Polyurethane curing agent and its application

By using polyisocyanates and encapsulated thermally latent catalysts as polyurethane curing agents, the balance between crosslinking and storage stability of polyurethane resin coatings during post-coating drying was resolved, achieving excellent storage stability and low-temperature curing properties, and forming a coating film with good scratch resistance.

CN116323837BActive Publication Date: 2024-10-25ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202180064181.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-09-30
Filing Date
2021-09-03
Publication Date
2024-10-25
Estimated Expiration
2041-09-03

AI Technical Summary

Technical Problem

Existing polyurethane resin coatings have difficulty balancing crosslinking during drying and storage stability after application, resulting in insufficient storage stability.

Method used

A polyurethane-based curing agent containing polyisocyanate and encapsulated thermally latent catalyst is used. The encapsulated thermally latent catalyst is covered by a polyamine compound and a polyurea film derived from polyisocyanate to form a capped polyisocyanate. This is used to prepare two-component coating compositions, solvent-based one-component coating compositions, and water-based one-component coating compositions.

Benefits of technology

The coating composition exhibits excellent storage stability and low-temperature curing properties, resulting in a coating film with excellent scratch resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004133810970000241
    Figure BDA0004133810970000241
  • Figure BDA0004133810970000391
    Figure BDA0004133810970000391
  • Figure BDA0004133810970000611
    Figure BDA0004133810970000611
Patent Text Reader

Abstract

Provided are a polyurethane curing agent containing a first polyisocyanate and an encapsulated thermal latent catalyst, wherein the encapsulated thermal latent catalyst is covered with a polyurea film derived from a polyamine compound and a second polyisocyanate; a coating composition containing the polyurethane curing agent and a polyvalent active hydrogen compound; and a coating film formed by curing the coating composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polyurethane curing agent and its application. Specifically, the present invention relates to a polyurethane curing agent, an encapsulated thermal latent catalyst, a method for producing an encapsulated thermal latent catalyst, a kit for a two-component coating composition, a solvent-based one-component coating composition, a water-based one-component coating composition, a coating film, and a coated article.

[0002] This application claims priority based on Japanese Patent Application No. 2020-164749 filed in Japan on September 30, 2020, the contents of which are incorporated herein. Background Art

[0003] Conventionally, polyurethane resin coatings have very excellent abrasion resistance, chemical resistance, and stain resistance. In particular, polyurethane resin coatings using polyisocyanates obtained from aliphatic diisocyanates or alicyclic diisocyanates have even better weather resistance, and the demand for them tends to increase.

[0004] However, polyurethane resin coatings are generally two-component, and it is known that there is a trade-off between the crosslinking properties after coating and drying and the storage stability of the coating after compounding.

[0005] Therefore, generally, when the crosslinking property after coating and drying is excellent, the storage stability is poor, and on the other hand, when the storage stability is excellent, the crosslinking property after drying is poor.

[0006] As a technology for breaking the relationship between the crosslinking property after drying and the storage stability after the coating is mixed, for example, there can be cited a technology containing a thermolatent catalyst that is believed to change the structure of the organic metal complex by utilizing heat and exhibit catalytic activity (for example, see Patent Document 1, etc.); and a technology using a photolatent catalyst (for example, see Patent Document 2, etc.).

[0007] In addition, in polyurethane resin coatings, as a technology to improve the storage stability which is a disadvantage of the two-component type, a blocked polyisocyanate formed by blocking a polyisocyanate with a blocking agent is proposed. The blocked polyisocyanate does not react with a polyol at room temperature. However, the blocking agent is dissociated by heating, and the active isocyanate group is regenerated to react with the polyol to produce a cross-linking reaction, thereby improving the problem of storage stability. Therefore, a large number of blocking agents have been studied, and representative blocking agents include phenol, methyl ethyl ketoxime, 3,5-dimethylpyrazole, etc.

[0008] In addition, studies have been conducted to improve the catalytic activity of a blocked polyisocyanate composition by adding a metal catalyst to the composition compared to a case where no metal catalyst is added (see, for example, Patent Document 3).

[0009] Alternatively, a technology has been developed in which the drug contained in the substance is covered with an outer film such as gelatin to control the release of the drug contained in the substance (see, for example, Patent Document 4).

[0010] Prior art literature

[0011] Patent Literature

[0012] Patent Document 1: International Publication No. 2017 / 182429

[0013] Patent Document 2: Japanese Patent No. 5894919

[0014] Patent Document 3: Japanese Patent No. 6165152

[0015] Patent Document 4: Japanese Patent No. 6404826 Summary of the invention

[0016] Problem that the invention aims to solve

[0017] However, the system described in Patent Document 3 and the like, in which a metal catalyst is added to a blocked polyisocyanate composition, exhibits catalytic activity even in a coating, and therefore may have insufficient storage stability.

[0018] The present invention is proposed in view of the above circumstances, and provides a polyurethane curing agent that can obtain a coating composition with excellent storage stability and low-temperature curing properties, and can obtain a coating film with excellent scratch resistance. In addition, a two-component coating composition kit, a solvent-based one-component coating composition, a water-based one-component coating composition, a coating film, and a coated article using the above polyurethane curing agent are provided.

[0019] Solutions for solving problems

[0020] That is, the present invention includes the following aspects.

[0021] (1) A polyurethane curing agent comprising a polyisocyanate (first polyisocyanate) and an encapsulated thermal latent catalyst, wherein the encapsulated thermal latent catalyst is covered with a polyurea film derived from a polyamine compound and a polyisocyanate (second polyisocyanate).

[0022] (2) The polyurethane curing agent according to the above (1), which contains a polyisocyanate (first polyisocyanate) and an encapsulated thermal latent catalyst, wherein the encapsulated thermal latent catalyst comprises a metal compound covered with a polyurea film derived from a polyamine compound and a polyisocyanate (second polyisocyanate).

[0023] (3) The polyurethane curing agent according to (1) or (2), wherein the first polyisocyanate is a blocked polyisocyanate derived from a polyisocyanate and a blocking agent.

[0024] (4) The polyurethane curing agent according to (1) or (2), wherein the first polyisocyanate is a hydrophilic blocked polyisocyanate derived from a polyisocyanate, a hydrophilic compound, and a blocking agent.

[0025] (5) A two-component coating composition kit comprising the polyurethane curing agent described in (1) or (2) above and a polyvalent active hydrogen compound.

[0026] (6) A solvent-based one-component coating composition comprising the polyurethane curing agent described in (3) above and a polyvalent active hydrogen compound.

[0027] (7) A water-based one-component coating composition comprising the polyurethane curing agent described in (4) above and a polyvalent active hydrogen compound.

[0028] (8) A coating film obtained by curing a two-component coating composition comprising the polyurethane curing agent described in (1) or (2) above and a polyvalent active hydrogen compound.

[0029] (9) A coating film formed by curing the solvent-based one-component coating composition described in (6) above.

[0030] (10) A coating film formed by curing the water-based one-component coating composition described in (7) above.

[0031] (11) A coated article comprising the coating film according to any one of (8) to (10) above.

[0032] (12) An encapsulated thermal latent catalyst covered with a polyurea film derived from a polyamine compound and a polyisocyanate (a second polyisocyanate).

[0033] (13) The encapsulated thermal latent catalyst according to (12) above, comprising a metal compound covered with a polyurea film derived from a polyamine compound and a polyisocyanate (a second polyisocyanate).

[0034] (14) The encapsulated thermal latent catalyst according to (12) or (13), wherein the second polyisocyanate is a water-dispersible polyisocyanate.

[0035] (15) A method for preparing an encapsulated thermal latent catalyst, comprising:

[0036] A step of mixing a polyamine compound and a metal compound to prepare a mixture;

[0037] A step of dispersing the mixture in water to produce a dispersion; and

[0038] A step of adding a water-dispersible polyisocyanate dropwise to the dispersion to form a polyurea film derived from the polyamine compound and the water-dispersible polyisocyanate by an interfacial polymerization method, and covering the metal compound with the polyurea film.

[0039] Effects of the Invention

[0040] According to the polyurethane curing agent of the above embodiment, it is possible to provide a coating composition having excellent storage stability and low-temperature curability and a coating film having excellent scratch resistance. DETAILED DESCRIPTION

[0041] The following is a detailed description of the mode for implementing the present invention (hereinafter referred to as "this embodiment"). The following this embodiment is an example for illustrating the present invention, and the purpose is not to limit the present invention to the following content. The present invention can be implemented by appropriate deformation within the scope of its purpose.

[0042] In addition, in this specification, "polyol" refers to a compound having two or more hydroxyl groups (-OH).

[0043] In the present specification, "polyisocyanate" refers to a reaction product in which a plurality of monomer compounds having one or more isocyanate groups (-NCO) (hereinafter referred to as "isocyanate monomers") are bonded together.

[0044] 《Polyurethane curing agent》

[0045] The polyurethane curing agent of the present embodiment contains a polyisocyanate (first polyisocyanate) and an encapsulated thermal latent catalyst covered with a polyurea film derived from a polyamine compound and a polyisocyanate (second polyisocyanate).

[0046] The first polyisocyanate may be a blocked polyisocyanate derived from a polyisocyanate and a blocking agent, or may be a blocked polyisocyanate derived from a polyisocyanate, a hydrophilic compound, and a blocking agent.

[0047] The content ratio of the first polyisocyanate and the encapsulated thermal latent catalyst in the polyurethane curing agent at 100% by mass of each solid content (first polyisocyanate: encapsulated thermal latent catalyst) (mass ratio) is preferably 99:1 to 70:30, more preferably 98:2 to 75:25, and further preferably 96:4 to 80:20. By being within the above range, there is a tendency that the curing property during low temperature sintering is good and the coating film appearance remains smooth.

[0048] <Polyisocyanate (first polyisocyanate)>

[0049] The polyisocyanate (first polyisocyanate) of the present embodiment may be not only a polyisocyanate but also a blocked polyisocyanate derived from a polyisocyanate and a blocking agent, or a hydrophilic blocked polyisocyanate derived from a polyisocyanate, a hydrophilic compound and a blocking agent.

[0050] <Polyisocyanate>

[0051] The polyisocyanate of the present embodiment is a reaction product obtained by reacting a plurality of isocyanate monomers.

[0052] The isocyanate monomer is preferably an isocyanate monomer having a carbon number of 4 or more and 30 or less. Specifically, the isocyanate monomers described above include the following isocyanate monomers. These isocyanate monomers may be used alone or in combination of two or more.

[0053] (1) Aromatic diisocyanates such as diphenylmethane-4,4′-diisocyanate (hereinafter sometimes referred to as “MDI”), 1,5-naphthalene diisocyanate, toluene diisocyanate (hereinafter sometimes referred to as “TDI”), xylylene diisocyanate, and m-tetramethylxylylene diisocyanate (hereinafter sometimes referred to as “TMXDI”).

[0054] (2) Aliphatic diisocyanates such as 1,4-tetramethylene diisocyanate, 1,6-hexamethylene diisocyanate (hereinafter sometimes referred to as “HDI”), 2,2,4-trimethyl-1,6-diisocyanatohexane, 2,4,4-trimethyl-1,6-hexamethylene diisocyanate, 2-methylpentane-1,5-diisocyanate (hereinafter sometimes referred to as “MPDI”), and lysine diisocyanate (hereinafter sometimes referred to as “LDI”).

[0055] (3) Alicyclic diisocyanates such as isophorone diisocyanate (hereinafter sometimes referred to as “IPDI”), 1,3-bis(diisocyanate methyl)cyclohexane, 4,4′-dicyclohexylmethane diisocyanate, diisocyanate norbornane, and di(isocyanate methyl)norbornane.

[0056] (4) Triisocyanates such as 4-isocyanatemethyl-1,8-octamethylene diisocyanate (hereinafter sometimes referred to as "NTI"), 1,3,6-hexamethylene triisocyanate (hereinafter sometimes referred to as "HTI"), bis(2-isocyanatoethyl) 2-isocyanatoglutarate (hereinafter sometimes referred to as "GTI"), and lysine triisocyanate (hereinafter sometimes referred to as "LTI").

[0057] Among them, from the viewpoint of better weather resistance of the obtained coating film, as the aforementioned isocyanate monomer, it is preferably one or more diisocyanates selected from the group consisting of aliphatic diisocyanates and alicyclic diisocyanates. In addition, as the aforementioned isocyanate monomer, from the viewpoint of ease of industrial acquisition, HDI or IPDI is more preferably used.

[0058] As the aforementioned isocyanate monomer, any one of aliphatic diisocyanate and alicyclic diisocyanate can be used alone or in combination. Among them, it is preferred to use aliphatic diisocyanate alone or in combination with aliphatic diisocyanate, and it is more preferred to use HDI alone or in combination with HDI and IPDI. By using aliphatic diisocyanate and alicyclic diisocyanate in combination, the toughness and elasticity when forming a coating film can be further improved.

[0059] When an aliphatic diisocyanate and an alicyclic diisocyanate are used in combination among polyisocyanates, the mass ratio of the structural unit derived from the aliphatic diisocyanate to the structural unit derived from the alicyclic diisocyanate is preferably 50 / 50 or more and 95 / 5 or less, more preferably 60 / 40 or more and 90 / 10 or less, and further preferably 70 / 30 or more and 80 / 20 or less.

[0060] When the mass ratio of the structural unit derived from aliphatic diisocyanate to the structural unit derived from alicyclic diisocyanate is greater than the above lower limit, the decrease in flexibility when forming the coating film can be more effectively suppressed. On the other hand, when it is less than the above upper limit, the hardness when forming the coating film can be further improved.

[0061] The mass ratio of the structural unit derived from aliphatic diisocyanate to the structural unit derived from alicyclic diisocyanate can be calculated using the following method. First, the mass of the unreacted diisocyanate after the reaction and the aliphatic diisocyanate concentration and the alicyclic diisocyanate concentration in the unreacted diisocyanate obtained by gas chromatography are used to calculate the mass of the unreacted aliphatic diisocyanate and the mass of the unreacted alicyclic diisocyanate. Then, the mass of the unreacted aliphatic diisocyanate and the mass of the unreacted alicyclic diisocyanate calculated above are deducted from the mass of the aliphatic diisocyanate and the mass of the alicyclic diisocyanate respectively, and the obtained difference is used as the mass of the structural unit derived from aliphatic diisocyanate and the mass of the structural unit derived from alicyclic diisocyanate. Then, by dividing the mass of the structural unit derived from aliphatic diisocyanate by the mass of the structural unit derived from alicyclic diisocyanate, the mass ratio of the structural unit derived from aliphatic diisocyanate to the structural unit derived from alicyclic diisocyanate is obtained.

[0062] Specific examples of the polyisocyanate derived from the isocyanate monomer include the polyisocyanates shown in (1) to (8) below, but are not limited to these.

[0063] (1) A polyisocyanate compound having a uretdione structure obtained by cyclizing and dimerizing two isocyanate groups.

[0064] (2) A polyisocyanate compound having an isocyanurate structure and an iminooxadiazinedione structure obtained by cyclotrimerization of three isocyanate groups.

[0065] (3) A polyisocyanate compound having a biuret structure obtained by reacting three isocyanate groups with one water molecule.

[0066] (4) A polyisocyanate compound having an oxadiazinetrione structure obtained by reacting two isocyanate groups with one molecule of carbon dioxide.

[0067] (5) A polyisocyanate compound having a plurality of carbamate groups obtained by reacting one isocyanate group with one hydroxyl group.

[0068] (6) A polyisocyanate compound having an allophanate structure obtained by reacting two isocyanate groups with one hydroxyl group.

[0069] (7) A polyisocyanate compound having an acylurea group obtained by reacting one isocyanate group with one carboxyl group.

[0070] (8) A polyisocyanate compound having a urea structure obtained by reacting one isocyanate group with one primary or secondary amine.

[0071] That is, the polyisocyanate includes, in addition to the polyisocyanates derived from the above-mentioned isocyanate monomers, polyisocyanates which are reaction products obtained by reacting a plurality of isocyanate monomers with compounds other than the above-mentioned isocyanate monomers (for example, alcohol, water, amine, etc.).

[0072] [Method for producing polyisocyanate]

[0073] The method for producing polyisocyanate will be described in detail below.

[0074] For example, polyisocyanates can be obtained by performing allophanate reaction to form allophanate groups, uretdione reaction to form uretdione groups, iminooxadiazinedione reaction to form iminooxadiazinedione groups, isocyanurate reaction to form isocyanurate groups, carbamate reaction to form carbamate groups, and biuret reaction to form biuret groups at one time in the presence of excess isocyanate monomers, and removing unreacted isocyanate monomers after the reaction is completed. That is, the polyisocyanate obtained by the above reaction is a reaction product in which a plurality of the above isocyanate monomers are bonded and have one or more selected from the group consisting of an allophanate group, a uretdione group, an iminooxadiazinedione group, an isocyanurate group, a carbamate group, and a biuret group.

[0075] Alternatively, the above reactions may be performed separately and the polyisocyanates obtained respectively may be mixed at a specific ratio.

