A method for preparing modified thermoplastic polyurethane elastomer multifilament

By blending polyborosiloxane with thermoplastic polyurethane elastomer and adding coupling agent and plasticizer, the degradation problem of thermoplastic polyurethane elastomer under shearing is solved, and its moldability and elongation of break are improved. Achieve an environmentally friendly and pollution-free high-efficiency spinning process.

CN116288811BActive Publication Date: 2024-11-22XIAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310269255.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-11-22
Estimated Expiration
2043-03-20

AI Technical Summary

Technical Problem

Existing thermoplastic polyurethane elastomer fibers are prone to degradation under shearing, resulting in a decrease in melt viscosity, making it difficult to form and wind smoothly, and the phenomenon of wire breakage during production is severe, limiting its application.

Method used

Polyborsiloxane is used to blend with thermoplastic polyurethane elastomer, and coupling agent and plasticizer are added to modify the thermoplastic polyurethane elastomer through melt blending method to improve its shear resistance and compatibility and enhance the melt Strength and fluidity, melt spinning is prepared.

Benefits of technology

The spinning and moldability of thermoplastic polyurethane elastomers is significantly improved, the filament breaking phenomenon is reduced, the filament elongation and elastic recovery rate of fibers are improved, and the processability of melt spinning re-filled.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004134072600000041
    Figure BDA0004134072600000041
  • Figure BDA0004134072600000051
    Figure BDA0004134072600000051
  • Figure BDA0004134072600000052
    Figure BDA0004134072600000052
Patent Text Reader

Abstract

The invention discloses a method for preparing a modified thermoplastic polyurethane elastomer multifilament, and the steps are as follows: step 1: weigh polyborosiloxane, coupling agent and plasticizer in a certain mass ratio, and stir and mix them evenly at a certain temperature; step 2: take the mixture described in step 1, melt blend with thermoplastic polyurethane elastomer in a certain ratio, and granulate; step 3: take the modified thermoplastic polyurethane elastomer particles described in step 2, and vacuum dry them at a certain temperature for a certain time; step 4: take the thermoplastic polyurethane elastomer particles after drying described in step 3, and melt spin them under certain process conditions to obtain modified thermoplastic polyurethane elastomer multifilament. The elastomer multifilament largely overcomes the influence of shear thinning of thermoplastic polyurethane elastomer on fiber molding during melt extrusion, improves melt strength, greatly improves the molding property of thermoplastic polyurethane elastomer fiber, and avoids the phenomenon of broken wire in the winding process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of modified synthetic fibers and relates to a method for preparing a modified thermoplastic polyurethane elastomer multifilament which is environmentally friendly, pollution-free, and has excellent elongation at break and elastic recovery. Background Art

[0002] Elastic fiber fabrics fit the human body and feel smooth, giving clothing fabrics good comfort and excellent beauty. Spandex is the elastic fiber with the widest application range and the most mature commercialization. In recent years, the application of spandex has become increasingly widespread, and the amount added to various new fabrics and functional clothing has increased, ranging from 3% to 30%. Spandex has a large elongation and high elastic recovery rate. A small amount of addition can significantly improve the elasticity of the fabric, so it is known as the "MSG" of textiles.

[0003] At present, there are four production methods for spandex, namely dry spinning, wet spinning, chemical reaction, and melt spinning. The wet spinning and chemical reaction methods have been basically eliminated, and dry spinning is currently used more. Dry-spinning spandex has excellent performance, but its production equipment investment is large and the production cost is high (the cost of raw materials is low); especially in the dry spinning process, a large amount of organic solvents (such as DMF, DMAC, etc.) are used. These toxic solvents are easy to remain on the surface or inside of the fiber. Direct contact will cause damage to the liver and are not suitable for manufacturing fabrics that come into direct contact with the skin; and dry spinning has serious "three wastes" problems, which will cause serious pollution to the environment; in addition, traditional spandex cannot be recycled. Since general spandex is a thermosetting fiber, it is difficult to recycle. With the expansion of the application range of spandex, a large amount of spandex fabrics will inevitably be discarded, causing huge pollution and waste.

