Preparation technology of composite multifunctional fiber

By precisely controlling the melting temperature and pressure of the material, combined with electrospinning and dry and wet cooling technology, the problems of limited functions and poor quality of composite fiber products are solved, and the preparation of multifunctional fibers and the production of high-value-added products are realized.

CN116288765BActive Publication Date: 2024-11-08TIANJIN HENGYU MAGNETIC PLASTIC PROD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310390873.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2024-11-08
Estimated Expiration
2043-04-13

AI Technical Summary

Technical Problem

The existing composite fiber products have limited functions and are limited by materials and structure, and have poor application effects. In the fiber manufacturing process, there are problems such as unstable melting temperature, uneven cooling, and insufficient monofilament strength, resulting in poor product quality and shortened life.

Method used

The multi-functional fiber preparation process is adopted, and the melting temperature and pressure of the material is accurately controlled, electrospinning control technology and dry and wet cooling technology are used, and composite fiber filaments are formed to improve the functionality and quality of the fibers.

Benefits of technology

The production of various functional fiber filaments has been achieved, which has increased the added value of fibers, extended the product life, and improved the breaking strength and uniformity of fibers, meeting the functional application needs of tourism, economy, clothing and special industries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116288765B_ABST
    Figure CN116288765B_ABST
Patent Text Reader

Abstract

The present invention provides a composite multi-functional fiber preparation process, which is characterized in that it includes step one: injecting functional materials into different extruders to form functional masterbatches, and controlling the supply amount of the functional masterbatches by a metering pump; then passing through respective biphenyl heating furnaces, accurately controlling the melting temperature and suitable pressure of each material and conveying them through a single tube and single temperature control; step two: the molten functional masterbatch is pumped into a biphenyl spinning box, and passes through a composite mold in the box to form composite fiber filaments; in the present invention, the discharge ports of multiple extruders all adopt sleeve drainage, and adopt single tube and single temperature control technology, each material uses its own separate temperature control device to accurately control the melting temperature of the material, and a biphenyl heating circulation method is adopted on the spinneret and pipeline of the processing mold to ensure that the melting temperatures of various materials in the melt in the mold are appropriate and uniform, thereby improving the compatibility and production efficiency of the product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite fiber preparation, and in particular to a process for preparing composite multifunctional fibers. Background Art

[0002] Functional fibers are developing rapidly at this stage. Typical composite functional fiber structures include skin-core type, parallel type, and M-shaped type. Fibers with composite structures will have some functions attached. For example, antibacterial fiber and polyester-nylon composite fiber are products currently prepared from composite fibers. They are a composite fiber composed of two polymers with different chemical structures and properties. Through the composite structure, the functional monofilaments can achieve antibacterial, mosquito repellent, micro-conductivity and other functional properties.

[0003] However, at present, the skin-core type, parallel type and cross-shaped structures can generally only have one or two functions at the same time, and the functions are relatively few. At the same time, they are affected by the specific surface area, surface energy and surface activity, so that their application effects are greatly reduced, and it is difficult to produce high value-added products. Moreover, the functions of the products formed are affected by the materials and structures themselves, and their efficacy is far lower than the application effect, and the life of the products themselves is greatly reduced.

[0004] In addition, in the current fiber manufacturing process, there are still problems such as unsatisfactory melting temperatures between various materials, unstable conveying temperatures, resulting in poor material fusion effects, uneven cooling of single filaments, poor quality, insufficient single filament strength, and easy breakage. Summary of the invention

[0005] In view of the above technical problems, the present invention provides a process for preparing composite multi-functional fibers capable of producing fiber yarns with multiple functions.

[0006] The present invention provides a process for preparing a composite multifunctional fiber, which is characterized by comprising the following steps:

[0007] Step 1: First, the main material and functional auxiliary materials are dried and pre-treated separately, and then various materials are injected into different extruders respectively, and the supply amount of functional masterbatch is controlled by metering pumps; then, the melting temperature of each material is accurately controlled through their respective biphenyl heating furnaces, and they are transported through single-tube single-control with appropriate temperature and pressure;

[0008] Step 2: The molten main material and the functional auxiliary material are pumped into the tooth-shaped composite mold respectively, and the composite fiber monofilament is formed after flowing through the composite mold;

[0009] Step 3: Use the electrospinning control process to add an electrostatic field to the wire outlet of the mold. Through the action of the electric field, the monofilament runs stably to avoid clogging the wire outlet;

[0010] Step 4: The composite fiber filaments obtained in step 3 are cooled by dry-wet cooling technology, firstly pre-cooling by ring-blown air cooling, then cooling by coolant to ensure a smooth surface; then further cooling by air cooling machine to achieve air drying effect;

[0011] Step 5: The composite fiber obtained in step 4 is subjected to a high temperature and low cooling stress relief method, and is subjected to multiple shaping processes to be drawn and shaped;

[0012] Step 6: The composite fiber yarn obtained in step 5 is wound by a single-spindle coiling and collecting machine to form a finished product and then packaged in barrels.