[0076] From the viewpoint of ease of production, it is preferred to conduct the above-mentioned reactions at once to obtain a polyisocyanate, and from the viewpoint of freely adjusting the molar ratio of each functional group, it is preferred to produce them separately and then mix them.

[0077] (1) Method for producing allophanate-containing polyisocyanate

[0078] The allophanate group-containing polyisocyanate is obtained by adding an alcohol to an isocyanate monomer and using an allophanation reaction catalyst.

[0079] The alcohol used in the formation of the allophanate group is preferably an alcohol composed only of carbon, hydrogen and oxygen.

[0080] Specific examples of the alcohol include, but are not limited to, monohydric alcohols and diols. These alcohols may be used alone or in combination of two or more.

[0081] Examples of the monohydric alcohol include methanol, ethanol, propanol, butanol, pentanol, hexanol, heptanol, octanol, and nonanol.

[0082] Examples of the diol include ethylene glycol, 1,3-butanediol, neopentyl glycol, and 2-ethylhexanediol.

[0083] Among them, the alcohol is preferably a monohydric alcohol, and more preferably a monohydric alcohol having a molecular weight of 200 or less.

[0084] Examples of the allophanation reaction catalyst include, but are not limited to, alkyl carboxylates of tin, lead, zinc, bismuth, zirconium, zirconyl, and the like.

[0085] Examples of the tin alkyl carboxylate (organotin compound) include 2-ethylhexanoate tin and dibutyltin dilaurate.

[0086] Examples of the lead alkyl carboxylate (organolead compound) include lead 2-ethylhexanoate and the like.

[0087] Examples of zinc alkyl carboxylates (organozinc compounds) include zinc 2-ethylhexanoate and the like.

[0088] Examples of bismuth alkyl carboxylates include bismuth 2-ethylhexanoate and the like.

[0089] Examples of zirconium alkyl carboxylates include zirconium 2-ethylhexanoate and the like.

[0090] Examples of zirconyl alkyl carboxylates include 2-ethylhexanoic acid zirconyl salt and the like.

[0091] These catalysts can be used alone or in combination of two or more.

[0092] In addition, the isocyanurate reaction catalyst described later can also be an allophanate reaction catalyst. When the allophanate reaction is carried out using the isocyanurate reaction catalyst described later, an isocyanurate type polyisocyanate is naturally produced.

[0093] Among them, it is preferred in terms of economical production to use an isocyanurate reaction catalyst described later as an allophanate reaction catalyst and to conduct both the allophanate reaction and the isocyanurate reaction.

[0094] The lower limit of the amount of the allophanation reaction catalyst used is preferably 10 mass ppm, more preferably 20 mass ppm, further preferably 40 mass ppm, particularly preferably 80 mass ppm, relative to the mass of the charged isocyanate monomer.

[0095] The upper limit of the amount of the allophanation reaction catalyst used is preferably 1000 mass ppm, more preferably 800 mass ppm, further preferably 600 mass ppm, particularly preferably 500 mass ppm, relative to the mass of the charged isocyanate monomer.

[0096] That is, relative to the mass of the isocyanate monomer introduced, the amount of the allophanate reaction catalyst used is preferably 10 mass ppm or more and 1000 mass ppm or less, more preferably 20 mass ppm or more and 800 mass ppm or less, further preferably 40 mass ppm or more and 600 mass ppm or less, and particularly preferably 80 mass ppm or more and 500 mass ppm or less.

[0097] Moreover, as a lower limit of the allophanation reaction temperature, 40 degreeC is preferable, 60 degreeC is more preferable, 80 degreeC is further preferable, and 100 degreeC is especially preferable.

[0098] Moreover, as an upper limit of the allophanation reaction temperature, 180 degreeC is preferable, 160 degreeC is more preferable, and 140 degreeC is further more preferable.

[0099] That is, the allophanation reaction temperature is preferably 40°C to 180°C, more preferably 60°C to 160°C, further preferably 80°C to 140°C, particularly preferably 100°C to 140°C.

[0100] When the allophanation reaction temperature is at least the above lower limit, the reaction rate can be further improved. When the allophanation reaction temperature is at most the above upper limit, there is a tendency that the coloration of the polyisocyanate can be more effectively suppressed.

[0101] (2) Method for producing uretdione group-containing polyisocyanate

[0102] In the case of deriving the polyisocyanate containing the polyisocyanate having a uretdione group from an isocyanate monomer, the polyisocyanate can be produced by polymerizing the isocyanate monomer using a uretdione reaction catalyst or by heat, for example.

[0103] The uretdione reaction catalyst is not particularly limited, and examples thereof include tertiary phosphines such as trialkylphosphines, tri(dialkylamino)phosphines, and cycloalkylphosphines, and Lewis acids.

[0104] Examples of the trialkylphosphine include tri-n-butylphosphine and tri-n-octylphosphine.

[0105] Examples of the tri(dialkylamino)phosphine include tri-(dimethylamino)phosphine and the like.

[0106] Examples of the cycloalkylphosphine include cyclohexyl-di-n-hexylphosphine and the like.

[0107] Examples of the Lewis acid include boron trifluoride and zinc chloride.

[0108] Most uretdione reaction catalysts can also promote isocyanurate reaction at the same time.

[0109] When a uretdione reaction catalyst is used, it is preferred to add a deactivator for the uretdione reaction catalyst such as phosphoric acid or methyl p-toluenesulfonate to stop the uretdione reaction when a desired yield is achieved.

[0110] In addition, when a polyisocyanate having a uretdione group is obtained by heating one or more diisocyanates selected from the group consisting of the above-mentioned aliphatic diisocyanates and the above-mentioned alicyclic diisocyanates without using a uretdione reaction catalyst, the heating temperature is preferably 120° C. or more, more preferably 150° C. or more and 170° C. or less. In addition, the heating time is preferably 1 hour or more and 4 hours or less.

[0111] (3) Method for producing polyisocyanate containing iminooxadiazinedione group

[0112] When deriving the iminooxadiazinedione group-containing polyisocyanate from an isocyanate monomer, an iminooxadiazinedione reaction catalyst is generally used.

[0113] Examples of the iminooxadiazinedionization catalyst include the iminooxadiazinedionization catalysts described in 1) or 2) below.

[0114] 1) (Poly)hydrogen fluoride represented by the general formula M[Fn] or the general formula M[Fn(HF)m].

[0115] In the above formula, m and n are integers satisfying the relationship of m / n> 0. M is an n-charged cation (mixture) or one or more radicals having a total valence of n.

[0116] 2) From the general formula R 1 -CR'2-C(O)O- or general formula R 2 =CR'-C(O)O- and a quaternary ammonium cation or a quaternary phosphonium cation.

[0117] In the above formula, R 1 and R 2 Each is independently a linear, branched or cyclic saturated or unsaturated perfluoroalkyl group having 1 to 30 carbon atoms. Each of the multiple R's is independently selected from the group consisting of a hydrogen atom and an alkyl or aryl group having 1 to 20 carbon atoms which may contain a heteroatom.

[0118] Specific examples of the compound 1) ((poly)hydrogen fluoride) include tetramethylammonium fluoride hydrate and tetraethylammonium fluoride.

[0119] Specific examples of the compound 2) include 3,3,3-trifluorocarboxylic acid, 4,4,4,3,3-pentafluorobutyric acid, 5,5,5,4,4,3,3-heptafluoropentanoic acid, and 3,3-difluoroprop-2-enoic acid.

[0120] Among them, as the iminooxadiazinedionization reaction catalyst, 1) is preferred from the viewpoint of availability, and 2) is preferred from the viewpoint of safety.

[0121] The lower limit of the amount of the iminooxadiazinedionization catalyst used is not particularly limited, but is preferably 5 ppm, more preferably 10 ppm, and even more preferably 20 ppm in terms of mass ratio relative to the mass of the charged isocyanate monomer from the viewpoint of reactivity.

[0122] The upper limit of the amount of the iminooxadiazinedionization catalyst used is preferably 5000 ppm, more preferably 2000 ppm, and even more preferably 500 ppm in terms of mass ratio relative to the mass of the charged isocyanate monomer, from the viewpoint of suppressing coloration and discoloration of the product and controlling the reaction.

[0123] That is, the amount of the iminooxadiazinedionization catalyst used is preferably 5 ppm to 5000 ppm, more preferably 10 ppm to 2000 ppm, and further preferably 20 ppm to 500 ppm, in terms of mass ratio, relative to the mass of the charged isocyanate monomer.

[0124] The lower limit of the reaction temperature for iminooxadiazinedionization is not particularly limited, but is preferably 40°C, more preferably 50°C, and even more preferably 60°C from the viewpoint of reaction rate.

[0125] The upper limit of the reaction temperature for iminooxadiazinedionization is preferably 150°C, more preferably 120°C, and further preferably 110°C, from the viewpoint of suppressing coloration and discoloration of the product.

[0126] That is, the reaction temperature of the iminooxadiazinedionization is preferably 40°C to 150°C, more preferably 50°C to 120°C, and further preferably 60°C to 110°C.

[0127] When the imino-oxadiazinedionization reaction reaches the desired imino-oxadiazinedione content, the imino-oxadiazinedionization reaction can be stopped. The imino-oxadiazinedionization reaction can be stopped, for example, by adding an acidic compound to the reaction solution. Examples of the acidic compound include phosphoric acid, acidic phosphates, sulfuric acid, hydrochloric acid, and sulfonic acid compounds. Thus, the imino-oxadiazinedionization catalyst is neutralized or deactivated by thermal decomposition or chemical decomposition. After the reaction is stopped, filtration is performed as required.

[0128] (4) Method for producing isocyanurate group-containing polyisocyanate

[0129] Examples of the catalyst for deriving the isocyanurate group-containing polyisocyanate from the isocyanate monomer include commonly used isocyanurate formation reaction catalysts.

[0130] The isocyanurate reaction catalyst is not particularly limited, but is generally preferably an isocyanurate reaction catalyst having alkalinity. Specific examples of the isocyanurate reaction catalyst include the following.

[0131] (1) Hydroxides of tetraalkylammonium such as tetramethylammonium, tetraethylammonium, and tetrabutylammonium, and organic weak acid salts such as acetates, propionates, octanoates, decanoates, myristates, and benzoates of the aforementioned tetraalkylammonium.

[0132] (2) Hydroxides of aryltrialkylammonium such as benzyltrimethylammonium and trimethylphenylammonium, and organic weak acid salts such as acetates, propionates, octanoates, decanoates, myristates and benzoates of the above aryltrialkylammonium.

[0133] (3) Hydroxides of hydroxyalkylammonium such as trimethylhydroxyethylammonium, trimethylhydroxypropylammonium, triethylhydroxyethylammonium, triethylhydroxypropylammonium, and the like; and organic weak acid salts such as acetates, propionates, caprylates, caprates, myristates, benzoates, and the like of the above hydroxyalkylammonium.

[0134] (4) Metal salts of tin, zinc, lead, etc. of alkyl carboxylic acids such as acetic acid, propionic acid, caproic acid, caprylic acid, capric acid, and myristic acid.

[0135] (5) Metal alkoxides of sodium, potassium, etc.

[0136] (6) Aminosilyl group-containing compounds such as hexamethylenedisilazane.

[0137] (7) Mannich bases.

[0138] (8) A mixture of tertiary amines and epoxy compounds.

[0139] (9) Phosphorus compounds such as tributylphosphine.

[0140] Among them, from the viewpoint of being less likely to generate unnecessary by-products, the isocyanurate reaction catalyst is preferably a hydroxide or an organic weak acid salt of quaternary ammonium, and more preferably a hydroxide of tetraalkylammonium, an organic weak acid salt of tetraalkylammonium, a hydroxide of aryltrialkylammonium, or an organic weak acid salt of aryltrialkylammonium.

[0141] The upper limit of the amount of the isocyanuration reaction catalyst used is preferably 1000 mass ppm, more preferably 500 mass ppm, and further preferably 100 mass ppm, relative to the mass of the charged isocyanate monomer.

[0142] On the other hand, the lower limit of the amount of the isocyanuration reaction catalyst used is not particularly limited, and may be, for example, 10 mass ppm.

[0143] The isocyanuration reaction temperature is preferably 50° C. to 120° C., more preferably 60° C. to 90° C. When the isocyanuration reaction temperature is below the upper limit, coloration of the polyisocyanate tends to be more effectively suppressed.

[0144] When a desired conversion rate (ratio of the mass of polyisocyanate produced by isocyanuration reaction to the mass of isocyanate monomer fed) is reached, the isocyanuration reaction is stopped by adding an acidic compound (eg, phosphoric acid, acidic phosphate, etc.).

[0145] It should be noted that in order to obtain polyisocyanates, the reaction needs to be stopped at the initial stage. However, since the reaction rate of the isocyanurate reaction is very fast at the initial stage, it is difficult to stop the reaction at the initial stage, and the reaction conditions, especially the amount and method of adding the catalyst, need to be carefully selected. For example, a method of adding the catalyst at a certain time is recommended as a preferred method.

[0146] Therefore, the conversion rate of the isocyanuration reaction for obtaining the polyisocyanate is preferably 10% by mass or more and 60% by mass or less, more preferably 15% by mass or more and 55% by mass or less, and further preferably 20% by mass or more and 50% by mass or less.

[0147] When the conversion rate of the isocyanurate reaction is below the upper limit, the blocked polyisocyanate composition containing the polyisocyanate can be made to have a lower viscosity. In addition, when the conversion rate of the isocyanurate reaction is above the lower limit, the reaction termination operation can be performed more easily.

[0148] When deriving an isocyanurate group-containing polyisocyanate, in addition to the above-mentioned isocyanate monomer, an alcohol having a valence of more than one valence and less than six valence may be used.

[0149] As the alcohol having a valence of 1 or more and 6 or less that can be used, for example, non-polymeric alcohol and polymeric alcohol can be mentioned.

[0150] Examples of the non-polymerizable alcohol include polyols such as monools, diols, triols, and tetraols.

[0151] Examples of the monohydric alcohols include methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, sec-butanol, n-pentanol, n-hexanol, n-octanol, n-nonanol, 2-ethylbutanol, 2,2-dimethylhexanol, 2-ethylhexanol, cyclohexanol, methylcyclohexanol, and ethylcyclohexanol.

[0152] Examples of the glycols include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, 2,3-butylene glycol, 2-methyl-1,2-propylene glycol, 1,5-pentanediol, 2-methyl-2,3-butylene glycol, 1,6-hexanediol, 1,2-hexanediol, 2,5-hexanediol, 2-methyl-2,4-pentanediol, 2,3-dimethyl-2,3-butylene glycol, 2-ethyl-hexanediol, 1,2-octanediol, 1,2-decanediol, 2,2,4-trimethylpentanediol, 2-butyl-2-ethyl-1,3-propylene glycol, and 2,2-diethyl-1,3-propylene glycol.

[0153] Examples of the triols include glycerin and trimethylolpropane.

[0154] Examples of the tetraols include pentaerythritol and the like.

[0155] The polymerizable alcohol is not particularly limited, but for example, the average number of hydroxyl groups in the polymerizable alcohol is preferably 3 to 8, more preferably 3 to 6, further preferably 3 to 5, and particularly preferably 3 or 4.

[0156] Specific examples of the polymerizable alcohol include polyester polyols, polyether polyols, acrylic polyols, and polyolefin polyols.

[0157] The polyester polyol can be obtained, for example, by subjecting a dibasic acid alone or in a mixture of two or more thereof to a condensation reaction with a polyol alone or in a mixture of two or more thereof.

[0158] Examples of the dibasic acid include carboxylic acids such as succinic acid, adipic acid, dimer acid, maleic anhydride, phthalic anhydride, isophthalic acid, terephthalic acid, and 1,4-cyclohexanedicarboxylic acid.

[0159] Examples of the polyol include ethylene glycol, propylene glycol, diethylene glycol, 1,4-butanediol, neopentyl glycol, 1,6-hexanediol, trimethylpentanediol, cyclohexanediol, trimethylolpropane, glycerin, pentaerythritol, 2-methylolpropanediol, and ethoxylated trimethylolpropane.

[0160] As a specific method for producing polyester polyol, for example, the above components are mixed and heated at about 160° C. to 220° C. to perform a condensation reaction. In addition, polycaprolactones obtained by ring-opening polymerization of lactones such as ε-caprolactone using a polyol can also be used as polyester polyol.

[0161] From the viewpoint of weather resistance and yellowing resistance of the obtained coating film, the polyester polyol obtained by the above-mentioned production method is preferably modified with an aliphatic diisocyanate, an alicyclic diisocyanate, or a compound obtained therefrom.

[0162] The polyether polyol can be obtained, for example, by any one of the following methods (1) to (3).

[0163] (1) A method of obtaining polyether polyols by randomly or block-adding an alkylene oxide alone or in mixture to a polyvalent hydroxy compound alone or in mixture using a catalyst.