[0004] To solve the above problems, thermoplastic polyurethane elastomer fibers produced by melt spinning have attracted widespread attention in the textile industry. Melt spinning equipment requires low investment, the process is simple and stable, the output is high, the production cost is low, and melt spinning does not use organic solvents. The production process is environmentally friendly and pollution-free. The thermoplastic polyurethane elastomer fibers produced are harmless to the human body and have good recycling performance.

[0005] At present, melt-spun thermoplastic polyurethane elastomer yarn has become the most promising alternative to spandex. However, since thermoplastic polyurethane elastomer is very sensitive to shearing, it will degrade with the increase of shear stress or frequency during the melting and heating process, and the melt viscosity will drop sharply. The fiber cannot be smoothly formed and becomes a sparse fluid. In addition, when spinning multifilament, the yarn is very easy to break under the action of winding tension. These problems have greatly limited the production and application of thermoplastic polyurethane elastomer multifilament. Summary of the invention

[0006] In view of the problems existing in the prior art, an object of the present invention is to provide a modified thermoplastic polyurethane elastomer multifilament fiber having good elongation at break and elastic recovery.

[0007] The second object of the present invention is to provide a method for preparing the modified thermoplastic polyurethane elastomer multifilament, which can meet the process requirements of melt-spinning multifilament.

[0008] In order to achieve the above objectives, the present invention adopts the following technical solutions:

[0009] Polyborosiloxane is a new type of polymer material of element-modified polysiloxane, which is a polymer obtained by introducing boron atoms into the silicon-oxygen skeleton of polysiloxane. It has a special physical network structure. The boron atoms in the Si-O-B structure of the polyborosiloxane molecular chain can form a B-O electron bridge pair with the oxygen atoms in the adjacent chain. The electron bridge pair is a dynamically variable physical crosslinking that is in a dynamic process of continuous dissociation and re-formation. Therefore, it has special rheological properties and good viscoelasticity.

[0010] The present invention uses a melt blending method to modify a thermoplastic polyurethane elastomer with polyborosiloxane, thereby improving the shear resistance of the thermoplastic polyurethane elastomer, enhancing its melt strength, and enabling it to be smoothly molded and wound, thereby improving the spinnability of the thermoplastic polyurethane elastomer. A coupling agent is added to improve the compatibility of polyborosiloxane and the thermoplastic polyurethane elastomer, improve their blending dispersion state, and a plasticizer is added to increase melt fluidity, thereby improving the processability of its melt-spinning multifilament. Then, melt spinning is performed to obtain modified thermoplastic polyurethane elastomer multifilament. This scheme is carried out in sequence according to the following steps:

[0011] Step 1: Weigh a certain mass ratio of polyborosiloxane, coupling agent, and plasticizer, and stir and mix them evenly at a certain temperature;

[0012] Step 2: Take the mixture described in step 1, melt blend it with thermoplastic polyurethane elastomer in a certain proportion, and granulate it;

[0013] Step 3: Take the modified thermoplastic polyurethane elastomer particles described in step 2 and vacuum dry them at a certain temperature for a certain period of time.

[0014] Step 4: taking the dried thermoplastic polyurethane elastomer particles described in step 3 and performing melt spinning under certain process conditions to obtain modified thermoplastic polyurethane elastomer multifilaments.

[0015] Preferably, the molar ratio of silicon atoms to boron atoms in the polyborosiloxane described in step 1 is 15.1:1-5.3:1.

[0016] Preferably, the coupling agent described in step 1 includes but is not limited to γ-aminopropyltrimethoxysilane and γ-methacryloyloxy functional alkoxysilane.

[0017] Preferably, the mass ratio of the coupling agent to the polyborosiloxane in step 1 is 2:45-1:18.

[0018] Preferably, the plasticizer described in step 1 includes but is not limited to dimethoxyethylene glycol phthalate and triethylene glycol dipelargonate.

[0019] Preferably, the mass ratio of the plasticizer to the polyborosiloxane in step 1 is 1:18-1:15.

[0020] Preferably, the ratio of the polyborosiloxane to the thermoplastic polyurethane elastomer in step 2 is 1:10.