[0013] Furthermore, the main material in step 1 is PET, and the specific steps of the main material drying pretreatment are: drying the main material twice, the first drying temperature is 110°C, and the drying lasts for 2 hours, the main material forms pre-crystallization to prevent sticking, and then the temperature is adjusted to 160°C for 4 hours to remove moisture and make the moisture content less than 100PPM; then pre-heating is performed at a temperature of 200°C;

[0014] Furthermore, the functional auxiliary material in step 1 includes a base material and a functional masterbatch, the base material is PE, and the functional masterbatch is added and mixed into the base material according to the required function, and the functional masterbatch component is added to 30-50% of the base material, which can improve the surface function of the composite monofilament by 20-40%; and the meltability is relatively good, which can enhance the adhesion of the material;

[0015] Furthermore, the specific steps of pre-drying the functional auxiliary material are: drying the functional auxiliary material once at a drying temperature of 110°C for 4 hours to make the moisture content less than 100PPM; then pre-heating to 200°C.

[0016] Furthermore, the heating temperature of the extruder for conveying the main material in the step one is set at 260-290°C, the pressure of the metering pump for conveying the main material in the step one is less than 35 MPa, the conveying temperature of the single-tube single-control for conveying the main material in the step one is 270°C, and the mass ratio of the input molten material is 1.00-1.15g / ml; the temperature of the extruder for conveying the functional auxiliary material in the step one is 160-220°C, the pressure of the metering pump for conveying the auxiliary material in the step one is less than 10 MPa, the conveying temperature of the single-tube single-control for conveying the auxiliary material in the step one is 230°C, and the mass ratio of the input molten material is 0.86-0.96g / ml.

[0017] Furthermore, the composite mold in step 2 is composed of a plurality of spinnerets, the plurality of spinnerets are interconnected, each spinneret is provided with a feed hole, and the temperature of each spinneret is 260°C.

[0018] Furthermore, the specific steps of the multi-step shaping process in step 5 are:

[0019] First drafting: Use steam engine to heat to 83-88℃, and then do the first drafting, the drafting multiple is 3-5 times;

[0020] Second drafting: Use steam engine to heat to 140℃, and then do the second drafting, the drafting multiple is 0.8-1.2 times;

[0021] Stress relief stretching: Use a steam engine to heat to 160°C and perform the third stretching with a stretching multiple of 0.8-1.2 times.

[0022] The beneficial effects of the present invention are as follows: the present invention is a composite multifunctional fiber preparation process, different materials are extruded by multiple extruders, and then the flow rate is controlled by a metering pump, and then the metering pump is pumped into the composite mold, wherein the main material uses PET as a carrier and flows into the middle of the composite mold, and the PET melt passes through the thin strip gap formed by the internal tooth shape of the composite mold in another patent application, and the melt in the gap rubs against the inner wall of the tooth shape in a small space to form a fixed embedded structure, and then the auxiliary materials with different functions such as bactericidal masterbatch, antibacterial masterbatch, conductive masterbatch and mosquito repellent masterbatch are used as PE as a carrier, placed in other extruders and then the flow rate is controlled by a metering pump, and then the temperature control device is used to pump the constant temperature and pressure into the outer ring of the composite mold, and the composite monofilament is extruded and leveled through the leveling groove in the composite mold, and then processed into a composite monofilament with the main material, and the composite monofilament can be further processed into different functional products, such as tourism economy, clothing and its products, civil construction and special industry dust prevention, protective shielding and many other functional series applications.

[0023] For melt spinning, the temperature of the melt directly affects the viscosity of the melt surface. If the viscosity is greatly different, the spinning stripping is uneven, which leads to poor functional use of the fiber. In order to avoid this problem, the discharge ports of multiple extruders in the present invention all use sleeve drainage, and adopt single-tube single-control temperature control technology. Each material uses its own separate temperature control device to accurately control the melting temperature of the material, and a biphenyl heating circulation method is used on the spinneret and pipeline of the processing mold to ensure that the melting temperature of various materials in the melt is appropriate and uniform in the mold, thereby improving the compatibility and production efficiency of the product;

[0024] In the current fiber filament production, the commonly used cooling method is mostly wind cooling, but wind cooling will cause uneven cooling of the single filament, and the side wind will also affect the uniformity of the single filament, so that the melt cannot be effectively cooled after being ejected, affecting the quality of the filament. The present invention adopts dry and wet cooling technology, first uses ring blowing air cooling for pre-cooling, and then uses coolant for cooling, which can ensure the smooth surface of the fiber filament and solve the problem of uneven air cooling; then it is further cooled to the optimal temperature by a cold air machine and air-dried.