[0164] Examples of the catalyst include hydroxides of lithium, sodium, potassium, etc., strong alkaline catalysts, and composite metal cyanide complexes. Examples of the strong alkaline catalyst include alkoxides and alkylamines, and examples of the composite metal cyanide complex include metalloporphyrins and zinc hexacyanocobaltate complexes.

[0165] Examples of the alkylene oxide include ethylene oxide, propylene oxide, butylene oxide, cyclohexene oxide, and styrene oxide.

[0166] Examples of the polyvalent hydroxy compound include the polyvalent hydroxy compounds shown in the following (i) to (vi).

[0167] (i) Diglycerol, di(trimethylolpropane), pentaerythritol, dipentaerythritol, etc.

[0168] (ii) Sugar alcohol compounds such as erythritol, D-threitol, L-arabitol, ribitol, xylitol, sorbitol, mannitol, dulcitol, and rhamnitol.

[0169] (iii) Monosaccharides such as arabinose, ribose, xylose, glucose, mannose, galactose, fructose, sorbitol, rhamnose, fucose and deoxyribose.

[0170] (iv) Disaccharides such as trehalose, sucrose, maltose, cellobiose, gentiobiose, lactose and melibiose.

[0171] (v) trisaccharides such as raffinose, gentiotriose and melezitose.

[0172] (vi) Tetrasaccharides such as stachyose.

[0173] (2) A method of obtaining polyether polyols by reacting a polyamine compound with an alkylene oxide.

[0174] Examples of the polyamine compound include ethylenediamines and the like.

[0175] Examples of the alkylene oxide include the same ones as exemplified in (1).

[0176] (3) A method of obtaining so-called polymer polyols by using the polyether polyols obtained in (1) or (2) as a medium and polymerizing acrylamide or the like.

[0177] The acrylic polyols are not particularly limited, and examples thereof include acrylic polyols obtained by copolymerizing an ethylenically unsaturated bond-containing monomer having a hydroxyl group, alone or in mixture, and other ethylenically unsaturated bond-containing monomers copolymerizable therewith, alone or in mixture.

[0178] The ethylenically unsaturated bond-containing monomer having a hydroxyl group is not particularly limited, and examples thereof include hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxybutyl acrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, and hydroxybutyl methacrylate.

[0179] The other ethylenically unsaturated bond-containing monomer copolymerizable with the ethylenically unsaturated bond-containing monomer having a hydroxyl group is not particularly limited, and examples thereof include acrylic acid esters, methacrylic acid esters, unsaturated carboxylic acids, unsaturated amides, vinyl monomers, and vinyl monomers having a hydrolyzable silyl group.

[0180] Examples of the acrylic acid ester include methyl acrylate, ethyl acrylate, propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, n-hexyl acrylate, cyclohexyl acrylate, 2-ethylhexyl acrylate, lauryl acrylate, benzyl acrylate, and phenyl acrylate.

[0181] Examples of the methacrylate include methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-hexyl methacrylate, cyclohexyl methacrylate, 2-ethylhexyl methacrylate, lauryl methacrylate, benzyl methacrylate, and phenyl methacrylate.

[0182] Examples of the unsaturated carboxylic acid include acrylic acid, methacrylic acid, maleic acid, and itaconic acid.

[0183] Examples of the unsaturated amide include acrylamide, methacrylamide, N,N-methylenebisacrylamide, diacetone acrylamide, diacetone methacrylamide, maleamide, and maleimide.

[0184] Examples of the vinyl monomer include glycidyl methacrylate, styrene, vinyltoluene, vinyl acetate, acrylonitrile, and dibutyl fumarate.

[0185] Examples of the vinyl monomer having a hydrolyzable silyl group include vinyltrimethoxysilane, vinylmethyldimethoxysilane, and γ-(meth)acryloxypropyltrimethoxysilane.

[0186] Examples of the polyolefin polyols include terminal hydroxylated polybutadiene and hydrogenated products thereof.

[0187] Among them, as the polymerizable alcohol, polyester polyol is preferred, and polycaprolactone polyol obtained by ring-opening polymerization of ε-caprolactone using a low molecular weight polyol is more preferred.

[0188] (5) Method for producing polyisocyanate containing carbamate group

[0189] When the polyisocyanate containing a urethane group is derived from an isocyanate monomer, it can be produced by, for example, mixing an excess amount of an isocyanate monomer and an alcohol and, if necessary, adding a urethanization reaction catalyst.

[0190] Examples of the alcohol include the same alcohols as exemplified in the above-mentioned “method for producing an isocyanurate group-containing polyisocyanate”.

[0191] The urethanization reaction catalyst is not particularly limited, and examples thereof include tin compounds, zinc compounds, and amine compounds.

[0192] The urethanization reaction temperature is preferably 50°C or higher and 160°C or lower, and more preferably 60°C or higher and 120°C or lower.

[0193] When the urethanization reaction temperature is at most the above upper limit, coloration of the polyisocyanate tends to be more effectively suppressed.

[0194] The urethanization reaction time is preferably 30 minutes to 4 hours, more preferably 1 hour to 3 hours, and even more preferably 1 hour to 2 hours.

[0195] The ratio of the molar amount of the isocyanate group of isocyanate monomer to the molar amount of the hydroxyl group of alcohol is preferably more than 2 / 1 and less than 50 / 1.Being more than the above-mentioned lower limit by this molar ratio, polyisocyanates can be formed with lower viscosity.Being below the above-mentioned upper limit by this molar ratio, the yield of polyisocyanates containing carbamate groups is further improved.

[0196] (6) Method for producing biuret group-containing polyisocyanate

[0197] The biuret-forming agent for deriving the biuret group-containing polyisocyanate from the isocyanate monomer is not particularly limited, and examples thereof include water, monovalent tertiary alcohols, formic acid, organic primary monoamines, and organic primary diamines.

[0198] The amount of isocyanate groups is preferably 6 or more, more preferably 10 or more, and further preferably 10 or more and 80 or less, relative to 1 mol of the biuretizing agent. If the molar amount of isocyanate groups relative to 1 mol of the biuretizing agent is above the lower limit, the polyisocyanate will sufficiently have a low viscosity, and if it is below the upper limit, the curability will be further improved when forming a coating composition.

[0199] In addition, a solvent may be used during the biuret reaction. The solvent may be any solvent as long as it dissolves the isocyanate monomer and the biuret-forming agent such as water and forms a uniform phase under the reaction conditions.

[0200] Specific examples of the solvent include ethylene glycol-based solvents and phosphoric acid-based solvents.

[0201] Examples of the ethylene glycol solvent include ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol mono-n-propyl ether acetate, ethylene glycol monoisopropyl ether acetate, ethylene glycol mono-n-butyl ether acetate, ethylene glycol diacetate, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol di-n-propyl ether, ethylene glycol diisopropyl ether, ethylene glycol di-n-butyl ether, ethylene glycol methyl ethyl ether, ethylene glycol methyl isopropyl ether, ethylene glycol methyl-n-butyl ether, ethylene glycol ethyl-n-propyl ether, ethylene glycol ethyl isopropyl ether, ethylene glycol ethyl-n-butyl ether, ethylene glycol-n-propyl-n-butyl ether, ethylene glycol isopropyl-n-butyl ether, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol mono-n-propyl ether acetate, diethylene glycol monoisopropyl ether acetate, diethylene glycol mono-n-butyl ether acetate, diethylene glycol diacetate, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol di-n-propyl ether, diethylene glycol diisopropyl ether, diethylene glycol di-n-butyl ether, diethylene glycol methyl ethyl ether, diethylene glycol methyl isopropyl ether, diethylene glycol methyl-n-propyl ether, diethylene glycol methyl-n-butyl ether, diethylene glycol ethyl isopropyl ether, diethylene glycol ethyl-n-propyl ether, diethylene glycol ethyl-n-butyl ether, diethylene glycol-n-propyl-n-butyl ether, diethylene glycol isopropyl-n-butyl ether, and the like.

[0202] Examples of the phosphoric acid-based solvent include trimethyl phosphate, triethyl phosphate, tripropyl phosphate, and tributyl phosphate.

[0203] These solvents can be used alone or in combination of two or more.

[0204] Among them, the ethylene glycol-based solvent is preferably ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol diacetate or diethylene glycol dimethyl ether.

[0205] In addition, as the phosphoric acid-based solvent, trimethyl phosphate or triethyl phosphate is preferred.

[0206] The biuret reaction temperature is preferably 70° C. to 200° C., more preferably 90° C. to 180° C. When the temperature is equal to or lower than the upper limit, coloration of the polyisocyanate tends to be more effectively prevented.

[0207] The allophanation reaction, uretdione reaction, iminooxadiazinedionation reaction, isocyanuration reaction, urethanation reaction, and biuretation reaction described above may be carried out in sequence, or several of them may be carried out simultaneously.

[0208] When a polyisocyanate derived from an isocyanate monomer and a polymerizable alcohol is produced, the polyisocyanate is obtained, for example, by reacting an isocyanate group of the isocyanate monomer with a hydroxyl group of a polymerizable alcohol (preferably a polyol).

[0209] The molar ratio (NCO / OH) of the isocyanate group of the diisocyanate to the hydroxyl group of the polyol is preferably 3 / 1 or more and 30 / 1 or less, more preferably 10 / 1 or more and 20 / 1 or less. When NCO / OH is above the lower limit, the excessive increase in viscosity of the obtained polyisocyanate composition can be effectively suppressed. On the other hand, when NCO / OH is below the upper limit, the reduction in productivity of the obtained polyisocyanate composition can be effectively suppressed.

[0210] The reaction temperature is preferably 50° C. to 200° C., more preferably 50° C. to 150° C. When the reaction temperature is at least the above lower limit, the reaction proceeds more efficiently, while when the reaction temperature is at most the above upper limit, undesirable side reactions such as coloration of the obtained polyisocyanate composition can be more effectively suppressed.

[0211] The reaction time is preferably in the range of 0.5 hours to 5 hours.

[0212] After or during the reaction of the isocyanate group of the diisocyanate and the hydroxyl group of the polyol, at least one reaction selected from the group consisting of the above-mentioned allophanate reaction, uretdione reaction, iminooxadiazinedione reaction, isocyanurate reaction, carbamate reaction, and biuret reaction can be performed, wherein the isocyanurate reaction is preferably performed. By performing the isocyanurate reaction, the hardness when forming the coating film can be further improved.

[0213] The polyisocyanate can be obtained by removing the unreacted isocyanate monomer from the reaction solution after the above-mentioned various reactions by thin film distillation, extraction or the like.

[0214] [Physical properties of polyisocyanates]

[0215] The average number of functional groups of the polyisocyanate (preferably a water-dispersible polyisocyanate) is preferably 2.5 or more and 4.0 or less, more preferably 2.8 or more and 3.8 or less, and further preferably 3.0 or more and 3.5 or less. When the average number of functional groups is equal to or greater than the above lower limit, the strength of the obtained urea film can be more fully maintained, while when it is equal to or less than the above upper limit, the metal compound contained in the encapsulated thermal latent catalyst of the present embodiment can further exhibit catalytic activity when heated.

[0216] The average number of functional groups is the number of isocyanate functional groups statistically possessed by one polyisocyanate molecule, and can be calculated from the number average molecular weight (Mn) and isocyanate group content (NCO%) of the polyisocyanate using the following formula.

[0217] (Average number of functional groups) = Mn × NCO% / 4200

[0218] <(Hydrophilic) Blocked Polyisocyanate>

[0219] The first polyisocyanate of the polyurethane-based curing agent of the present embodiment may be a blocked polyisocyanate derived from a polyisocyanate and a blocking agent.

[0220] Alternatively, in other embodiments, the first polyisocyanate may be a hydrophilic blocked polyisocyanate derived from a polyisocyanate, a hydrophilic compound, and a blocking agent.

[0221] The polyurethane curing agent of the present embodiment contains an encapsulated thermal latent catalyst in the first polyisocyanate, so that a coating composition having excellent storage stability and low-temperature curability can be obtained, and a coating film having excellent scratch resistance can be obtained.

[0222] <Blocked polyisocyanate>

[0223] The blocked polyisocyanate is derived from a polyisocyanate and a blocking agent. That is, the blocked polyisocyanate is a reaction product of a polyisocyanate and a blocking agent, and at least a part (preferably all) of the isocyanate groups of the polyisocyanate are blocked by the blocking agent.

[0224] Alternatively, the blocked polyisocyanate is derived from a polyisocyanate, a hydrophilic compound and a blocking agent. That is, the blocked polyisocyanate is a reaction product of a polyisocyanate, a hydrophilic compound and a blocking agent. A portion of the isocyanate groups of the polyisocyanate are blocked by the blocking agent, and a portion of the isocyanate groups of the polyisocyanate form a bond with the functional group of the hydrophilic compound to introduce a hydrophilic group.

[0225] Examples of the polyisocyanate serving as a raw material of the blocked polyisocyanate and a method for producing the same include the same examples as those exemplified in the above-mentioned "polyisocyanate".

[0226] The blocking agent used as a raw material of the blocked polyisocyanate is described below.

[0227] [Capping agent]

[0228] The end-capping agent is not particularly limited, and examples thereof include (1) alcohol compounds, (2) alkylphenol compounds, (3) phenol compounds, (4) active methylene compounds, (5) thiol compounds, (6) acid amide compounds, (7) acid imide compounds, (8) imidazole compounds, (9) urea compounds, (10) oxime compounds, (11) amine compounds, (12) imine compounds, (13) hydrogen sulfite compounds, (14) pyrazole compounds, (15) pyridine compounds, (16) guanidine compounds, (17) imidazoline compounds, (18) pyrimidine compounds, (19) triazole compounds, and (20) tetrazole compounds. More specifically, the end-capping agent includes the following end-capping agents.

[0229] (1) Alcohol compounds: methanol, ethanol, 2-propanol, n-butanol, sec-butanol, 2-ethyl-1-hexanol, 2-methoxyethanol, 2-ethoxyethanol, 2-butoxyethanol and the like.

[0230] (2) Alkylphenol compounds: mono- and di-alkylphenols having an alkyl group having 4 or more carbon atoms as a substituent. Specific examples of the alkylphenol compounds include mono-alkylphenols such as n-propylphenol, iso-propylphenol, n-butylphenol, sec-butylphenol, tert-butylphenol, n-hexylphenol, 2-ethylhexylphenol, n-octylphenol, and n-nonylphenol; and di-alkylphenols such as di-n-propylphenol, diisopropylphenol, isopropylcresol, di-n-butylphenol, di-tert-butylphenol, di-sec-butylphenol, di-n-octylphenol, di-2-ethylhexylphenol, and di-n-nonylphenol.

[0231] (3) Phenol compounds: phenol, cresol, ethylphenol, styrenated phenol, hydroxybenzoic acid esters, etc.

[0232] (4) Active methylene compounds.

[0233] (5) Mercaptan compounds: butyl mercaptan, dodecyl mercaptan, etc.

[0234] (6) Acid amide compounds: acetanilide, acetic acid amide, ε-caprolactam, δ-pentyl propionamide, γ-butyrolactam, etc.

[0235] (7) Acid imide compounds: succinimide, maleic imide, etc.

[0236] (8) Imidazole compounds: imidazole, 2-methylimidazole, 2-ethylimidazole, 4-methylimidazole, benzimidazole, etc.

[0237] (9) Urea compounds: urea, thiourea, ethylene urea, etc.

[0238] (10) Oxime compounds: formaldehyde oxime, acetaldehyde oxime, acetone oxime, methyl ethyl ketone oxime, cyclohexanone oxime, etc.

[0239] (11) Amine compounds: diphenylamine, aniline, carbazole, di-n-propylamine, diisopropylamine, isopropylethylamine, etc.

[0240] (12) Imine compounds: ethyleneimine, polyethyleneimine, etc.

[0241] (13) Bisulfite compounds: sodium bisulfite, etc.

[0242] (14) Pyrazole compounds: pyrazole, 3-methylpyrazole, 3,5-dimethylpyrazole, etc.

[0243] (15) Pyridine compounds: 2-(methylamino)pyridine, 4-hydroxypyridine, 2-hydroxypyridine, etc.

[0244] (16) Guanidine compounds: 3,3-dimethylguanidine, 1,1,3,3-tetramethylguanidine, etc.

[0245] (17) Imidazolinium compounds: 2-methylimidazoline, 2-phenylimidazoline, etc.

[0246] (18) Pyrimidine compounds: 2-methyl-1,4,5,6-tetrahydropyrimidine, etc.

[0247] (19) Triazole compounds: 1,2,4-triazole, 1,2,3-triazole, 3,5-dimethyl-1,2,4-triazole, etc.

[0248] (20) Tetrazolyl compounds: 1H-1,2,3,4-tetrazolyl, etc.

[0249] Among them, the end-capping agent is preferably at least one compound selected from the group consisting of oxime compounds, amine compounds, pyrazole compounds, imidazole compounds, active methylene compounds, and triazole compounds, more preferably pyrazole compounds, active methylene compounds, or triazole compounds, and further preferably triazole compounds. In addition, in order to improve the compatibility with polyvalent active hydrogen compounds, it is particularly preferred to combine triazole compounds with other end-capping agents, such as active methylene compounds.

