary of the invention

[0006] The present invention provides a high-stability and low-yield ratio hot-rolled welded bottle steel and a production method thereof, that is, a hot-rolled welded bottle steel and a production method thereof, so as to solve the problems of large fluctuation in the yield ratio and low yield ratio hit rate of the hot-rolled welded bottle steel.

[0007] To this end, the present invention proposes a method for producing hot-rolled welded steel with high stability and low yield ratio, the method comprising:

[0008] The composition of the hot-rolled welding bottle steel is as follows by weight percentage Wt%: C≤0.18, Si≤0.10, Mn: 0.70~1.00, P≤0.025, S≤0.012, Alt≥0.020, Ti≤0.060;

[0009] The method for producing hot-rolled welded steel with high stability and low yield ratio is produced according to the following processes: slab continuous casting, hot-rolled slab heating, rough rolling, finishing rolling, layer cooling and coiling; according to the different laminar cooling control capabilities of the rolling line, the laminar flow speed, temperature and layer cooling mode are set. Among them, the laminar cooling control capability of the rolling line is based on whether it has the ability to independently set the target temperature of the middle section, the air cooling time, and the cooling speed of the front and rear sections.

[0010] Furthermore, the fluctuation of the throwing speed of the entire strip coil is limited, the speed of the tail of the strip is limited to be 30% higher than the speed of the head, the feedback adjustment function of the cooling water between the frames and the final rolling temperature is added, and the final rolling temperature of the strip is corrected by the amount of cooling water between the frames to within ±20°C of the target final rolling temperature value.

[0011] Furthermore, 0.12≤C≤0.18 to achieve precise control.

[0012] Furthermore, 0.24≤Alt≤0.30 to achieve precise control.

[0013] Furthermore, 0.01≤Ti≤0.20 to achieve precise control.

[0014] Furthermore, Mn: 0.76-0.80 to achieve precise control.

[0015] Furthermore, when the laminar cooling control capability of the rolling line is high, the goal is still to ensure the final stable laminar temperature, and the newly added laminar middle section target temperature, air cooling time, front section cooling rate, rear section cooling rate, front and rear section boiling water groups and header numbers are automatically adjusted.

[0016] Furthermore, when the laminar cooling control capability is low, the dynamic laminar temperature target temperature is set with the cooling rate control as the purpose. The laminar temperature adjustment range is set, and the actual control of the strip laminar target temperature matches the percentage of the finishing rolling speed range. For example, the minimum strip rolling speed Vmin, the maximum strip rolling speed Vmax, the speed Vactual at a certain moment, the laminar setting temperature Tset, and the laminar temperature adjustment range Tfan, then the actual laminar target temperature Tactual = (Vactual-Vmin) / (Vmax-Vmin)*Tfan+Tset, where Vmin, Vmax, and Vactual are all in m / s, and Tset and Tfan are in seconds.

[0017] Furthermore, a hot coil box is put into use.

[0018] Furthermore, the time from the finishing rolling exit to the start of laminar cooling is shortened, and the starting header of the laminar front cooling is ensured to be in the first group.

[0019] Furthermore, when sampling the strip test samples, the tail cutting length is increased, and the tails are cut and piled together for air cooling to avoid separate cooling.

[0020] Furthermore, the hot-rolled welded steel is a 3 mm thick steel strip, a hot coil box is used, the finishing rolling speed is 9.5 m / s, the final rolling temperature is 880°C, the laminar flow temperature is 600°C, and the laminar flow cooling mode is two-stage cooling.

[0021] Furthermore, the hot-rolled welding bottle steel is a 3mm thick steel strip, the hot coil box is not used, the finishing rolling speed is: 8.5m / s at the head and 11.5m / s at the tail, the final rolling temperature is 880℃, the laminar temperature is 600℃, the laminar cooling mode is two-stage cooling, the target temperature of the laminar middle section is 720℃, the air cooling time is 4s, and the maximum cooling rate of the front and rear sections is 50℃ / s.

[0022] Furthermore, the hot-rolled welded steel is a 3mm thick steel strip, the hot coil box is not used, the finishing rolling speed is: 9m / s at the head and 12m / s at the tail, the final rolling temperature is 880℃, the laminar temperature is 600℃, the laminar cooling mode is two-stage cooling, the minimum strip rolling speed Vmin, the maximum strip rolling speed Vmax, the speed at a certain moment Vactual, the laminar set temperature Tset, the laminar temperature adjustment range is Tfan, the actual laminar target temperature Tactual = (Vactual-Vmin) / (Vmax-Vmin)*Tfan+Tset, the units of Vmin, Vmax, and Vactual are all m / s, and the units of Tset and Tfan are all seconds.