[0025] During the winding process, the present invention adopts a high-temperature steam engine, which repeatedly performs three shaping steps with 83-160 degree high-temperature steam to achieve a stress relief effect, replacing the hot water tank in traditional single-filament process equipment to achieve a high-speed and stable wire drawing process. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic diagram of the process of the present invention;

[0027] Figure 2 It is a cross-sectional schematic diagram of the main material and the functional auxiliary material of the present invention being respectively injected into the composite mold;

[0028] Figure 3 A cross-sectional view of the composite fiber produced by the present invention;

[0029] Figure 4 This is a schematic diagram of a single-tube single-control process in step 1 of the present invention;

[0030] Figure 5 This is a schematic diagram of the dry and wet cooling process in step 4 of the present invention;

[0031] Figure 6 This is a schematic diagram of the multi-pass shaping and stress relief process in step five of the present invention;

[0032] Figure 7 This is a schematic diagram of adding a conductive material in Example 4 of the present invention.

[0033] Figure numerals: 1-extruder outlet; 2-toothed composite mold; 3-main material; 4-functional auxiliary material; 5-conductive material. DETAILED DESCRIPTION

[0034] The technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings of the present invention.

[0035] Example 1

[0036] First, PET after drying and pretreatment is used as the main material and injected from the extruder connected to the middle of the tooth-shaped composite mold, wherein the main material is injected into the middle extruder, and the extrusion temperature range of the extruder is set to 260-290°C. At the same time, the auxiliary material with PE as the base material and mixed with other functional masterbatches after drying and pretreatment is injected into other extruders, and the temperature of the extruder is set to 160-220°C; then the main material and the auxiliary material are respectively pumped into the tooth-shaped composite mold through the corresponding metering pump and the single-tube single-control device, wherein the metering pump pressure corresponding to the main material is less than 35MPa, and the temperature of the single-tube single-control delivery is 270°C, and the metering pump pressure corresponding to the auxiliary material is less than 10MPa, and the temperature of the single-tube single-control delivery is 230°C;

[0037] The molten functional material is pumped into the tooth-shaped composite mold, and forms composite fiber filaments after flowing through the tooth-shaped composite mold; the tooth-shaped composite mold is placed in a biphenyl heating box and maintained at a constant temperature of 260°C. The tooth-shaped composite mold has been patented separately and will not be described in detail here;

[0038] Using the electrostatic spinning control process, an electrostatic field is added to the die outlet hole. Through the action of the electric field, the monofilament runs stably and avoids clogging the spinneret hole.

[0039] After that, it is cooled by dry and wet cooling technology, firstly using ring-blown air cooling for pre-cooling, then using coolant to cool and ensure its surface is smooth; then it is further cooled by air cooler and achieves air drying effect, specifically, first using ring-blown air cooling, the purpose is to reduce the temperature of the just-exported monofilament from 260℃ to 150℃, wind speed: 5m / s, then it enters the cooling water tank, the water tank temperature is controlled at about 40℃, and then adding another air cooling, wind speed: 5m / s, to reduce humidity, dry the monofilament, and reduce the humidity to 15%;

[0040] Then, a high-temperature and low-cooling stress relief preparation method is used, and multiple shaping processes are performed to shape the wire. Specifically, the first drawing process is to heat the wire to 83-88°C with a steam engine, and then draw the wire for the first time. The drawing multiple is 3-5 times, for example, the single wire is stretched from 50 meters per minute to 150-250 meters, and then enters natural wind cooling.

[0041] Second drawing: use steam engine to heat 140℃, carry out second drawing, drawing multiple: 0.8-1.2 times, for example: stretch the monofilament from 50 meters per minute to 40-60 meters, and then enter natural wind cooling; finally stress relief drawing: use steam engine to heat 160℃, carry out third drawing, drawing multiple: 0.8-1.2 times, for example: stretch the monofilament from 50 meters per minute to 40-60 meters, and then enter natural wind cooling, to achieve high-speed and stable wire drawing process;

[0042] Finally, the finished product is wound by a single-spindle coiling machine and packaged into barrels.