[0250] Among the triazole compounds, 1,2,4-triazole, 1,2,3-triazole, or 3,5-dimethyl-1,2,4-triazole is preferred.

[0251] Among the pyrazole compounds, 3,5-dimethylpyrazole is preferred.

[0252] Examples of active methylene compounds include dimethyl malonate, diethyl malonate, methyl acetoacetate, ethyl acetoacetate, acetylacetone, and compounds represented by the following general formula (IV) (hereinafter sometimes referred to as "compound (IV)"). Among them, compound (IV) is preferred.

[0253]

[0254] In the general formula (IV), R 41 is a hydroxyl group; an alkyl group which may contain one or more substituents selected from the group consisting of a hydroxyl group and an amino group; an amino group which may contain one or more substituents selected from the group consisting of a hydroxyl group and an alkyl group; an aryl group which may contain one or more substituents selected from the group consisting of a hydroxyl group and an amino group; or an alkoxy group which may contain one or more substituents selected from the group consisting of a hydroxyl group and an amino group. For the aforementioned amino group, two of the aforementioned substituents may be linked to each other to form a ring.

[0255] R 42 , R 43 and R 44 Each independently represents a hydrogen atom; a hydroxyl group; an alkyl group which may contain one or more substituents selected from the group consisting of a hydroxyl group and an amino group; an amino group which may contain one or more substituents selected from the group consisting of a hydroxyl group and an alkyl group; an aryl group which may contain one or more substituents selected from the group consisting of a hydroxyl group and an amino group; or an alkoxy group which may contain one or more substituents selected from the group consisting of a hydroxyl group and an amino group. For the aforementioned amino group, two aforementioned substituents may be connected to each other to form a ring. Among them, R 42 , R 43 and R 44 At least two of them are not hydrogen atoms.

[0256] 1. Compound (IV)

[0257] (1)R 41

[0258] (1-1)R 41 :alkyl

[0259] R 41In the case of an alkyl group having no substituent, the alkyl group preferably has a carbon number of 1 to 30, more preferably 1 to 8, further preferably 1 to 6, and particularly preferably 1 to 4. Specific examples of the alkyl group having no substituent include a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, a tert-butyl group, a sec-butyl group, an isobutyl group, an n-pentyl group, an isopentyl group, a neopentyl group, a tert-pentyl group, a 1-methylbutyl group, an n-hexyl group, a 2-methylpentyl group, a 3-methylpentyl group, a 2,2-dimethylbutyl group, a 2,3-dimethylbutyl group, an n-heptyl group, a 2-methylhexyl group, a 3-methylhexyl group, a 2,2-dimethylpentyl group, a 2,3-dimethylpentyl group, a 2,4-dimethylpentyl group, a 3,3-dimethylpentyl group, a 3-ethylpentyl group, a 2,2,3-trimethylbutyl group, an n-octyl group, an isooctyl group, a 2-ethylhexyl group, a nonyl group, and a decyl group.

[0260] In addition, R 41 In the case of an alkyl group having a substituent, the substituent is a hydroxyl group or an amino group.

[0261] Examples of the alkyl group having a hydroxyl group as a substituent include a hydroxymethyl group, a hydroxyethyl group, and a hydroxypropyl group.

[0262] Examples of the alkyl group having an amino group as a substituent include an aminomethyl group, an aminoethyl group, an aminopropyl group, and an aminobutyl group.

[0263] Examples of the alkyl group having a hydroxyl group and an amino group as substituents include a hydroxyaminomethyl group, a hydroxyaminoethyl group, and a hydroxyaminopropyl group.

[0264] (1-2)R 41 :Amino

[0265] R 41 In the case of an amino group having a substituent, the substituent is a hydroxyl group or an alkyl group.

[0266] Examples of the amino group having a hydroxy group as a substituent include a hydroxyamino group (—NH—OH).

[0267] Examples of the amino group having an alkyl group as a substituent include methylamino, ethylamino, n-butylamino, dimethylamino, diethylamino, dipropylamino, diisopropylamino, di-n-butylamino, di-tert-butylamino, di-sec-butylamino, diisobutylamino, and 2,6-dimethylpiperidinyl.

[0268] Examples of the amino group having a hydroxyl group and an alkyl group as substituents include a hydroxymethyleneamino group, a hydroxyethyleneamino group, a hydroxypropyleneamino group, and a hydroxybutyleneamino group.

[0269] Examples of the amino group in which two substituents are linked to each other to form a ring include ethyleneimino, azetidinyl, pyrrolidinyl, piperidinyl, 2,6-dimethylpiperidinyl, and hexamethyleneimino.

[0270] (1-3)R 41 : Aryl

[0271] R 41 In the case of an aryl group having no substituent, the aryl group preferably has a carbon number of 5 to 30, more preferably 6 to 20, and even more preferably 6 to 14. Specific examples of the aryl group include a monocyclic aromatic hydrocarbon group, a bicyclic aromatic hydrocarbon group, a tricyclic aromatic hydrocarbon group, a tetracyclic aromatic hydrocarbon group, a pentacyclic aromatic hydrocarbon group, a hexacyclic aromatic hydrocarbon group, and a heptacyclic aromatic hydrocarbon group.

[0272] Examples of the monocyclic aromatic hydrocarbon group include a phenyl group, a benzyl group, a tolyl group, and an o-xylyl group.

[0273] Examples of the bicyclic aromatic hydrocarbon group include indanyl, indenyl, pentalenyl, azulenyl, naphthyl, and tetrahydronaphthyl.

[0274] Examples of the tricyclic aromatic hydrocarbon group include anthracenyl, fluorenyl, phenalenyl, and phenanthrenyl.

[0275] Examples of the tetracyclic aromatic hydrocarbon group include pyrenyl, naphthacetyl, Ji et al.

[0276] Examples of the pentacyclic aromatic hydrocarbon group include a perylenyl group, a perylene group, and a fused pentaphenyl group.

[0277] Examples of the hexacyclic aromatic hydrocarbon group include naphthopyrenyl and the like.

[0278] Examples of the heptad aromatic hydrocarbon group include a coronene group and the like.

[0279] R 41 In the case of an aryl group having a substituent, the substituent is a hydroxyl group or an amino group.

[0280] Examples of the aryl group containing a hydroxyl group as a substituent include a phenol group and the like.

[0281] Examples of the aryl group having an amino group as a substituent include an anilino group and the like.

[0282] Examples of the aryl group having a hydroxyl group and an amino group as a substituent include an aminophenol group (hydroxyaniline group) and the like.

[0283] (1-4)R 41 :Alkoxy

[0284] R 41 In the case of an alkoxy group having no substituent, the alkoxy group preferably has 1 to 30 carbon atoms, more preferably 1 to 8 carbon atoms, further preferably 1 to 6 carbon atoms, and particularly preferably 1 to 4 carbon atoms.

[0285] Specific examples of the alkoxy group include a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, an n-butoxy group, a tert-butoxy group, a sec-butoxy group, an isobutoxy group, an n-pentyloxy group, an isopentyloxy group, a neopentyloxy group, a tert-pentyloxy group, a 1-methylbutoxy group, an n-hexyloxy group, a 2-methylpentyloxy group, a 3-methylpentyloxy group, a 2,2-dimethylbutoxy group, a 2,3-dimethylbutoxy group, an n-heptyloxy group, a 2-methylhexyloxy group, a 3-methylhexyloxy group, a 2,2-dimethylpentyloxy group, a 2,3-dimethylpentyloxy group, a 2,4-dimethylpentyloxy group, a 3,3-dimethylpentyloxy group, a 3-ethylpentyloxy group, a 2,2,3-trimethylbutoxy group, an n-octyloxy group, an isooctyloxy group, a 2-ethylhexyloxy group, a nonyloxy group, and a decyloxy group.

[0286] R 41 In the case of an alkoxy group having a substituent, the substituent is a hydroxyl group or an amino group.

[0287] Examples of the alkoxy group containing a hydroxy group as a substituent include a hydroxymethyleneoxy group, a hydroxyethyleneoxy group, a hydroxypropyleneoxy group, and a hydroxybutyleneoxy group.

[0288] Examples of the alkoxy group containing an amino group as a substituent include an aminomethyleneoxy group, an aminoethyleneoxy group, an aminopropyleneoxy group, and an aminobutyleneoxy group.

[0289] Examples of the alkoxy group containing a hydroxyl group and an amino group as a substituent include a hydroxyaminomethyleneoxy group, a hydroxyaminoethyleneoxy group, and a hydroxyaminopropyloxy group.

[0290] (2)R 42 , R 43 and R 44

[0291] In the general formula (IV), R 42 , R 43 and R 44 Each independently represents a hydrogen atom; a hydroxyl group; an alkyl group which may contain one or more substituents selected from the group consisting of a hydroxyl group and an amino group; an amino group which may contain one or more substituents selected from the group consisting of a hydroxyl group and an alkyl group; an aryl group which may contain one or more substituents selected from the group consisting of a hydroxyl group and an amino group; or an alkoxy group which may contain one or more substituents selected from the group consisting of a hydroxyl group and an amino group. For the aforementioned amino group, two aforementioned substituents may be connected to each other to form a ring. Among them, R 42, R 43 and R 44 At least two of them are not hydrogen atoms.

[0292] Examples of the alkyl group, the amino group, the aryl group, and the alkoxy group include the group corresponding to the above “R 41 The same example as shown in "

[0293] Among them, R 42 , R 43 and R 44 Preferably, each independently is a hydrogen atom; an alkyl group which may contain one or more substituents selected from the group consisting of a hydroxyl group and an amino group; or an aryl group which may contain one or more substituents selected from the group consisting of a hydroxyl group and an amino group, and R 42 , R 43 and R 44 At least 2 of them are not hydrogen atoms.

[0294] Among the compounds (IV), R 41 is an alkoxy group, R 42 is a hydrogen atom or an alkyl group, and R 43 and R 44 It is an alkyl group.

[0295] In addition, since compound (IV) has a tert-butyl ester structure or a tert-amyl ester structure, the low-temperature curing property and water resistance when forming a coating film are excellent. In addition, since compound (IV) has a sec-butyl ester structure or an isopropyl ester structure, there is a tendency that the storage stability (water dispersion stability and viscosity stability) when forming a coating composition and the low-temperature curing property and hardness retention when forming a coating film are excellent.

[0296] Specific preferred examples of compound (IV) include isopropyl acetoacetate, di-sec-butyl malonate, di-tert-butyl malonate, di-tert-amyl malonate, diisopropyl malonate, tert-butyl ethyl malonate, and isopropyl ethyl malonate.

[0297] Among them, from the viewpoint of further improving the low-temperature curability of the obtained coating film, di-sec-butyl malonate, di-t-butyl malonate, di-t-amyl malonate, diisopropyl malonate, or t-butyl ethyl malonate is preferred.

[0298] The hydrophilic compound used as a raw material of the hydrophilic blocked polyisocyanate is described below.

[0299] [Hydrophilic compounds]

[0300] The hydrophilic compound is a compound having a hydrophilic group, and in order to react with one isocyanate group, it is preferred that the hydrophilic compound has one or more active hydrogen groups for reacting with the isocyanate group possessed by the polyisocyanate relative to one molecule of the hydrophilic compound. Specifically, the active hydrogen group includes a hydroxyl group, a mercapto group, a carboxylic acid group, an amino group, and a thiol group.

[0301] The hydrophilic group can include nonionic hydrophilic groups, cationic hydrophilic groups, and anionic hydrophilic groups. These hydrophilic groups can be used alone or in combination of two or more. Among them, as the hydrophilic group, from the viewpoint of easy acquisition and not susceptible to electrical interaction with the compound, it is preferably a nonionic hydrophilic group.

[0302] (1) Hydrophilic compounds having nonionic hydrophilic groups

[0303] As the hydrophilic compound having a nonionic hydrophilic group (hereinafter sometimes referred to as "nonionic hydrophilic compound"), specifically, monohydric alcohols and compounds formed by adding ethylene oxide to the hydroxyl group of alcohols can be listed. Examples of monohydric alcohols include methanol, ethanol, butanol, etc. Examples of compounds formed by adding ethylene oxide to the hydroxyl group of alcohols include ethylene glycol, diethylene glycol, polyethylene glycol, etc. These nonionic hydrophilic compounds also have active hydrogen groups that react with isocyanate groups.

[0304] Among them, as the nonionic hydrophilic compound, from the viewpoint of improving the water dispersibility of the water-dispersible polyisocyanate with a small amount, preferably a polyalkylene glycol monoalkyl ether obtained by adding an alkylene oxide to the hydroxyl group of a monohydric alcohol, more preferably a polyethylene glycol monoalkyl ether, and still more preferably a polyethylene glycol monomethyl ether.

[0305] The number of ethylene oxide additions of the compound to which ethylene oxide is added is preferably 4 or more and 30 or less, more preferably 4 or more and 20 or less. When the number of ethylene oxide additions is at least the above lower limit, water dispersibility tends to be more effectively imparted to the water-dispersible polyisocyanate, and when the number of ethylene oxide additions is at most the above upper limit, precipitation of the water-dispersible polyisocyanate tends to be less likely to occur during low-temperature storage.

[0306] From the viewpoint of water dispersion stability of the water-dispersible polyisocyanate, the lower limit of the amount of nonionic hydrophilic groups added to the polyisocyanate (hereinafter sometimes referred to as "the content of nonionic hydrophilic groups") is preferably 1% by mass, more preferably 3% by mass, further preferably 4% by mass, and particularly preferably 4.5% by mass, relative to the mass of the solid content of the water-dispersible polyisocyanate.

[0307] From the viewpoint of water resistance of the obtained coating film, the upper limit of the content of the nonionic hydrophilic group is preferably 30% by mass, more preferably 20% by mass, further preferably 10% by mass, and particularly preferably 8% by mass, based on the mass of the solid content of the water-dispersible polyisocyanate.

[0308] That is, the upper limit of the content of the nonionic hydrophilic group is preferably 1% by mass or more and 30% by mass or less, more preferably 3% by mass or more and 20% by mass or less, further preferably 4% by mass or more and 10% by mass or less, and particularly preferably 4.5% by mass or more and 8% by mass or less, relative to the mass of the solid content of the water-dispersible polyisocyanate.

[0309] When the content of the nonionic hydrophilic group is within the above range, the water-dispersible polyisocyanate is further dispersed in water, and the water resistance of the obtained coating film tends to be improved.

[0310] (2) Hydrophilic compounds having cationic hydrophilic groups

[0311] As the hydrophilic compound having a cationic hydrophilic group (hereinafter sometimes referred to as "cationic hydrophilic compound"), specifically, a compound having a cationic hydrophilic group and an active hydrogen group in combination can be cited. In addition, a compound having an active hydrogen group such as a glycidyl group and a compound having a cationic hydrophilic group such as a sulfide or a phosphine can also be combined as a hydrophilic compound. In this case, a compound having an isocyanate group is reacted with a compound having an active hydrogen group in advance, a functional group such as a glycidyl group is added, and then reacted with a compound such as a sulfide or a phosphine. From the viewpoint of ease of manufacture, a compound having a cationic hydrophilic group and an active hydrogen group in combination is preferably used.

[0312] Specific examples of the compound having a cationic hydrophilic group and an active hydrogen group in combination include dimethylethanolamine, diethylethanolamine, diethanolamine, methyldiethanolamine, etc. In addition, the tertiary amino group added using these compounds can also be quaternized using, for example, dimethyl sulfate or diethyl sulfate.

[0313] The reaction between the cationic hydrophilic compound and the polyisocyanate may be carried out in the presence of a solvent. The solvent in this case preferably does not contain an active hydrogen group, and specific examples thereof include ethyl acetate, propylene glycol monomethyl ether acetate, and dipropylene glycol dimethyl ether.

[0314] The cationic hydrophilic group added to the polyisocyanate is preferably neutralized with a compound having an anionic group. Specific examples of the anionic group include a carboxyl group, a sulfonic acid group, a phosphoric acid group, a halogen group, and a sulfate group.

[0315] Specific examples of the compound having a carboxyl group include formic acid, acetic acid, propionic acid, butyric acid, and lactic acid.

[0316] Specific examples of the compound having a sulfonic acid group include ethanesulfonic acid and the like.

[0317] Specific examples of the compound having a phosphoric acid group include phosphoric acid and acidic phosphoric acid esters.

[0318] Specific examples of the compound having a halogen group include hydrochloric acid and the like.

[0319] Specific examples of the compound having a sulfate group include sulfuric acid and the like.

[0320] Among them, as the compound having an anionic group, a compound having a carboxyl group is preferred, and acetic acid, propionic acid, or butyric acid is more preferred.

[0321] (3) Hydrophilic compounds having anionic hydrophilic groups

[0322] Specific examples of the anionic hydrophilic group include a carboxyl group, a sulfonic acid group, a phosphoric acid group, a halogen group, and a sulfate group.