[0023] The present invention also provides a high-stability and low-yield ratio hot-rolled welding bottle steel, wherein the composition of the hot-rolled welding bottle steel is as follows by weight percentage Wt%: C≤0.18, Si≤0.10, Mn: 0.70-1.00, P≤0.025, S≤0.012, Alt≥0.020, Ti≤0.060;

[0024] The high stability and low yield ratio hot rolled welded bottle steel adopts the high stability and low yield ratio hot rolled welded bottle steel production method mentioned above. The metallographic structure of the high stability and low yield ratio hot rolled welded bottle steel is: ferrite + pearlite, grain size level 11, and yield ratio less than 0.75.

[0025] The welding bottle steel is a strip steel with a thickness of, for example, 3 mm.

[0026] Furthermore, 0.12≤C≤0.18 to achieve precise control.

[0027] Furthermore, 0.24≤Alt≤0.30 to achieve precise control.

[0028] Furthermore, 0.01≤Ti≤0.20 to achieve precise control.

[0029] Furthermore, Mn: 0.76-0.80 to achieve precise control.

[0030] Through the analysis of production conditions, the applicant found that the yield strength ratio of welding bottle steel is also strongly affected by the use of hot coil box, steel throwing speed, front and rear header water mode, and sampling method under the premise of using forward and backward cooling. Based on the above analysis, the applicant innovatively limits the increase in finishing rolling speed steel throwing speed by combining the steel throwing speed with the temperature and cooling rate of laminar cooling without significantly modifying the existing equipment of the rolling line. The microstructure of the obtained welding bottle steel is basically normal equiaxed ferrite + pearlite microstructure, with a yield strength ratio of less than 0.75 and a yield strength ratio hit rate of 100%. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The metallographic structure photograph of the hot-rolled welding bottle steel with high stability and low yield strength ratio obtained by the production method of the present invention. DETAILED DESCRIPTION

[0032] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the present invention is now described with reference to the accompanying drawings.

[0033] The applicant has found that in the actual production of hot-rolled welding bottle steel, even if a two-stage cooling mode is used, there is often a large fluctuation in the yield strength ratio of the welding bottle steel and a low hit rate. Through a detailed analysis of the production conditions, it is found that the yield strength ratio of the welding bottle steel is also strongly affected by the use of the hot coil box, the steel throwing speed, and the front and rear header water opening mode under the premise of using forward and backward cooling. The present invention specifically controls the influencing factors such as the use of the hot coil box, the steel throwing speed, and the front and rear header water opening mode, thereby forming a complete high-stability and low-yield ratio hot-rolled welding bottle steel production method.

[0034] In the existing production and research of welding bottle steel, the hot rolling laminar cooling mode is generally two-stage cooling, that is, after the finishing rolling is completed, a part of the laminar header is opened in the front section of the laminar flow to cool the strip to a certain temperature, and then the middle section of the laminar flow is air-cooled for a period of time, and finally a certain laminar header is opened in the end section of the laminar flow to ensure the final laminar temperature. For most hot rolling production lines, only the final laminar flow temperature can be controlled more accurately, and the temperature and cooling rate in the middle process of the laminar flow are often controlled by model self-learning and cannot be accurately controlled. The rolling line process regulations usually only define the final rolling temperature, laminar flow temperature and cooling mode, and there are no clear regulations on the actual laminar start method, cooling rate, etc. When the working conditions change, the rationality and stability of temperature control will be lacking. Among them, whether the hot coil box is put into use and the actual water opening method of the laminar flow have the greatest impact on the yield strength ratio.

[0035] When the hot coil box is put into use in the rolling line production, the temperature difference between the head and tail of the strip is small, and the finishing rolling and polishing speed is more uniform. For example, the most common thickness of welding bottle steel is 3.0mm. Taking the rolling line laminar cooling length of 100m, air cooling length of 40m, final rolling temperature of 880℃, and laminar temperature of 600℃ as an example, the finishing rolling exit speed is about 9.5m / s when the hot coil box is put into use. It can be concluded that the time of the strip in the laminar section is 10.5s, the air cooling time is 4.2s, and the average cooling rate of the front and rear cooling sections is 44.4℃ / s.