[0043] The composite yarn thus obtained has a breaking strength of >0.28 cN / dtex, a breaking strength variation coefficient of 2.03, a breaking elongation of <148%, a breaking elongation variation coefficient of 3.25, a linear density of 249.3 dtex, a linear density variation coefficient of 0.21, and an antibacterial effect that meets the SEK orange standard.

[0044] The temperature of the aqueous solution in the water tank is 40-80°C, the distance between the spinning end of the spinneret assembly and the water surface of the water tank is 20-40cm, the distance between the roller in the water tank and the water surface is 40-160cm, and the aqueous solution is a clean water liquid without additives.

[0045] Example 2

[0046] The main material PET is mixed with functional materials with pro-conductive properties, heated and melted together, extruded through the middle extruder, and transported to the tooth-shaped composite spinning mold through a metering pump and a single-tube single-control. The main material mixed with the pro-conductive material is fed into the mold through the mold feed port and processed to form the central tooth-shaped substrate of the composite fiber. At this time, the pro-conductive material is evenly integrated into the tooth-shaped substrate, and then fused with various functional materials to form a successful composite monofilament, which flows out of the mold through the mold outlet hole.

[0047] At this time, electrostatic spinning control technology is used at the wire outlet of the mold. By adding a strong electric field around the monofilament and adding another electric field on the receiving plate, the conductive material in the composite monofilament toothed substrate is guided to run smoothly, preventing blockage of the wire outlet and causing problems such as insufficient roundness of the monofilament. At the same time, it can ensure that the monofilament maintains roundness and uniformity when cooled by natural wind. The monofilament is then received by the receiving plate and enters the next process.

[0048] The conductive masterbatch is made by mixing resin substrate, carbon black and other additives. It can increase the conductivity or anti-static performance of the main material on the inherent characteristics. The addition amount is very low, generally 0.1% of the PET main material, and the added electric field is generally 30,000 volts of high-voltage static electricity. This technology can effectively improve the roundness of the single yarn and prevent the phenomenon of clogging the outlet hole. At the same time, less functional materials are added, saving costs, and there is no need to change the spinning mold. This method does not require the use of spinning solution, spinning cones, spinning nozzles and other components, which greatly simplifies the electrospinning process and improves the effect.

[0049] Example 3

[0050] A functional material with conductive properties is mixed into one of the auxiliary materials PE, heated and melted, extruded through an extruder for the adjacent auxiliary material, and transported to a tooth-shaped composite spinning die through a metering pump and a single-tube single-control system. The PE auxiliary material mixed with conductive materials is fed into the die through the feed port on the outer ring of the die, evenly buffered by a multi-layer die, extruded at an even pressure through a leveling layer, and the conductive materials are filled into the gap of the tooth structure every 120°, fused with the main material base material, to form a composite monofilament with multiple functions, which flows out of the die through the die outlet hole.

[0051] At the wire outlet of the mold, electrostatic spinning control technology is used. By adding a strong electric field around the monofilament and adding another electric field on the receiving plate, the conductive material in the composite monofilament tooth-shaped substrate is guided to run smoothly to prevent blockage of the wire outlet and insufficient roundness of the monofilament. Through the three-point positioning plane, there is conductive material every 120° to maintain structural stability, ensure the uniformity and roundness of the monofilament, and ensure that the monofilament is not affected by crosswind when in the natural wind cooling state, thus maintaining roundness and uniformity. After that, the monofilament is received by the receiving plate and enters the next process.

[0052] This spinning die is transformed and upgraded on the basis of the 1+N multi-tooth structure die, and the tooth structure is changed into a multiple structure of 3 equal parts (3, 6, 9...), and a special single-filament structure is formed by filling the gap between the gears at every 120-degree angle with conductive materials. Then, when passing through the electrospinning process, under the action of the electric field, the uniformity and roundness of the single filament are kept unaffected by a three-point fixing method, and at the same time, it runs stably without clogging the outlet of the spinneret.

[0053] The conductive masterbatch is made by mixing resin matrix, carbon black and other additives. It can increase the conductivity or anti-static performance of the auxiliary material on the inherent properties. The amount of addition is very low, generally 0.1% of the PE auxiliary material, and the added electric field is generally 30,000 volts of high-voltage static electricity. The spinning nozzle (wire outlet) faces the receiving electrode, the spinning nozzle is electrically connected to the positive electrode of the power supply, and the receiving electrode is electrically connected to the negative electrode of the power supply or grounded. This method does not require the use of spinning solution, spinning cones, spinning nozzles and other components, which greatly simplifies the electrospinning process and improves the effect.