[0323] As the hydrophilic compound having an anionic hydrophilic group (hereinafter sometimes referred to as "anionic hydrophilic compound"), specifically, there can be listed compounds having a combination of anionic groups and active hydrogen groups, and more specifically, there can be listed compounds having, for example, a carboxyl group of a monohydroxycarboxylic acid or a polyhydroxycarboxylic acid as an anionic group.

[0324] Examples of the monohydroxycarboxylic acid include 1-hydroxyacetic acid, 3-hydroxypropionic acid, 12-hydroxy-9-octadecanoic acid, hydroxypivalic acid (hydroxypivalic acid), and lactic acid.

[0325] Examples of the compound having a carboxyl group of a polyhydroxycarboxylic acid as an anionic group include dimethylolacetic acid, 2,2-dimethylolbutanoic acid, 2,2-dimethylolvaleric acid, dihydroxysuccinic acid, and dimethylolpropionic acid.

[0326] In addition, compounds having a sulfonic acid group and an active hydrogen group in combination may also be mentioned, and more specific examples thereof include isethionic acid.

[0327] Among them, as the compound having an anionic group and an active hydrogen group in combination, hydroxypivalic acid or dimethylolpropionic acid is preferred.

[0328] The anionic hydrophilic group added to the polyisocyanate is preferably neutralized with an amine compound which is a basic substance.

[0329] Specific examples of the amine compound include ammonia and water-soluble amino compounds.

[0330] As the water-soluble amino compound, specifically, for example, monoethanolamine, ethylamine, dimethylamine, diethylamine, triethylamine, propylamine, dipropylamine, isopropylamine, diisopropylamine, triethanolamine, butylamine, dibutylamine, 2-ethylhexylamine, ethylenediamine, propylenediamine, methylethanolamine, dimethylethanolamine, diethylethanolamine, morpholine, etc. can also be listed. In addition, tertiary amines such as triethylamine and dimethylethanolamine can also be listed and can also be used. These amine compounds can be used alone or in combination of two or more.

[0331] [Method for producing blocked polyisocyanate]

[0332] The blocked polyisocyanate is obtained, for example, by reacting a polyisocyanate with the above-mentioned blocking agent.

[0333] The blocking reaction between the polyisocyanate and the blocking agent can be carried out in the presence or absence of a solvent, and the reaction liquid (blocked polyisocyanate composition) obtained by the blocking reaction can be blended with the polyurethane-based curing agent.

[0334] Regarding the mixing ratio of the polyisocyanate and the blocking agent, from the viewpoint of the storage stability of the one-component coating composition, the molar ratio of the active hydrogen groups contained in the blocking agent when the isocyanate groups contained in the polyisocyanate are set to 1 is preferably 0.5 or more and 3.0 or less, more preferably 0.8 or more and 2.0 or less, and further preferably 1 or more and 1.5 or less.

[0335] In the reaction step, the reaction temperature and reaction time are appropriately determined according to the progress of the reaction. The reaction temperature is preferably 0° C. or higher and 150° C. or lower, and the reaction time is preferably 0.5 hour or higher and 24 hours or lower.

[0336] When two blocking agents are used in combination, the blocking reaction using the two blocking agents may be performed simultaneously, or the remaining free isocyanate groups may be blocked first with one blocking agent and then with the other blocking agent.

[0337] In the reaction, a known general catalyst can be used as required. The catalyst is not particularly limited, and examples thereof include the catalysts shown in (1) to (6) below. The catalysts shown below can be used alone or in combination.

[0338] (1) Organic tin compounds such as tin octanoate, 2-ethyl-1-tin hexanoate, ethyltin hexanoate, tin laurate, tin palmitate, dibutyltin oxide, dibutyltin dichloride, dibutyltin diacetate, dibutyltin dimaleate, dibutyltin dilaurate, dioctyltin diacetate, and dioctyltin dilaurate.

[0339] (2) Organic zinc compounds such as zinc chloride, zinc octoate, zinc 2-ethyl-1-hexanoate, zinc 2-ethylhexanoate, zinc stearate, zinc naphthenate, and zinc acetylacetonate.

[0340] (3) Organic titanium compounds.

[0341] (4) Organic zirconium compounds.

[0342] (5) Tertiary amines such as triethylamine, tributylamine, N,N-diisopropylethylamine, and N,N-dimethylethanolamine.

[0343] (6) Diamines such as triethylenediamine, tetramethylethylenediamine, and 1,4-diazabicyclo[2.2.2]octane.

[0344] The completion of the reaction can be determined by confirming the disappearance or reduction of isocyanate groups using infrared spectroscopy or the like, for example.

[0345] When a solvent is used, it is sufficient to use a solvent that is inactive to isocyanate groups.

[0346] When a solvent is used, the content of the solid content derived from the polyisocyanate and the blocking agent relative to 100 parts by mass of the blocked polyisocyanate composition can be generally 10 parts by mass or more and 95 parts by mass or less, preferably 20 parts by mass or more and 80 parts by mass or less, and more preferably 30 parts by mass or more and 70 parts by mass or less.

[0347] Alternatively, the blocked polyisocyanate can be obtained as a hydrophilic blocked polyisocyanate by, for example, reacting a polyisocyanate, a hydrophilic compound, and a blocking agent.

[0348] The reaction of the isocyanate group of the polyisocyanate with the hydrophilic compound and the reaction of the polyisocyanate with the blocking agent may be carried out simultaneously, or any one of the reactions may be carried out in advance and then the second reaction may be carried out. Among them, it is preferred to first carry out the reaction of the isocyanate group with the hydrophilic compound to obtain a polyisocyanate modified with the hydrophilic compound (hereinafter sometimes referred to as "modified polyisocyanate"), and then carry out the reaction of the obtained modified polyisocyanate with the blocking agent.

[0349] The reaction between the polyisocyanate and the hydrophilic compound can use an organic metal salt, a tertiary amine compound, or an alkali metal alkoxide as a catalyst. Examples of the metal constituting the organic metal salt include tin, zinc, and lead. Examples of the alkali metal include sodium.

[0350] The reaction temperature of the polyisocyanate and the hydrophilic compound is preferably -20°C or higher and 150°C or lower, more preferably 30°C or higher and 100°C or lower. When the reaction temperature is above the lower limit, there is a tendency that the reactivity can be further increased. In addition, when the reaction temperature is below the upper limit, there is a tendency that the side reaction can be more effectively suppressed.

[0351] It is preferred that the hydrophilic compound completely reacts with the polyisocyanate so that it does not remain in an unreacted state. By not remaining in an unreacted state, there is a tendency to more effectively suppress the water dispersion stability of the blocked isocyanate composition of the present embodiment and the decrease in low temperature curability when forming a coating composition.

[0352] The blocking reaction of the polyisocyanate or modified polyisocyanate with the blocking agent can be carried out in the presence or absence of a solvent.

[0353] The capping reaction can be carried out by the above-mentioned reaction.

[0354] When the blocking reaction is carried out using water or a solvent, it is sufficient to use a solvent inactive to an isocyanate group.

[0355] Examples of the solvent include 1-methylpyrrolidone, ethylene glycol monoethyl ether, diethylene glycol monoethyl ether, ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, dipropylene glycol monomethyl ether, propylene glycol monomethyl ether, 3-methoxy-3-methyl-1-butanol, ethylene glycol diethyl ether, diethylene glycol diethyl ether, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dipropylene glycol dimethyl ether, propylene glycol dimethyl ether, methyl ethyl ketone, acetone, Methyl isobutyl ketone, propylene glycol monomethyl ether acetate, ethanol, methanol, isopropanol, 1-propanol, isobutyl alcohol, 1-butanol, 2-ethylhexanol, cyclohexanol, ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, 1,4-butanediol, 1,3-butanediol, ethyl acetate, isopropyl acetate, butyl acetate, toluene, xylene, pentane, isopentane, hexane, isohexane, cyclohexane, solvent naphtha, mineral spirits, etc. These solvents may be used alone or in combination of two or more.

[0356] When a solvent is used, the content of the solid content derived from the polyisocyanate and the blocking agent relative to 100 parts by mass of the blocked polyisocyanate composition can be generally 10 parts by mass or more and 95 parts by mass or less, preferably 20 parts by mass or more and 80 parts by mass or less, and more preferably 30 parts by mass or more and 70 parts by mass or less.

[0357] When water is used, it is preferred to add the prescribed amount by dividing or dropping. When divided, it is preferably divided into 4 or more and 8 or less of the prescribed amount. In addition, it is preferred that the liquid temperature is maintained at 50°C or higher when the blocked polyisocyanate concentration relative to water is 55% by mass or higher, the liquid temperature is maintained at 45°C or higher and 50°C or lower when it is 45% by mass or higher and lower than 55% by mass, and the liquid temperature is maintained at lower than 50°C when it is lower than 45% by mass.

[0358] When water is added, the liquid temperature is 80° C. or higher and lower than 20° C., thereby increasing the average particle size (average dispersed particle size) of the aqueous dispersion of the blocked polyisocyanate, and sometimes causing precipitation, separation, etc., which may reduce the stability of the aqueous dispersion. Therefore, the blocked polyisocyanate concentration of the aqueous dispersion composition obtained in this way is preferably 10% by mass or higher and 40% by mass or lower.

[0359] In any of the above-mentioned methods for producing blocked polyisocyanates, the encapsulated thermal latent catalyst can be added at any time before or after the reaction of the polyisocyanate with the hydrophilic compound, and before or after the blocking reaction. In order to suppress the deterioration of the encapsulated thermal latent catalyst, it is preferably added after the reaction of the polyisocyanate with the hydrophilic compound and after the blocking reaction, and the temperature is lowered to below 100° C. The amount of the encapsulated thermal latent catalyst added is preferably added in such a manner that the content of the encapsulated thermal latent catalyst when forming the coating composition is within the range described below.

[0360] Furthermore, an antioxidant or an ultraviolet absorber may be added to the obtained polyisocyanate in order to suppress coloration during storage, for example.

[0361] As antioxidants, hindered phenols such as 2,6-di-tert-butyl-p-cresol, etc. can be listed. As ultraviolet absorbers, for example, benzotriazole, benzophenone, etc. can be listed. These antioxidants and ultraviolet absorbers can be used alone or in combination of two or more. Their addition amount is preferably 10 mass ppm or more and 500 mass ppm or less relative to the mass of the polyisocyanate.

[0362] <Encapsulated thermal latent catalyst>

[0363] The encapsulated thermal latent catalyst of the present embodiment is covered with a polyurea film derived from a polyamine compound and a polyisocyanate (second polyisocyanate).

[0364] The encapsulated thermal latent catalyst of the present embodiment is covered with a polyurea film by a compound having catalytic activity. When it is mixed with a coating composition, etc., the expression of catalytic activity can be suppressed, and storage stability can be well maintained. On the other hand, when a coating film is formed using a coating composition containing the encapsulated thermal latent catalyst of the present embodiment, the polyurea film is ruptured or swelled by heat, and the compound having catalytic activity is released into the coating liquid, thereby showing catalytic activity, and the curing property at a low temperature of about 60°C or more and about 110°C or less (hereinafter also referred to as "low-temperature curing property") can be good. Furthermore, the obtained coating film can exhibit excellent scratch resistance through the presence of the polyurea film derived from the encapsulated thermal latent catalyst in the cured coating film.

[0365] The constituent components of the encapsulated thermal latent catalyst according to the present embodiment will be described in detail below.

[0366] <Compounds having catalytic activity>

[0367] The compound having catalytic activity corresponds to a substance that catalyzes the urethanization reaction or the dissociation reaction of the blocking agent of the blocked isocyanate group.

[0368] For example, organic basic compounds such as tertiary amine compounds, organic acidic compounds having a carboxyl group, a sulfonyl group, an acidic phosphoric acid group, and the like, and metal compounds are mentioned.

[0369] Among them, organic basic compounds and metal compounds are preferred, and metal compounds are most preferred.

[0370] [Organic basic compounds]

[0371] Examples of the organic basic compound include tertiary amines such as triethylamine, tributylamine, N,N-diisopropylethylamine, and N,N-dimethylethanolamine, and 1,4-diazabicyclo[2.2.2]octane.

[0372] [Organic acid compounds]

[0373] Examples of the organic acidic compound include acetic acid, propionic acid, p-toluenesulfonic acid, and dibutyl phosphate.

[0374] [Metal compounds]

[0375] The metal compound is a compound having a basic group or an organic ligand on a metal, and preferably exhibits a catalytic effect on the urethanization reaction.

[0376] Examples of the metal species constituting the metal compound include sodium, potassium, lithium, cesium, nickel, cobalt, cadmium, barium, calcium, zinc, manganese, copper, cerium, zirconium, tin, iron, lead, germanium, antimony, aluminum, titanium, and bismuth. Among them, the metal species is preferably a metal having a valence of two or more, more preferably nickel, cobalt, cadmium, barium, calcium, zinc, manganese, copper, cerium, zirconium, tin, iron, lead, germanium, antimony, aluminum, titanium, or bismuth, further preferably tin, zirconium, or bismuth, and still more preferably tin or bismuth.

[0377] Examples of the basic group include hydroxides, alkoxides, hydroxides of onium salts, carboxylic acid onium salts, halides of onium salts, aminosilanes, amines, phosphines, etc. The onium salt is preferably an ammonium salt, a phosphonium salt or a sulfonium salt.

[0378] Examples of the organic ligand include carboxylates (carboxylic acids), acetylacetonates, carboxylic acid onium salts, metal salts of active methylene compounds, onium salts of active methylene compounds, etc. The onium salt is preferably an ammonium salt, a phosphonium salt or a sulfonium salt.

[0379] Among them, the metal compound is preferably soluble in a solvent during synthesis and exhibits hydrophobicity, and therefore a metal carboxylate or a metal acetylacetonate is preferred.

[0380] The carboxylates (carboxylic acids) constituting the metal carboxylates include both monocarboxylic acids and dicarboxylic acids, and examples thereof include aliphatic saturated acids, unsaturated acids, and aromatic acids such as formic acid, acetic acid, acrylic acid, methacrylic acid, propionic acid, butyric acid, caproic acid, octyl acid, octanoic acid, capric acid, stearic acid, oleic acid, eicosanoic acid, myristic acid, and benzoic acid. Among them, as the carboxylates (carboxylic acids), from the viewpoint of compatibility, preferably the carbon number is 1 or more and 12 or less, and from the viewpoint of yellowing of the coating film, more preferably the aliphatic acid has a carbon number of 1 or more and 12 or less.

[0381] Specific examples of preferred metal carboxylates include bismuth 2-ethylhexanoate, dibutyltin dilaurate, and dioctyltin dilaurate.

[0382] <Polyurea film>

[0383] The polyurea film is derived from a polyamine compound and a second polyisocyanate. Among them, the second polyisocyanate is preferably derived from a water-dispersible polyisocyanate, and the polyurea film is preferably a reaction product of a polyamine compound and a water-dispersible polyisocyanate.

[0384] [Polyamine compounds]

[0385] The polyamine compound is not particularly limited, and is a polyamine compound having one or more primary or secondary amino groups in one molecule and two or more functional groups capable of reacting with an isocyanate group in one molecule.

[0386] That is, the polyamine compound includes a polyamine having only a primary amino group or a secondary amino group, and an alkanolamine having a primary amino group or a secondary amino group and a hydroxyl group.

[0387] Specific examples of the polyamine include the polyamines shown in the following (1) to (3).

[0388] (1) Diamines such as ethylenediamine, propylenediamine, butylenediamine, triethylenediamine, hexamethylenediamine, 4,4'-diaminodicyclohexylmethane, piperazine, 2-methylpiperazine, and isophoronediamine.

[0389] (2) Chain polyamines having three or more amino groups, such as hexamethylenetriamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentamethylenehexamine, and tetrapropylenepentamine.

[0390] (3) Cyclic polyamines such as 1,4,7,10,13,16-hexaazacyclooctadecane, 1,4,7,10-tetraazacyclodecane, 1,4,8,12-tetraazacyclopentadecane, and 1,4,8,11-tetraazacyclotetradecane.

[0391] Specific examples of the alkanolamine include monoethanolamine, diethanolamine, aminoethylethanolamine, N-(2-hydroxypropyl)ethylenediamine, mono-, di-(n- or iso-)propanolamine, ethylene glycol-bis-propylamine, neopentanolamine, and methylethanolamine.

[0392] Among them, the polyamine compound is preferably a polyamine having only primary or secondary amino groups, and from the viewpoint of reaction control during polyurea film formation and catalytic activity of the metal compound during heating, a polyamine having two or more secondary amino groups in one molecule is more preferred, and a polyamine having two secondary amino groups in one molecule is further preferred.

[0393] Examples of the polyamine having two or more secondary amino groups in one molecule include a compound represented by the following general formula (I) (hereinafter sometimes referred to as “compound (I)”).