[0036] When the hot rolled coil cannot be put into use or the rolling line deliberately does not use the hot coil box to improve the rolling rhythm, the temperature difference between the head and tail of the strip will increase significantly. In order to ensure that the final rolling temperature of the tail hits, the control system will adopt the speed-up rolling mode. For example, the most common thickness of welding bottle steel is 3.0mm, with a laminar cooling length of 100m, an air cooling length of 40m, a final rolling temperature of 880℃, and a laminar temperature of 600℃. When the hot coil box is not used, the speed of the front section of the strip is about 8.5m, and the speed of the rear section can reach nearly 11.5m / s. In order to increase the hot rolling output or ensure the rolling rhythm when the hot rolled coil is not put into use, the operator often manually speeds up the throwing speed, so that the speed of the tail of the strip can eventually reach about 12m / s. At this time, it can be concluded that when the hot coil box is not in use, the time the tail of the strip is in the laminar flow section is 8.33s, the air cooling time is 3.33s, and the average cooling rate of the front and rear cooling sections is 56℃ / s; the time the head of the strip is in the laminar flow section is 12.5s, the air cooling time is 5s, and the average cooling rate of the front and rear cooling sections is 37.3℃ / s.

[0037] From the above analysis, it can be concluded that the large fluctuation of the yield strength ratio of welding bottle steel under the same laminar cooling mode is closely related to its actual laminar cooling rate. When the cooling rate is too high, quasi-polygonal ferrite or bainite structure may even appear, resulting in a significant increase in the yield strength ratio. The cooling rate is also affected by the actual steel throwing speed of the rolling line. The steel throwing speed is most strongly affected by whether the hot coil box is put into use or not. In addition, the manual intervention of the operator is also an important factor in the fluctuation of the steel throwing speed.

[0038] In addition, under the same cooling mode, the actual laminar water boiling method is affected by the failure of the laminar flow headers, especially when the first two sets of headers cannot be put into use due to failure. There will be a certain amount of air cooling time after finishing rolling, which will cause the deformed austenite grains after finishing rolling to grow and cause fluctuations in the yield ratio.

[0039] When the coil is sampled off the line, the temperature of the coil is about 400-500℃. The sampler usually cuts a 50-70cm long section from the tail, air cools it or puts it in front of a fan to cool it to near room temperature before taking the test sample. The short sampling length and the large fluctuation of the cooling speed of air cooling or wind cooling after sampling are also the reasons for the large fluctuation of yield strength ratio.

[0040] In view of the above situation, the present invention provides a high stability and low yield ratio hot-rolled welding bottle steel and a production method thereof. The composition control is shown in Table 1:

[0041] Table 1 Composition of hot-rolled welding bottle steel with high stability and low yield strength ratio

[0042] C Si Mn P S Alt Ti ≤0.18 ≤0.10 0.70~1.00 ≤0.025 ≤0.012 ≥0.020 ≤0.060

[0043] The specific operation control of the production method is as follows:

[0044] (1) Limit the fluctuation of the throwing speed of the whole coil of strip, such as limiting the maximum speed of the tail of the strip to 30% higher than the speed of the head, increase the feedback adjustment function of the cooling water between the racks and the final rolling temperature, and correct the final rolling temperature of the strip by the amount of cooling water between the racks.

[0045] (2) When the laminar cooling control capability of the rolling line is high, the goal is still to ensure the final stable laminar temperature. The target temperature of the middle section of the laminar flow, air cooling time, cooling speed of the front and rear sections are added, and the number of hot water groups and the number of headers in the front and rear sections are automatically adjusted.

[0046] (3) When the laminar cooling control capability is low, the dynamic laminar temperature target temperature is set with the cooling speed control as the purpose. Set the laminar temperature adjustment range, and the actual control of the strip laminar target temperature matches the percentage of the finishing rolling speed range. For example, set the minimum strip rolling speed Vmin, the maximum strip rolling speed Vmax, and the speed V at a certain moment 实 , laminar flow set temperature T 设 , the laminar flow temperature adjustment range is T 范 , then the actual laminar flow target temperature T 实 =(V 实 -Vmin) / (Vmax-Vmin)*T 范 +T 设 .

[0047] (4) Use hot coil boxes as much as possible.

[0048] (5) Operators are not allowed to accelerate manually;

[0049] (6) Shorten the time from the finishing rolling exit to the start of laminar cooling, and ensure that the starting header of the laminar front cooling (laminar front cooling mainly increases the driving force of phase transformation by increasing the degree of supercooling and promotes the nucleation of ferrite. Ensuring the first group of cooling can reduce the recovery process of grains after finishing rolling and increase the nucleation rate of ferrite) is in the first group;

[0050] (7) When sampling the strip test sample, the cutting tail length is increased, and the tail is cut and stacked together for air cooling to avoid separate cooling.