[0021] Preferably, the spinning speed in step 4 is 400-750 m / min.

[0022] Compared with the prior art, the present invention blends and modifies polyborosiloxane with thermoplastic polyurethane elastomer. Under the action of a coupling agent, polyborosiloxane and thermoplastic polyurethane elastomer can be uniformly mixed and dispersed, thereby improving the interfacial bonding force between polyborosiloxane and thermoplastic polyurethane elastomer in the blended material and improving the mechanical properties of the blended material. The use of a plasticizer will improve the fluidity of polyborosiloxane during processing, thereby improving the spinnability of the blended material. At the same time, since the shear viscosity platform of polyborosiloxane is extremely wide and has a strong anti-shear thinning ability, the combination of the two improves the melt strength of the modified thermoplastic polyurethane elastomer and improves its spinnability.

[0023] The specific principle is as follows: at the spinning temperature, as the shear strength increases, the viscosity of polyborosiloxane remains basically stable, the polyborosiloxane is evenly dispersed in the thermoplastic polyurethane elastomer matrix, and the combination of the two is very stable, which largely overcomes the effect of shear thinning of the thermoplastic polyurethane elastomer on fiber forming during melt extrusion, improves the melt strength, greatly improves the formability of the thermoplastic polyurethane elastomer fiber, and avoids wire breakage during the winding process. DETAILED DESCRIPTION

[0024] A 9032 and GTZ 095 of Wanhua Chemical Company are used as thermoplastic polyurethane elastomer substrates, and the present invention is further described in detail in conjunction with specific embodiments.

[0025] Embodiment one:

[0026] The material improved by the present invention is prepared by the following raw materials in mass proportion:

[0027]

[0028] First, polyborosiloxane, γ-aminopropyl trimethoxysilane and dimethoxyethylene glycol phthalate were mixed at room temperature with a kneader for 0.5 hours; then the mixture was blended with A 9032 in an internal mixer at 180°C for 15 minutes, and then extruded into granules. The blended particles were then vacuum dried at 70°C, 90°C and 110°C for 1 hour, 1 hour and 1.5 hours respectively. Finally, the fibers were spun with a multifilament spinning machine, with a die head temperature of 213°C, a spinning speed of 500 m / min and a denier of 100D / 18F.

[0029] Embodiment 2:

[0030] The material improved by the present invention is prepared by the following raw materials in mass proportion:

[0031]

[0032] First, polyborosiloxane, γ-aminopropyl trimethoxysilane and triethylene glycol dipelargonate were mixed at room temperature with a kneader for 0.5 hours; then the mixture was blended with A 9032 in an internal mixer at 180°C for 15 minutes, and then extruded for granulation. The blended particles were then vacuum dried at 70°C, 90°C and 110°C for 1 hour, 1 hour and 1.5 hours respectively. Finally, the fibers were spun with a multifilament spinning machine at a die head temperature of 213°C, a spinning speed of 500 m / min and a denier of 100D / 18F.

[0033] Embodiment 3

[0034] The material improved by the present invention is prepared by the following raw materials in mass proportion:

[0035]

[0036] First, polyborosiloxane, γ-methacryloyloxy functional alkoxysilane and dimethoxyethylene glycol phthalate were mixed at room temperature with a kneader for 0.5 hours; then the mixture was blended with GTZ 095 in an internal mixer at 180°C for 15 minutes, and then extruded into granules. The blended particles were then vacuum dried at 70°C, 90°C and 110°C for 1 hour, 1 hour and 1.5 hours respectively. Finally, the multifilament spinning machine was used for spinning, with a die temperature of 213°C, a spinning speed of 500 m / min and a denier of 100D / 18F.

[0037] Embodiment 4

[0038] The material improved by the present invention is prepared by the following raw materials in mass proportion:

[0039]

[0040] First, polyborosiloxane, γ-methacryloyloxy functional alkoxysilane and triethylene glycol dipelargonate were mixed at room temperature with a kneader for 0.5 hours; then the mixture was blended with GTZ 095 in an internal mixer at 180°C for 15 minutes, and then extruded into granules. The blended particles were then vacuum dried at 70°C, 90°C and 110°C for 1 hour, 1 hour and 1.5 hours respectively. Finally, the fibers were spun with a multifilament spinning machine, with a die temperature of 213°C, a spinning speed of 500 m / min and a denier of 100D / 18F.