[0394]

[0395] In the above general formula (I), X 11 It is an n-valent organic group obtained by removing the primary amino group of an n11-valent polyamine. 11 and R 12 are the same or different organic groups that are inactive to isocyanate groups under the reaction conditions. n11 is an integer greater than 2.

[0396] X in formula (I) 11There are no particular limitations, but from the viewpoint of yellowing resistance, an organic group based on an aliphatic and / or alicyclic polyamine having no aromatic group is preferred, for example, an n11-valent polyamine selected from the group consisting of ethylenediamine, 1,2-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, 2,5-diamino-2,5-dimethylhexane, 2,2,4- and / or 2,4,4-trimethyl-1,6-diaminohexane, 1,11-diaminoundecane, alkane, 1,12-diaminododecane, 1-amino-3,3,5-trimethyl-5-aminomethylcyclohexane, 2,4- and / or 2,6-hexahydrobenzylidene diamine, 2,4'- and / or 4,4'-diaminodicyclohexylmethane, 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, 2,4,4'-triamino-5-methyldicyclohexylmethane, and an organic group having a number average molecular weight of 148 to 6000, a polyether polyamine having a primary amino group and an aliphatic bond.

[0397] Among them, as X 11 , preferably an organic group based on 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, 2,2,4- and / or 2,4,4-trimethyl-1,6-diaminohexane, 1-amino-3,3,5-trimethyl-5-aminomethylcyclohexane, 4,4'-diaminodicyclohexylmethane, or 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, and more preferably an organic group based on 4,4'-diaminodicyclohexylmethane or 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane.

[0398] R in formula (I) 11 and R 12 The term "inactive with respect to isocyanate groups under the reaction conditions" means that these groups do not have a Zerevitinoff-active hydrogen-containing group (CH acidic compound) such as a hydroxyl group, an amino group, or a thiol group.

[0399] R 11 and R 12 Preferably, they are each independently an alkyl group having 1 to 10 carbon atoms, and more preferably a methyl group, an ethyl group, or a butyl group.

[0400] n11 in formula (I) is preferably an integer of 2 or more and 6 or less, more preferably an integer of 2 or more and 4 or less, and further preferably 2.

[0401] Preferred examples of compound (I) include aspartic acid ester compounds derived from two molecules of aspartic acid having a secondary amino group and one molecule of 4,4′-diaminodicyclohexylmethane.

[0402] The method for producing the compound (I) is not particularly limited, and the compound (I) can be produced, for example, by reacting a primary polyamine represented by the following formula (II) with a maleate or fumarate represented by the following formula (III).

[0403] X 11 -[NH2] n11 (II)

[0404] R 11 OOC-CH=CH-COOR 12 (III)

[0405] In the above formula, X 11 , R 11 , R 12 , and n11 have the same meanings as those shown in formula (I).

[0406] Suitable polyamines are not particularly limited, for example, 11 The basis is the above-mentioned diamine.

[0407] In addition, suitable maleic acid esters or fumaric acid esters are not particularly limited, and for example, maleic acid esters or fumaric acid esters having R in formula (I) are 11 and R 12 The group specified in R 11 and R 12 Of these, preferably R 11 and R 12 The maleate or fumarate is an alkyl group having 1 to 10 carbon atoms, and more preferably dimethyl maleate, diethyl maleate, dibutyl maleate, dimethyl fumarate, diethyl fumarate, or dibutyl fumarate.

[0408] The preparation of the aspartic acid ester compound derived from the described starting material is preferably carried out in a temperature range of 0°C to 100°C. The starting material has a ratio such that at least one, preferably only one, olefinic double bond exists in each primary amino group. The starting material can be distilled after the reaction as needed to remove the starting material used in excess. The reaction can be carried out in bulk or in the presence of a suitable solvent (not particularly limited, for example, methanol, ethanol, propanol or dioxane, or a mixture of such solvents).

[0409] [Polyisocyanate (second polyisocyanate)]

[0410] A polyisocyanate (second polyisocyanate) is used for forming the urea film used in the encapsulated catalyst of the present embodiment. As the second polyisocyanate, a water-dispersible polyisocyanate is preferably used.

[0411] [Water-dispersible polyisocyanate]

[0412] In addition, the encapsulated thermal latent catalyst of the present embodiment is preferably manufactured by an interfacial polymerization method that forms a polyurea film at the interface of water and oil droplets, so the polyisocyanate preferably exhibits water dispersibility, that is, a water-dispersible polyisocyanate. The water-dispersible polyisocyanate is derived from a polyisocyanate and a hydrophilic compound, that is, a reaction product of a polyisocyanate and a hydrophilic compound. For water-dispersible polyisocyanates, at least a portion of the isocyanate groups of the polyisocyanate and the functional group of the hydrophilic compound form a bond and introduce a hydrophilic group. In other words, at least a portion of the isocyanate groups of the polyisocyanate are modified by a hydrophilic compound.

[0413] The ratio of the isocyanate groups of the water-dispersible polyisocyanate modified with the hydrophilic compound, i.e., the modification rate relative to 100 mol% of the isocyanate groups of the raw material polyisocyanate, is preferably 0.5 mol% to 50 mol%, more preferably 1 mol% to 30 mol%, further preferably 2 mol% to 20 mol%, particularly preferably 3 mol% to 15 mol%. When the modification rate is at least the lower limit, water dispersibility can be more fully ensured, and when it is at most the upper limit, the strength of the polyurea film can be more fully maintained.

[0414] (Hydrophilic Compounds)

[0415] As the hydrophilic compound, the hydrophilic compound described in the above-mentioned "hydrophilic blocked polyisocyanate" is used.

[0416] (Method for producing water-dispersible polyisocyanate)

[0417] The water-dispersible polyisocyanate can be obtained by, for example, reacting a polyisocyanate with a hydrophilic compound.

[0418] The reaction between the polyisocyanate and the hydrophilic compound can use an organic metal salt, a tertiary amine compound, or an alkali metal alkoxide as a catalyst. Examples of the metal constituting the organic metal salt include tin, zinc, and lead. Examples of the alkali metal include sodium.

[0419] The reaction temperature of the polyisocyanate and the hydrophilic compound is preferably -20°C or higher and 150°C or lower, more preferably 30°C or higher and 100°C or lower. When the reaction temperature is above the lower limit, there is a tendency that the reactivity can be further increased. In addition, when the reaction temperature is below the upper limit, there is a tendency that the side reaction can be more effectively suppressed.

[0420] It is preferred that the hydrophilic compound is completely reacted with the polyisocyanate so that it does not remain in an unreacted state. By not remaining in an unreacted state, there is a tendency to more effectively suppress the water dispersion stability of the water-dispersible isocyanate and the low-temperature curability of the coating composition containing the encapsulated thermal latent catalyst of the present embodiment.

[0421] <Method for producing encapsulated thermal latent catalyst>

[0422] The method for producing the encapsulated thermal latent catalyst according to the present embodiment will be described in detail below.

[0423] The capsule component of the encapsulated thermal latent catalyst is formed of a polyurea film and is formed by the reaction of a polyamine compound and a second polyisocyanate.

[0424] In addition, in the reaction of the polyamine compound with the second polyisocyanate, the molar ratio of the amine group derived from the polyamine compound to the isocyanate group of the polyisocyanate (amine group / isocyanate group) is not particularly limited, and the molar ratio of the amine group / isocyanate group is preferably 0.2 to 5, more preferably 0.33 to 4, further preferably 0.5 to 2.5, and particularly preferably 0.6 to 1.5. When the molar ratio of the amine group / isocyanate group is above the lower limit, a polyurea film can be formed more fully, and on the other hand, when it is below the upper limit, the separation of the compound having catalytic activity (such as a metal compound) after encapsulation is better.

[0425] The method for forming the polyurea film is not particularly limited, but an interfacial polymerization method is preferably used.

[0426] That is, as a method for producing an encapsulated thermally latent catalyst according to the present embodiment, a method including the following steps is specifically preferably exemplified.

[0427] A step of mixing a polyamine compound and a compound having catalytic activity (such as a metal compound) to prepare a mixture (hereinafter sometimes referred to as "step 1");

[0428] a step of dispersing the mixture in water to prepare a dispersion (hereinafter sometimes referred to as "step 2"); and

[0429] A step (hereinafter sometimes referred to as "step 3") of adding a water-dispersible polyisocyanate dropwise to the dispersion to form a polyurea film derived from the polyamine compound and the water-dispersible polyisocyanate by an interfacial polymerization method, thereby covering the catalytically active compound (e.g., a metal compound) with the polyurea film.

[0430] In step 1, a catalytically active compound (e.g., a metal compound) and a polyamine compound are uniformly mixed to prepare a mixture. Here, the mixing ratio of the active ingredient of the catalytically active compound to the polyamine compound (catalytically active compound: polyamine compound) (mass ratio) is preferably 5:1 to 1:5, more preferably 3:1 to 1:3. When the mixing ratio of the catalytically active compound to the polyamine compound satisfies the above range, there is a tendency to achieve both storage stability and low-temperature curing properties.

[0431] In step 1, a solvent is added as needed. The type of solvent and the amount of solvent added can be appropriately selected to uniformly disperse the above components in the mixture. Among them, as the solvent, a hydrophobic solvent is preferred. As the hydrophobic solvent, for example, toluene, xylene, butyl acetate, etc. can be listed.

[0432] In step 2, the mixture is dispersed in water to prepare a dispersion in which a compound having catalytic activity (for example, a metal compound) and an organic component containing a polyamine compound are dispersed in water.

[0433] The method for preparing the dispersion is not particularly limited, and examples thereof include a method of dropping the mixture into water while stirring.

[0434] The dropping speed is not particularly limited and can be appropriately adjusted so that the oil droplets containing the organic component have a desired size.

[0435] The temperature is not particularly limited, and the reaction may be performed at, for example, room temperature (a temperature of about 5° C. or higher and 35° C. or lower).

[0436] After the dropwise addition is completed, stirring is performed for 1 minute to 30 minutes, thereby obtaining a dispersion in which the organic component is uniformly dispersed.

[0437] In step 3, water-dispersible polyisocyanate is added to the dispersion dropwise and stirred. Thus, the water-dispersible polyisocyanate added to the reaction system is dispersed in water, and reacts with the oil droplets containing polyamine compounds close to each other, thereby forming a polyurea film at the interface between the oil droplets and water, and the catalytically active compound is covered by the polyurea film. Here, the mixing ratio of water-dispersible polyisocyanate (solid content 100% by mass component) and the catalytically active compound (water-dispersible polyisocyanate: catalytically active compound) (mass ratio) is preferably 5: 1 to 1: 5, more preferably 3: 1 to 1: 3. When the mixing ratio of the catalytically active compound to the polyamine compound satisfies the above range, there is a tendency to take into account both storage stability and low temperature curing.

[0438] The temperature when adding the polyisocyanate is not particularly limited, but is preferably 0° C. to 80° C., more preferably 20° C. to 40° C. When the temperature is at least the lower limit, the formation rate of the polyurea film can be more sufficiently maintained, while when the temperature is at most the upper limit, local reactions are suppressed, and finer capsules can be formed.

[0439] The reaction time after adding the polyisocyanate is preferably 15 minutes to 120 minutes, more preferably 30 minutes to 60 minutes.

[0440] The median particle size of the obtained encapsulated thermal latent catalyst is preferably 10 nm or more and 3 μm or less, more preferably 30 nm or more and 2 μm or less, further preferably 50 nm or more and 1 μm or less, and further preferably 50 nm or more and 200 nm or less. When the median particle size is above the lower limit, the aggregation stability can be further maintained, and on the other hand, when it is below the upper limit, the smoothness of the cured coating film formed using the encapsulated thermal latent catalyst can be further maintained.

[0441] The median diameter referred to herein refers to the 50% diameter (D) based on the number of particles measured using a cumulative distribution curve using a laser diffraction / scattering particle size distribution measuring device (MicrotracBEL Corp., "MICROTRAC NANOTRAC UPA-EX150"). 50 ).

[0442] In the encapsulated thermal latent catalyst of the present embodiment, the content of the compound having catalytic activity (e.g., a metal compound) relative to the total mass of the solid component of the encapsulated thermal latent catalyst can be set, for example, to 1% by mass or more and 60% by mass or less, 5% by mass or more and 50% by mass or less, 10% by mass or more and 40% by mass or less, or 20% by mass or more and 35% by mass or less.

[0443] The encapsulated thermal latent catalyst of the present embodiment can be used in a state of being dispersed in an organic solvent such as water, toluene, xylene, or butyl acetate.

[0444] The content of the encapsulated thermal latent catalyst in the dispersion can be, for example, 1% by mass to 50% by mass, 5% by mass to 45% by mass, 10% by mass to 40% by mass, or 20% by mass to 35% by mass, relative to the total mass of the dispersion.

[0445] <Other ingredients>

[0446] The polyurethane curing agent of the present embodiment may further contain one or more selected from the group consisting of other curing agents, antioxidants, light stabilizers, polymerization inhibitors, and surfactants. Among them, it is preferred to further contain a surfactant.

[0447] Examples of the other curing agent include melamine resins, urea resins, epoxy group-containing compounds or resins, carboxyl group-containing compounds or resins, acid anhydrides, alkoxysilyl group-containing compounds or resins, and hydrazide compounds.

[0448] As antioxidants and light stabilizers, for example, aliphatic, aromatic or alkyl-substituted aromatic esters of phosphoric acid or phosphorous acid, hypophosphorous acid derivatives; phosphorus compounds such as phenylphosphonic acid, phenylphosphinic acid, diphenylphosphonic acid, polyphosphonates, dialkyl pentaerythritol diphosphites, dialkyl bisphenol A diphosphites; phenol derivatives (particularly hindered phenol compounds); sulfur-containing compounds such as thioether compounds, disulfide carboxylate compounds, mercaptobenzimidazole compounds, diphenylthiourea compounds, thiodipropionate esters; tin compounds such as tin maleate and dibutyltin oxide, etc. These may be contained alone or in combination of two or more.

[0449] Examples of the polymerization inhibitor include hydroquinones, phenols, cresols, catechols, and benzoquinones. Specifically, examples of the polymerization inhibitor include benzoquinone, p-benzoquinone, p-toluoquinone, p-xylenequinone, naphthoquinone, 2,6-dichloroquinone, hydroquinone, trimethylhydroquinone, catechol, p-tert-butylcatechol, 2,5-di-tert-butylhydroquinone, monomethylhydroquinone, p-methoxyphenol, 2,6-di-tert-butyl-p-cresol, and hydroquinone monomethyl ether. These may be contained alone or in combination of two or more.

[0450] Examples of the surfactant include known anionic surfactants, cationic surfactants, and amphoteric surfactants.

[0451] 《Coating composition》

[0452] Hereinafter, a two-component coating composition, a solvent-based one-component coating composition, and an aqueous one-component coating composition may be collectively referred to as a coating composition.

[0453] <Content of Encapsulated Thermal Latent Catalyst>

[0454] The coating composition of the present embodiment contains the above-mentioned polyurethane curing agent. The coating composition of the present embodiment has excellent storage stability and low-temperature curability, and can obtain a coating film having excellent scratch resistance by containing the above-mentioned polyurethane curing agent.

[0455] The content of the encapsulated thermal latent catalyst in the coating composition of the present embodiment is not particularly limited. The mass of the catalytically active compound (e.g., a metal compound) contained in the encapsulated thermal latent catalyst, relative to the total mass of the solid component of the coating composition, is preferably greater than 0.01 mass % and less than 10.0 mass %, more preferably greater than 0.05 mass % and less than 5.0 mass %, further preferably greater than 0.1 mass % and less than 3.5 mass %, particularly preferably greater than 0.3 mass % and less than 2.5 mass %, and most preferably greater than 0.5 mass % and less than 2.0 mass %.

[0456] By the content of the encapsulated thermal latent catalyst being above the above lower limit, the catalytic activity can be more fully exerted, and the low temperature curing property and the scratch resistance when forming the coating film can be made better. On the other hand, by being below the above upper limit, the storage stability of the coating composition can be made better.

[0457] The coating composition of the present embodiment is mixed with a polyvalent active hydrogen compound. The content of the solid component of the polyvalent active hydrogen compound in the coating composition of the present embodiment is not particularly limited, and relative to the gross mass of the coating composition, is preferably 10% by mass or more and 50% by mass or less, more preferably 20% by mass or more and 40% by mass or less, and further preferably 23% by mass or more and 35% by mass or less. By being within the above range, there is a tendency for low temperature curing to improve.

[0458] <Kit for two-component coating composition>

[0459] The two-component coating composition kit according to the present embodiment comprises the above-mentioned polyurethane-based curing agent and a polyvalent active hydrogen compound.

[0460] [Polyvalent active hydrogen compounds]

[0461] The polyvalent active hydrogen compound is not particularly limited, and examples thereof include polyols, polyamines, alkanolamines, etc. These polyvalent active hydrogen compounds may be contained alone or in combination of two or more. Among them, polyols are preferred as the polyvalent active hydrogen compound.