[0051] Through the analysis of the actual working conditions of hot rolling, the factors causing large fluctuations in the yield strength ratio of welding bottle steel are determined. By combining the throwing speed with the temperature and cooling rate of laminar cooling, the increase in the speed of finishing rolling and throwing speed is innovatively limited without the need to significantly modify the existing equipment of the rolling line. At the same time, two laminar flow control modes with high stability and yield strength ratio of welding bottle steel are designed: ① Ensure the final stable laminar flow temperature as the target, add the target temperature of the middle section of the laminar flow, air cooling time, cooling rate of the front and rear sections, and automatically adjust the number of water groups and headers in the front and rear sections; ② A control method for matching the fluctuation of the laminar temperature target fluctuation with the fluctuation of the finishing rolling throwing speed. In addition, by controlling the water header in the front section of cooling, the manual speed increase of the operator, the sampling length and stacking, a set of high-stability and low-yield strength ratio welding bottle steel production methods is finally formed.

[0052] After the implementation of the present invention, the microstructure of the welding bottle steel is basically a normal equiaxed ferrite + pearlite microstructure, and the yield strength ratio hit rate reaches 100%. The yield strength ratio is less than 0.75, for example, 0.73, and further, less than 0.73, for example, the yield strength ratio is 0.69, 0.71 or 0.72. The elongation after fracture A% is greater than 35, for example, 35.5, 36, 36.5, 37, 38, or 39.5.

[0053] The high stability and low yield ratio hot rolled welding bottle steel and its production method of the present invention adopt the following composition ratio and specific process. Among them, Table 2 and Table 3 are the composition parameters and process parameters corresponding to the example welding bottle steel, and Table 4 is the comprehensive performance corresponding to the welding bottle steel described in each example of Table 2 and Table 3.

[0054] Table 2 Composition parameters of various examples of welding bottle steel

[0055] Examples C Si Mn P S Alt Ti Example 1 0.1414 0.0431 0.7686 0.0138 0.009 0.0259 0.0169 Example 2 0.1351 0.0499 0.7628 0.0115 0.0047 0.0254 0.013 Example 3 0.1357 0.0316 0.7761 0.012 0.0045 0.024 0.0154 Example 4 0.1255 0.0211 0.78 0.0153 0.0074 0.0287 0.0136 Example 5 0.1354 0.04 0.795 0.0179 0.0093 0.034 0.0174 Example 6 0.1377 0.0272 0.7631 0.0135 0.006 0.0291 0.0143

[0056] Table 3 Process parameters of welding cylinder steel

[0057]

[0058] Table 4 Performance parameters of welding bottle steel

[0059]

[0060]

[0061] The above description is only an illustrative embodiment of the present invention and is not intended to limit the scope of the present invention. The components of the present invention can be combined with each other without conflict, and any equivalent changes and modifications made by any technician in the field without departing from the concept and principle of the present invention should fall within the scope of protection of the present invention.

Claims

1. A hot-rolled welding bottle steel with high stability and low yield strength ratio, characterized in that: The composition of the hot-rolled welding bottle steel is as follows by weight percentage: C: 0.1414, Si: 0.0431, Mn: 0.7686, P: 0.0138, S: 0.009, Alt: 0.0259, Ti: 0.0169, and the rest is iron; The metallographic structure of the high stability and low yield strength ratio hot rolled welding bottle steel is: ferrite + pearlite, grain size 11, and the tensile strength of the high stability and low yield strength ratio hot rolled welding bottle steel is R m 458N / mm 2 , yield strength ratio is 0.69; lower yield strength R eL : 315N / mm 2 , elongation after break A% is: 39.5; The method for producing hot-rolled welded steel with high stability and low yield ratio is produced according to the following process: slab continuous casting, hot-rolled slab heating, rough rolling, finish rolling, layer cooling and coiling; The hot-rolled welding bottle steel is a 3mm thick steel strip, and a hot coil box is used. The finishing rolling speed is 9.5 m / s, the final rolling temperature is 880℃, the laminar flow temperature is 600℃, and the laminar cooling mode is two-stage cooling.

Citation Information

Patent Citations

  • Device and method for cooling intermediate rolled blank of hot rolled strip

    CN101972782A

  • 345 MPa-grade welding cylinder steel and manufacturing method thereof

    CN106319372A

  • Low-yield-ratio welding bottle steel and making method thereof

    CN107988549A

  • Low-yield-ratio high-reaming-property hot-rolled steel plate with tensile strength of 440 MPa grade

    CN110656292A

  • Hot-rolled steel plate with yield strength of 450 MPa and manufacturing method thereof