[0041] Comparative Example 1

[0042] The A9032 particles were vacuum dried at 70°C, 90°C and 110°C for 1 hour, 1 hour and 1.5 hours respectively using a vacuum drying drum, and finally spun using a multifilament spinning machine with a die temperature of 213°C, a spinning speed of 500 m / min and a denier of 100D / 18F.

[0043] Comparative Example 2

[0044] The GTZ 095 particles were vacuum dried at 70°C, 90°C and 110°C for 1 hour, 1 hour and 1.5 hours respectively. Finally, they were spun by a multifilament spinning machine with a die temperature of 213°C, a spinning speed of 500 m / min and a denier of 100D / 18F.

[0045] The spinning masterbatch of the above embodiment and comparative example was tested for melt shear viscosity at spinning temperature, and the average number of broken fibers after continuous spinning for 10,000 meters was recorded. The tensile properties and elastic recovery rate of the fiber were tested respectively using standards FZ / T50006-2013 and FZ / T50007-2012.

[0046] Table 1 Comparison of melt strength and average yarn breakage rate of 5000 meters between the embodiment and the comparative example

[0047]

[0048]

[0049] Table 2 Comparison of mechanical properties between the examples and the comparative examples

[0050] sample Tensile elongation at break (%) 300% fixed elongation rebound rate (%) Comparative Example 1 621 90% Comparative Example 2 615 91% Example 1 736 93% Example 2 753 94% Example 3 765 93% Example 4 784 95%

[0051] From the analysis of the above table, it can be seen that the melt shear viscosity of each modified example sample is increased by about 100% compared with the unmodified comparative example, which greatly improves the melt shear strength of the thermoplastic polyurethane elastomer and overcomes the effect of the shear thinning phenomenon on fiber forming during its melt spinning screw extrusion process; from the number of broken wires per 10,000 meters in the actual spinning process, the broken wire phenomenon of the modified example sample almost disappears, the fiber formability is good, and the spinning stability is greatly improved. From the data in Table 2, the elongation at break and the resilience of the modified fiber are improved to varying degrees compared with the unmodified comparative example, achieving the expected purpose.

[0052] The above data show that the technical solution of the present invention is stable and reliable, achieves the established purpose of the invention, and solves the technical problems that have always existed in the relevant fields.

[0053] The above description of the present invention is only a partial embodiment, but the present invention is not limited to the above embodiment. The above embodiment is illustrative and not restrictive. All specific extensions of the materials and methods of the present invention, without departing from the scope of protection of the present invention and the claims, are within the scope of protection of the present invention.

Claims

1. A method for preparing a modified thermoplastic polyurethane elastomer multifilament, characterized in that: Here are the steps: Step 1: Weigh a certain mass ratio of polyborosiloxane, a coupling agent, and a plasticizer, and stir and mix them evenly at a certain temperature; the molar ratio of silicon atoms to boron atoms in the polyborosiloxane is 15.1:1-5.3:1; the mass ratio of the coupling agent to the polyborosiloxane is 2:45-1:18; the mass ratio of the plasticizer to the polyborosiloxane is 1:18-1:15; Step 2: Take the mixture of step 1, melt blend it with thermoplastic polyurethane elastomer in a certain ratio, and granulate it; the ratio of polyborosiloxane to thermoplastic polyurethane elastomer is 1:10; Step 3: taking the modified thermoplastic polyurethane elastomer particles described in step 2 and vacuum drying them at a certain temperature for a certain period of time; Step 4: taking the dried thermoplastic polyurethane elastomer particles described in step 3 and performing melt spinning under certain process conditions to obtain modified thermoplastic polyurethane elastomer multifilaments.

2. The preparation method according to claim 1, characterized in that In step 4, the spinning speed is 400-750 m / min.