[0462] (Polyol)

[0463] Examples of the polyol include polyester polyol, polyether polyol, acrylic polyol, polyolefin polyol, fluorine polyol, polycarbonate polyol, polyurethane polyol, etc. These polyols may be contained alone or in combination of two or more.

[0464] Among them, as the polyol, polyester polyol or acrylic polyol is preferred.

[0465] 1. Polyester polyol

[0466] The polyester polyol can be obtained, for example, by subjecting a dibasic acid alone or in a mixture of two or more thereof to a condensation reaction with a polyol alone or in a mixture of two or more thereof.

[0467] Examples of the dibasic acid include carboxylic acids such as succinic acid, adipic acid, dimer acid, maleic anhydride, phthalic anhydride, isophthalic acid, terephthalic acid, and 1,4-cyclohexanedicarboxylic acid.

[0468] Examples of the polyol include ethylene glycol, propylene glycol, diethylene glycol, 1,4-butanediol, neopentyl glycol, 1,6-hexanediol, trimethylpentanediol, cyclohexanediol, trimethylolpropane, glycerin, pentaerythritol, 2-methylolpropanediol, and ethoxylated trimethylolpropane.

[0469] Furthermore, for example, polycaprolactones obtained by ring-opening polymerization of lactones such as ε-caprolactone using a polyol can also be used as the polyester polyol.

[0470] 2. Polyether polyols

[0471] The polyether polyols are not particularly limited, and examples thereof include the polyether polyols shown in the following (1) to (3).

[0472] (1) Polyether polyols obtained by randomly or block-adding an alkylene oxide alone or in mixture to a polyvalent hydroxy compound alone or in mixture using a catalyst.

[0473] Examples of the catalyst include hydroxides (lithium, sodium, potassium, etc.), strong alkaline catalysts (alkoxides, alkylamines, etc.), and composite metal cyanide complexes (metalloporphyrins, zinc hexacyanocobaltate complexes, etc.).

[0474] Examples of the alkylene oxide include ethylene oxide, propylene oxide, butylene oxide, cyclohexene oxide, and styrene oxide.

[0475] (2) Polyether polyols obtained by reacting a polyamine compound with an alkylene oxide.

[0476] Examples of the polyamine compound include ethylenediamines and the like.

[0477] Examples of the alkylene oxide include the same ones as exemplified in (1).

[0478] (3) So-called polymer polyols obtained by using the polyether polyols obtained in (1) or (2) as a medium to polymerize acrylamide or the like.

[0479] Examples of the polyvalent hydroxy compound include the polyvalent hydroxy compounds shown in the following (i) to (vi).

[0480] (i) Diglycerol, di(trimethylolpropane), pentaerythritol, dipentaerythritol, etc.

[0481] (ii) Sugar alcohol compounds such as erythritol, D-threitol, L-arabitol, ribitol, xylitol, sorbitol, mannitol, dulcitol, and rhamnitol.

[0482] (iii) Monosaccharides such as arabinose, ribose, xylose, glucose, mannose, galactose, fructose, sorbitol, rhamnose, fucose and deoxyribose.

[0483] (iv) Disaccharides such as trehalose, sucrose, maltose, cellobiose, gentiobiose, lactose and melibiose.

[0484] (v) trisaccharides such as raffinose, gentiotriose and melezitose.

[0485] (vi) Tetrasaccharides such as stachyose.

[0486] 3. Acrylic polyol

[0487] The acrylic polyol is not particularly limited, and examples thereof include acrylic polyols obtained by copolymerizing an ethylenically unsaturated bond-containing monomer having a hydroxyl group, alone or in mixture, and other ethylenically unsaturated bond-containing monomers copolymerizable therewith, alone or in mixture.

[0488] The monomer containing an ethylenically unsaturated bond having a hydroxyl group is not particularly limited, and examples thereof include hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxybutyl acrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, hydroxybutyl methacrylate, etc. These monomers may be used alone or in combination of two or more thereof. Among them, hydroxyethyl acrylate or hydroxyethyl methacrylate is preferred.

[0489] Examples of other ethylenically unsaturated bond-containing monomers copolymerizable with the above monomers include the following (1) to (6), etc. These monomers can be used alone or in combination of two or more.

[0490] (1) Acrylates such as methyl acrylate, ethyl acrylate, propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, n-hexyl acrylate, cyclohexyl acrylate, 2-ethylhexyl acrylate, lauryl acrylate, benzyl acrylate and phenyl acrylate.

[0491] (2) Methacrylates such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-hexyl methacrylate, cyclohexyl methacrylate, 2-ethylhexyl methacrylate, lauryl methacrylate, benzyl methacrylate and phenyl methacrylate.

[0492] (3) Unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, and itaconic acid.

[0493] (4) Unsaturated amides such as acrylamide, methacrylamide, N,N-methylenebisacrylamide, diacetone acrylamide, diacetone methacrylamide, maleamide, maleimide, etc.

[0494] (5) Vinyl monomers such as glycidyl methacrylate, styrene, vinyl toluene, vinyl acetate, acrylonitrile, and dibutyl fumarate.

[0495] (6) Vinyl monomers having a hydrolyzable silyl group, such as vinyltrimethoxysilane, vinylmethyldimethoxysilane, and γ-(meth)acryloxypropyltrimethoxysilane.

[0496] 4. Polyolefin polyols

[0497] The polyolefin polyol is not particularly limited, and examples thereof include polybutadiene having two or more hydroxyl groups, hydrogenated polybutadiene having two or more hydroxyl groups, polyisoprene having two or more hydroxyl groups, and hydrogenated polyisoprene having two or more hydroxyl groups.

[0498] The number of hydroxyl groups statistically present in one molecule of the polyol (hereinafter sometimes referred to as the "average number of hydroxyl groups") is preferably 2 or more. When the average number of hydroxyl groups of the polyol is 2 or more, there is a tendency to further suppress the reduction in the crosslinking density of the coating film obtained by curing the one-component coating composition of the present embodiment.

[0499] 5. Fluorinated polyols

[0500] In this specification, "fluoropolyol" refers to a polyol containing fluorine in the molecule. Specifically, examples of fluoropolyol include copolymers such as fluoroolefins, cyclovinyl ethers, hydroxyalkyl vinyl ethers, and monocarboxylic acid vinyl esters disclosed in Japanese Patent Application Laid-Open No. 57-34107 (Reference 1) and Japanese Patent Application Laid-Open No. 61-275311 (Reference 2).

[0501] 6. Polycarbonate polyol

[0502] The polycarbonate polyols are not particularly limited, and examples thereof include the polycarbonate polyols described in (1) to (4) below.

[0503] (1) Dialkyl carbonates such as dimethyl carbonate.

[0504] (2) Alkylene carbonates such as ethylene carbonate.

[0505] (3) Diaryl carbonates such as diphenyl carbonate.

[0506] (4) Polycarbonate polyols obtained by polycondensing low molecular weight carbonate compounds such as those described in (1) to (3) above.

[0507] 7. Polyurethane polyol

[0508] The polyurethane polyol is not particularly limited, and can be obtained, for example, by reacting a polyol not containing a carboxyl group with an isocyanate component by a conventional method.

[0509] Examples of the polyol not containing a carboxyl group include low molecular weight polyols not containing a carboxyl group such as ethylene glycol and propylene glycol, and examples of high molecular weight polyols not containing a carboxyl group include acrylic polyols, polyester polyols, and polyether polyols.

[0510] (Hydroxy value of polyol)

[0511] The hydroxyl value of the resin per unit amount of the polyol is not particularly limited, but is preferably 10 mgKOH / resin g or more and 300 mgKOH / resin g or less.

[0512] By the hydroxyl value of the resin per unit amount being above the above lower limit, the crosslinking density is suppressed from reducing, and there is a tendency that the physical property of the target can be more fully achieved. By the hydroxyl value of the resin per unit amount being below the above upper limit, the crosslinking density is suppressed from excessively increasing, and there is a tendency that the mechanical physical property of the coating film obtained by curing the one-component type coating composition of the present embodiment can be further improved.

[0513] In addition, the hydroxyl value of a polyol can be measured according to JIS K1557.

[0514] (Polyamine)

[0515] The polyamine is not particularly limited, but preferably has two or more primary or secondary amino groups in one molecule, and more preferably has three or more primary or secondary amino groups in one molecule.

[0516] Specific examples of the polyamine include the polyamines shown in the following (1) to (3).

[0517] (1) Diamines such as ethylenediamine, propylenediamine, butylenediamine, triethylenediamine, hexamethylenediamine, 4,4'-diaminodicyclohexylmethane, piperazine, 2-methylpiperazine, and isophoronediamine;

[0518] (2) Chain polyamines having three or more amino groups, such as hexamethylenetriamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentamethylenehexamine, and tetrapropylenepentamine;

[0519] (3) Cyclic polyamines such as 1,4,7,10,13,16-hexaazacyclooctadecane, 1,4,7,10-tetraazacyclodecane, 1,4,8,12-tetraazacyclopentadecane, and 1,4,8,11-tetraazacyclotetradecane.

[0520] (Alkanolamine)

[0521] In this specification, "alkanolamine" refers to a compound having an amino group and a hydroxyl group in one molecule.

[0522] Specific examples of the alkanolamine include monoethanolamine, diethanolamine, aminoethylethanolamine, N-(2-hydroxypropyl)ethylenediamine, mono-, di-(n- or iso-)propanolamine, ethylene glycol-bis-propylamine, neopentanolamine, and methylethanolamine.

[0523] [Other urethanization catalysts]

[0524] The two-component coating composition kit of the present embodiment may further include another urethanization catalyst within a range that does not adversely affect storage stability.

[0525] The urethanization catalyst may be a basic compound or a Lewis acidic compound.

[0526] Examples of the basic compound include metal hydroxides, metal alkoxides, metal acetylacetonates, hydroxides of onium salts, halides of onium salts, metal salts of active methylene compounds, onium salts of active methylene compounds, aminosilanes, amines, phosphines, etc. The onium salt is preferably an ammonium salt, a phosphonium salt or a sulfonium salt.

[0527] Examples of the Lewis acidic compound include organic tin compounds, organic zinc compounds, organic titanium compounds, and organic zirconium compounds.

[0528] [Other resin components]

[0529] The two-component coating composition kit of the present embodiment may further include other resin components such as existing melamine resin, epoxy resin, and polyurethane resin as necessary.

[0530] [Other additives]

[0531] When the two-component coating composition kit of this embodiment has a polyol having a carboxyl group, it may also have other curing agents such as oxazoline group-containing compounds and carbodiimide group-containing compounds as a curing agent component. These compounds may be contained alone or in combination of two or more.

[0532] When the two-component coating composition kit of this embodiment includes a polyol having a carbonyl group, it may further include other curing agents such as a hydrazide group-containing compound and a semicarbazide group-containing compound as a curing agent component. These compounds may be contained alone or in combination of two or more.

[0533] The two-component coating composition kit of the present embodiment may further include other additives such as an antioxidant, an ultraviolet absorber (light stabilizer), a pigment, a metal powder pigment, a rheology control agent, a curing accelerator, a surfactant, and a solvent, as needed.

[0534] Examples of the antioxidant, the light stabilizer, the surfactant, and the solvent include the same examples as those exemplified in the above-mentioned blocked polyisocyanate composition.

[0535] Examples of the pigment include titanium oxide, carbon black, indigo, quinacridone, and pearl mica.

[0536] Examples of the metal powder pigment include aluminum and the like.

[0537] Examples of the rheology control agent include hydroxyethyl cellulose, urea compounds, and microgels.

[0538] Examples of the curing accelerator include organic metal compounds other than the above-mentioned urethanization catalysts. Examples of the metal species constituting the organic metal compound include tin, zinc, and lead.

[0539] <(Solvent-based / water-based) one-component coating composition>

[0540] The solvent-based one-component coating composition of the present embodiment contains the above-mentioned encapsulated thermal latent catalyst and a polyurethane curing agent containing a blocked polyisocyanate, and a polyvalent active hydrogen compound.

[0541] The water-based one-component coating composition of the present embodiment includes a polyurethane curing agent containing the above-mentioned encapsulated thermal latent catalyst and a water-dispersible hydrophilic blocked polyisocyanate, and a polyvalent active hydrogen compound.

[0542] Examples of the polyvalent active hydrogen compound include the same polyvalent active hydrogen compounds as exemplified in the above-mentioned "kit for two-component coating composition".

[0543] The solvent-based or water-based one-component coating composition of the present embodiment may further include other urethanization catalysts within the range that does not adversely affect storage stability. Other urethanization catalysts include the same examples as those exemplified in the above-mentioned "two-component coating composition".

[0544] The solvent-based or water-based one-component coating composition of the present embodiment may further include other resin components and other additives. As other resin components and other additives, examples identical to those exemplified in the above-mentioned "two-component coating composition" may be cited.

[0545] <Method for producing coating composition>

[0546] The two-component coating composition of the present embodiment is obtained by mixing the polyurethane curing agent and the polyvalent active hydrogen compound, and other resin components and other additives as required, which are included in the two-component coating composition kit, using a known method.

[0547] The solvent-based one-component coating composition of the present embodiment first adds other resin components, other additives, etc. to the polyvalent active hydrogen compound or its solvent dilution as needed. Then, the above-mentioned polyurethane curing agent is added, and a solvent is also added as needed to adjust the viscosity. Then, the solvent-based one-component coating composition can be obtained by stirring by hand or a stirring machine such as MAZELAR.

[0548] The viscosity is preferably adjusted to a drop time of about 13 to 30 seconds, preferably about 16 to 25 seconds, when measured at 23° C. using Ford cup No. 4 according to ASTM D-1200.

[0549] Alternatively, the solvent-based one-component coating composition of the present embodiment first adds other resin components, other additives, etc. to a polyvalent active hydrogen compound or its solvent dilution as required. Then, the above-mentioned blocked polyisocyanate is added, and a solvent is also added as required to adjust the viscosity. Then, hand stirring or a stirring machine such as MAZELAR is used to stir. Then, the above-mentioned encapsulated thermal latent catalyst is added under stirring, and then stirred, so that a solvent-based one-component coating composition can be obtained.

[0550] The water-based one-component coating composition of the present embodiment first adds other resin components, other additives, etc. to the polyvalent hydroxy compound or its aqueous dispersion or water-soluble substance as needed. Then, the above-mentioned polyurethane curing agent is added, and water and solvent are also added as needed to adjust the viscosity. Then, a stirring machine is used for forced stirring to obtain the water-based one-component coating composition.

[0551] The viscosity is preferably adjusted to a drop time of about 15 to 30 seconds, preferably about 18 to 25 seconds, when measured at 23° C. using a Ford cup No. 4 according to ASTM D-1200.

[0552] Or, the water-based one-component coating composition of the present embodiment first adds other resin components, other additives, etc. as required to polyvalent active hydrogen compounds or their aqueous dispersions or water-solubles. Then add the above-mentioned hydrophilic blocked polyisocyanate or its aqueous dispersion, and also add water, solvent as required to adjust viscosity. Then utilize a stirring machine to force stirring. Then add the above-mentioned encapsulated thermal latent catalyst under stirring, and then stir, thus can obtain the water-based one-component coating composition.

[0553] <Application>

[0554] The coating composition of this embodiment can be applied by roller coating, curtain flow coating, spray coating, electrostatic coating, bell coating, dipping, roller coating, brush coating, etc., and can be suitably used as a primer, middle coating or top coating on metals such as steel plates and surface-treated steel plates, plastics, inorganic materials such as ceramics, glass, and concrete.

[0555] The coating composition of the present embodiment is suitably used to impart aesthetic properties, weather resistance, acid resistance, rust resistance, chipping resistance, adhesion, etc. to pre-coated metals including rust-proof steel sheets, automobile coatings, plastic coatings, and the like.

[0556] Furthermore, the coating composition of the present embodiment is also useful as an adhesive, a pressure-sensitive adhesive, an elastomer, a foam, a surface treatment agent, and the like.

[0557] 《Coating》

[0558] The coating film of the present embodiment is formed by curing the above-mentioned coating composition. The coating film of the present embodiment has excellent low-temperature curability and scratch resistance. The coating film of the present embodiment is obtained by applying the above-mentioned coating composition by a known method such as roller coating, curtain flow coating, spray coating, bell coating, electrostatic coating, etc., and curing after drying at room temperature or sintering process.

[0559] The coating film obtained by curing the coating composition has a urethane bond. Therefore, the coating film of the present embodiment formed from the coating composition tends to be excellent in chemical resistance, heat resistance, water resistance, etc., which are characteristics of a general urethane cross-linked coating film.

[0560] 《Painted Items》

[0561] The coated article of the present embodiment includes the above-mentioned coating film. The coated article of the present embodiment has excellent low-temperature curability and abrasion resistance by including the above-mentioned coating film.

[0562] The coated article of the present embodiment includes the above-mentioned coating film having excellent chemical resistance, heat resistance, water resistance, etc., and is further endowed with aesthetic properties, acid resistance, rust resistance, chipping resistance, adhesion, etc.