[0054] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. The various components mentioned in the present invention are common technologies in the existing field. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only to illustrate the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection claimed by the present invention is defined by the attached claims and their equivalents.

Claims

1. A process for preparing composite multifunctional fibers, characterized in that The following steps are involved: Step 1: First, the main material and functional auxiliary materials are dried and pre-treated separately, and then various materials are injected into different extruders respectively, and the supply amount of functional auxiliary materials is controlled by metering pumps; then, the melting temperature of each material is accurately controlled through their respective biphenyl heating furnaces, and they are transported through single-tube single-control with appropriate temperature and pressure. The main material is PET, and the functional auxiliary materials include base material PE and functional masterbatch; Step 2: The molten main material and various functional auxiliary materials are pumped into the tooth-shaped composite mold respectively, and the composite fiber monofilament is formed after flowing through the composite mold for processing. The composite mold is composed of a plurality of spinnerets, and the plurality of spinnerets are connected to each other. Each spinneret is provided with a feed hole. The composite mold is a 1+N complex tooth-shaped structure, 1 is the main material as the base material, and N is the various functional auxiliary materials as the base material, so that the main material is a tooth-shaped structure, and the various functional auxiliary materials are filled in the gap of the tooth-shaped structure of the main material, and the conductive material is filled in the gap of the tooth-shaped structure every 120°; Step 3: Use the electrospinning control process to add an electrostatic field to the wire outlet of the mold. Through the action of the electric field, the monofilament runs stably to avoid clogging the wire outlet; Step 4: The composite fiber obtained in step 3 is cooled by dry-wet cooling technology, firstly, pre-cooling is performed by ring-blown air cooling, then cooling is performed by coolant to ensure that the surface is smooth; then further cooling is performed by air cooling machine to achieve air drying effect; Step 5: The composite fiber obtained in step 4 is subjected to a high temperature and low cooling stress relief method, and is subjected to a multi-step shaping process to be drawn and shaped; the specific steps of the multi-step shaping process in step 5 are: First drafting: Use steam engine to heat to 83-88℃, carry out the first drafting, the drafting multiple is 3-5 times, and enter natural wind cooling; Second drafting: Use steam engine to heat to 140℃, carry out second drafting, the drawing multiple is 0.8-1.2 times, and enter natural wind cooling; Stress relief drawing: Use steam engine to heat to 160℃, carry out the third drawing, the drawing multiple is 0.8-1.2 times, and enter natural wind cooling; The obtained composite fiber has a breaking strength of >0.28 cN / dtex, a breaking strength variation coefficient of 2.03, a breaking elongation of <148%, a breaking elongation variation coefficient of 3.25, a linear density of 249.3 dtex, a linear density variation coefficient of 0.21, and an antibacterial effect that meets the SEK orange standard; Step 6: The composite fiber yarn obtained in step 5 is wound by a single-spindle coiling and collecting machine to form a finished product and then packaged in barrels.

2. The process for preparing the composite multifunctional fiber according to claim 1, characterized in that The specific steps of the main material drying pretreatment are: drying the main material twice, the first drying temperature is 110°C, lasting for 2 hours, the main material forms pre-crystallization to prevent sticking, and then adjusting the temperature to 160°C for 4 hours to remove moisture to make the moisture content less than 100PPM, and then pre-heating to 200°C; The functional masterbatch is added and mixed into the base material according to the required functions. The functional masterbatch component is added to 30-50% of the base material, which can improve the surface function of the composite monofilament by 20-40%, and has better meltability, which can enhance the adhesion of the material; The specific steps of pre-drying the functional auxiliary material are: drying the functional auxiliary material once at a drying temperature of 110° C. for 4 hours to reduce the moisture content to less than 100 PPM, and then pre-heating to 200° C.

3. The process for preparing the composite multifunctional fiber according to claim 1, characterized in that The heating temperature of the extruder for conveying the main material in the step one is set at 260-290°C, the pressure of the metering pump for conveying the main material in the step one is less than 35 MPa, the conveying temperature of the single-tube single-control for conveying the main material in the step one is 270°C, and the mass ratio of the input molten material is 1.00-1.15g / ml; the temperature of the extruder for conveying the functional auxiliary material in the step one is 160-220°C, the pressure of the metering pump for conveying the auxiliary material in the step one is less than 10 MPa, the conveying temperature of the single-tube single-control for conveying the auxiliary material in the step one is 230°C, and the mass ratio of the input molten material is 0.86-0.96g / ml.

4. The process for preparing the composite multifunctional fiber according to claim 1, characterized in that In step 2, the temperature of each spinneret is 260°C.