[0563] Example

[0564] The present invention will be described below using examples, but the present invention is not limited to the following examples.

[0565] The following describes the methods of measuring various physical properties and evaluating various properties. It should be noted that, unless otherwise specified, "parts" and "%" refer to "parts by mass" and "mass %".

[0566] <Measurement method and evaluation method>

[0567] [Physical properties 1]

[0568] (Isocyanate group (NCO) content of polyisocyanate)

[0569] Accurately weigh more than 1g and less than 3g of polyisocyanate in a conical flask (Wg). Then add 20mL of toluene to dissolve the polyisocyanate. Then, add 10mL of 2N di-n-butylamine toluene solution, mix, and leave at room temperature for 15 minutes. Then, add 70mL of isopropanol and mix. Then, titrate the liquid into the indicator using 1N hydrochloric acid solution (factor F). The obtained titration value is set to V2mL. Then perform the same operation without polyisocyanate, and the obtained titration value is set to V1ml. Then calculate the isocyanate group (NCO) content of the polyisocyanate by the following formula.

[0570] NCO content (mass %) = (V1-V2) × F × 42 / (W × 1000) × 100

[0571] [Physical Properties 2]

[0572] (Solid content of blocked polyisocyanate composition)

[0573] The solid content of the blocked polyisocyanate composition is determined as follows.

[0574] First, accurately weigh an aluminum pan with a bottom diameter of 38 mm. Next, accurately weigh the blocked polyisocyanate composition (W1) manufactured in the examples and comparative examples while placing about 1 g on the aluminum pan. Next, adjust the blocked polyisocyanate composition to a uniform thickness. Next, keep the blocked polyisocyanate composition placed on the aluminum pan in an oven at 105°C for 1 hour. Next, after the aluminum pan reaches room temperature, accurately weigh the blocked polyisocyanate composition (W2) remaining on the aluminum pan. Next, calculate the solid content of the blocked polyisocyanate composition of the polyisocyanate by the following formula.

[0575] Solid content of blocked polyisocyanate composition [mass %] = W2 / W1×100

[0576] [Physical Properties 3]

[0577] (Effective isocyanate group (NCO) content of blocked polyisocyanate composition)

[0578] The effective isocyanate group (NCO) content of the blocked polyisocyanate composition is determined as follows.

[0579] The “effective isocyanate group (NCO) content” referred to herein refers to a value expressed as mass % of isocyanate groups obtained by quantifying the amount of blocked isocyanate groups that can participate in the crosslinking reaction in the blocked polyisocyanate composition after the blocking reaction.

[0580] The effective NCO content is calculated by the following formula: In the following formula, "NCO%" and "solid content of blocked polyisocyanate composition" are the values ​​calculated in the above-mentioned physical properties 1 and physical properties 2, respectively. When the sample is diluted with a solvent or the like, the value in the diluted state is calculated.

[0581] Effective NCO content [mass %] = [(solid content of blocked polyisocyanate composition [mass %]) × {(mass of polyisocyanate used in blocking reaction) × NCO %}] / (mass of blocked polyisocyanate composition after blocking reaction)

[0582] [Physical Properties 4]

[0583] (Median particle size D of encapsulated thermal latent catalyst 50 )

[0584] The resulting encapsulated thermal latent catalyst was diluted to 1% by mass with ion exchange water and measured for a median particle size D using UPA-EX150 (manufactured by Microtrac BEL Corp.). 50 .

[0585] [Evaluation 1]

[0586] (Low-temperature curing properties of two-component coating compositions)

[0587] Each two-component coating composition manufactured in the embodiment and the comparative example is applied to a polypropylene (PP) plate using an air spray gun in a dry film thickness of 30 μm. Then, dry at 23°C for 15 minutes. Then, sinter at 60°C for 60 minutes to obtain a cured coating film. The obtained cured coating film is placed at 23°C for 1 hour and peeled off from the PP plate. Then, after accurately weighing the mass (hereinafter referred to as the "mass before immersion"), immerse in acetone at 20°C for 24 hours. Then, accurately weigh the mass after immersion (hereinafter referred to as the "mass of the undissolved portion"). Then, calculate the ratio of the mass of the undissolved portion to the mass before immersion (gel fraction). Then, for the calculated gel fraction, evaluate the low-temperature curing property based on the following evaluation criteria.

[0588] (Evaluation Criteria)

[0589] A: Gel fraction is 80% by mass or more

[0590] B: Gel fraction is 50 mass % or more and less than 80 mass %

[0591] C: Gel fraction less than 50% by mass

[0592] [Evaluation 2]

[0593] (Storage stability of two-component coating composition)

[0594] Each of the obtained two-component coating compositions was diluted with butyl acetate, and the initial drop time in Ford Cup No. 4 at 23° C. was adjusted to 15 seconds for the initial viscosity. Then, the compositions were stored at 23° C., the viscosity was measured every 0.5 hours, the time when the drop speed in Ford Cup No. 4 exceeded 30 seconds was measured, and the storage stability was evaluated based on the following evaluation criteria.

[0595] (Evaluation Criteria)

[0596] A: More than 3 hours

[0597] B: 2 hours or more and less than 3 hours

[0598] C: Less than 2 hours

[0599] [Evaluation 3]

[0600] (Low-temperature curing property of one-component coating composition)

[0601] Each one-component coating composition manufactured in the embodiment and the comparative example is applied to a polypropylene (PP) plate using an air spray gun in a dry film thickness of 30 μm. Then, dry at 23°C for 15 minutes. Then, sinter at a specified temperature for 30 minutes to obtain a cured coating film. The obtained cured coating film is placed at 23°C for 1 hour and peeled off from the PP plate. Then, after accurately weighing the mass (hereinafter referred to as the "mass before immersion"), immerse in acetone at 20°C for 24 hours. Then accurately weigh the mass after immersion (hereinafter referred to as the "mass of the undissolved portion"). Then, calculate the ratio of the mass of the undissolved portion to the mass before immersion (gel fraction). Then, for the calculated gel fraction, evaluate the low-temperature curing property based on the following evaluation criteria.

[0602] (Evaluation Criteria)

[0603] A: Gel fraction at 100°C is 80% by mass or more

[0604] B: Gel fraction at 110°C is 80% by mass or more

[0605] C: Gel fraction at 110°C is less than 80% by mass

[0606] [Evaluation 4]

[0607] (Storage stability of one-component coating composition)

[0608] The storage stability of each one-component coating composition was evaluated based on the following evaluation criteria regarding its appearance after being stored at 40° C. for 10 days.

[0609] (Evaluation Criteria)

[0610] A: No major changes were found.

[0611] B: Even but thickening or obvious separation is found

[0612] C: Gelation

[0613] [Evaluation 5]

[0614] (Abrasion resistance)

[0615] Each two-component coating composition or each one-component coating composition manufactured in the examples and comparative examples was applied to a polypropylene (PP) plate using an air spray gun in a dry film thickness of 30 μm. Then, it was dried at 23°C for 15 minutes. Then, it was sintered at 110°C for 30 minutes to obtain a cured coating film. For each obtained coating film, the initial gloss (gloss) (G0) was first measured. Then, on the coating surface (the portion where the initial gloss (gloss) (G0) was measured), a 4-row brass brush made by Industry Kowa was used to form defects by reciprocating 20 times in parallel with the handle with a weight of 600 g, a stroke speed of 30 cm / second, and a stroke width of 5 cm.

[0616] The sample used in the scratch resistance evaluation was then placed in a constant temperature room at 23°C for 24 hours. After 24 hours, the gloss (G1) of the scratched portion was measured. The gloss retention was calculated using the following formula, and the scratch resistance was evaluated according to the following evaluation criteria.

[0617] Gloss retention rate [%] = (G1 / G0) × 100

[0618] (Evaluation Criteria)

[0619] A: Gloss retention rate is more than 90%

[0620] B: Gloss retention rate is 80% or more and less than 90%

[0621] C: Gloss retention rate is less than 80%

[0622] <Synthesis of polyisocyanate>

[0623] [Synthesis Example 1-1]

[0624] (Synthesis of polyisocyanate P-1)

[0625] In a four-necked flask equipped with a thermometer, a stirring blade and a reflux condenser, 1000 parts by mass of HDI and 2 parts by mass of 2-ethylhexane-1,3-diol were added under a nitrogen flow, and the temperature in the reactor was kept at 70°C while stirring. Tetramethylammonium hydroxide was added thereto, and phosphoric acid was added to stop the reaction when the NCO content of the reaction solution at 25°C reached 38.7% by mass. After filtering the reaction solution, unreacted HDI was removed using a thin film distillation apparatus to obtain a polyisocyanate P-1 having an NCO content of 21.8% by mass.

[0626] [Synthesis example 1-2]

[0627] (Synthesis of Water-Dispersible Polyisocyanate P-2)

[0628] In a four-necked flask equipped with a thermometer, a stirring blade and a reflux condenser, 15.5 parts by mass of polyethylene glycol monomethyl ether having an average number of ethylene oxide repeating units of 9.0 (manufactured by Nippon Emulsifier Co., Ltd., trade name "MPG-130") was added to 100 parts by mass of the polyisocyanate P-1 obtained in Synthesis Example 1-1 under a nitrogen stream, and the mixture was stirred at 100° C. for 4 hours for reaction. After the reaction was completed, a water-dispersible polyisocyanate P-2 having an NCO content of 17.5% by mass was obtained.

[0629] [Synthesis Example 1-3]

[0630] (Synthesis of Water-Dispersible Polyisocyanate P-3)

[0631] In a four-necked flask equipped with a thermometer, a stirring blade and a reflux condenser, 100 parts by mass of isophorone diisocyanate-based polyisocyanurate (manufactured by Evonik Industries, trade name "T1890 / 100"), 64 parts by mass of dipropylene glycol dimethyl ether (manufactured by Dow Chemical Company, trade name "DMM"), and 12.3 parts by mass of polyethylene glycol monomethyl ether having an average number of ethylene oxide repeating units of 9.0 (manufactured by Nippon Emulsifier Co., Ltd., trade name "MPG-130") were added under a nitrogen stream, and the mixture was stirred at 100° C. for 4 hours for reaction. After the reaction was completed, a water-dispersible polyisocyanate P-3 having an NCO content of 9.1% by mass was obtained.

[0632] <Synthesis of blocked polyisocyanate composition>

[0633] [Synthesis example 2-1]

[0634] (Manufacture of Blocked Polyisocyanate Composition BL-1)

[0635] A nitrogen atmosphere was formed in a four-necked flask equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen blowing tube, and 17.8 parts by mass of 1,2,4-triazole was slowly added to 100 parts by mass of the polyisocyanate P-1 obtained in Synthesis Example 1-1, and the mixture was stirred for 3 hours under a temperature condition of 100° C. to 110° C. Subsequently, after the liquid temperature was lowered to 60° C. or less, 53.5 parts by mass of diisopropyl malonate and 106.1 parts by mass of propylene glycol monomethyl ether acetate (PMA) were added, and a methanol solution containing sodium methoxide (28% by mass) was further added in an amount of 0.05% by mass relative to the solid content and sodium in the reaction solution, and the mixture was reacted at 75° C. to 80° C. for 2 hours to obtain a blocked polyisocyanate composition BL-1.

[0636] [Synthesis example 2-2]

[0637] (Manufacture of Blocked Polyisocyanate Composition BL-2)

[0638] A nitrogen atmosphere was formed in a four-necked flask equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen blowing tube, and 17.8 parts by mass of 1,2,4-triazole was slowly added to 100 parts by mass of the polyisocyanate P-1 obtained in Synthesis Example 1-1, and the mixture was stirred for 3 hours under a temperature condition of 100° C. to 110° C. Then, after the liquid temperature was lowered to 80° C. or less, 26.0 parts by mass of 3,5-dimethylpyrazole and 93.9 parts by mass of PMA were added, and a methanol solution containing sodium methoxide (28% by mass) was further added in an amount of 0.05% by mass relative to the solid content and sodium in the reaction solution, and the mixture was reacted at 75° C. to 80° C. or less for 2 hours to obtain a blocked polyisocyanate composition BL-2.

[0639] [Table 1]

[0640]

[0641] <Synthesis of Hydrophilic Blocked Polyisocyanate Composition>

[0642] [Synthesis example 2-3]

[0643] (Production of Hydrophilic Blocked Polyisocyanate Composition BL-3)

[0644] A nitrogen atmosphere was formed in a four-necked flask equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen blowing tube, 100 parts by mass of the polyisocyanate P-1 obtained in Synthesis Example 1-1 and 35.7 parts by mass of methoxypolyethylene glycol (MPG-081, 15 ethylene oxide repeating units, manufactured by Nippon Emulsifier Co., Ltd.) were added, and the mixture was heated to 120° C. and maintained for 2 hours while stirring. Next, the reaction solution was cooled to about 110° C. or less, 16.0 parts by mass of 1,2,4-triazole was slowly added, and the mixture was stirred for 3 hours at a temperature of 100° C. or more and 110° C. or less to carry out the reaction. Next, after the liquid temperature was lowered to below 60°C, 48.1 parts by mass of diisopropyl malonate and 125.9 parts by mass of PMA were added, and a methanol solution containing sodium methoxide (28% by mass) was added in an amount of 0.05% by mass relative to the solid content and sodium in the reaction solution, and the mixture was reacted at 75°C to 80°C for 2 hours to obtain a hydrophilic blocked polyisocyanate composition BL-3.

[0645] [Table 2]

[0646]

[0647] <Manufacturing of encapsulated thermal latent catalyst>

[0648] [Example 1-1]

[0649] (Manufacturing of Encapsulated Thermal Latent Catalyst Aqueous Dispersion C-1 and Encapsulated Thermal Latent Catalyst Butyl Acetate Dispersion C-1SB)

[0650] In a four-necked flask equipped with a stirrer, a thermometer, and a reflux condenser, 10 parts by mass of ion exchange water and 0.25 parts by mass of anionic surfactant (manufactured by Nippon Emulsifier Co., Ltd., product name "Newcol N2320-SN") (hereinafter sometimes referred to as "N2320-SN") were added and stirred to prepare a reaction system. Next, 1.0 parts by mass of polyaspartic acid ester compound (manufactured by Covestro, trade name "Desmophen 1420", amine value 201 mgKOH / resin g) (hereinafter sometimes referred to as "D1420"), 5.0 parts by mass of toluene, and 1.0 parts by mass of dioctyltin dilaurate (manufactured by Nitto Chemical Industry Co., Ltd., trade name "NEOSTANN U-810") (hereinafter sometimes referred to as "U-810") were stirred and pre-mixed to obtain an organic mixed solution, and the organic mixed solution was dripped into the reaction system over 5 minutes. After the dripping was completed, the mixture was stirred for 5 minutes to disperse the organic mixed solution in water. Then, 1.4 parts by weight of the water-dispersible polyisocyanate P-3 obtained in Synthesis Example 1-3 was added dropwise over 10 minutes. After the addition was completed, the mixture was stirred for 5 minutes to obtain an encapsulated thermal latent catalyst aqueous dispersion C-1 (solid content: 30% by weight). The median particle size of the encapsulated thermal latent catalyst contained in the obtained encapsulated thermal latent catalyst aqueous dispersion C-1 was 90 nm.

[0651] Then, ion exchange water was added to the obtained encapsulated thermal latent catalyst aqueous dispersion C-1, and the solid content was diluted to 10% by mass. The centrifuge was applied at 50000 rpm × 30 minutes to separate the aqueous layer and the encapsulated thermal latent catalyst. The obtained encapsulated thermal latent catalyst was dried using a vacuum dryer at 30°C, 10 hours, and a vacuum degree of 0.1 Torr. Then, butyl acetate: 23 parts by mass was added to the obtained dried encapsulated thermal latent catalyst: 10 parts by mass, and stirred for 10 minutes to obtain an encapsulated thermal latent catalyst butyl acetate dispersion C-1SB (solid content: 30% by mass).

[0652] [Example 1-2]

[0653] (Manufacturing of Encapsulated Thermal Latent Catalyst Aqueous Dispersion C-2 and Encapsulated Thermal Latent Catalyst Butyl Acetate Dispersion C-2SB)

[0654] Into a four-necked flask equipped with a stirrer, a thermometer, and a reflux condenser, 10 parts by mass of ion exchange water and 0.25 parts by mass of N2320-SN were added and stirred to prepare a reaction system. Next, 1.0 parts by mass of D1420, 1.0 parts by mass of toluene, and 4.0 parts by mass of a 2-ethylhexanoic acid solution containing 25% by mass of bismuth 2-ethylhexanoate (manufactured by Nitto Kasei Co., Ltd., product name "NEOSTANN U-600") (hereinafter sometimes referred to as "U-600") were stirred and pre-mixed to obtain an organic mixed solution, which was dripped into the reaction system over 5 minutes. After the dripping was completed, the organic mixed solution was stirred for 5 minutes to disperse the organic mixed solution in water. Then, 1.1 parts by mass of the water-dispersible polyisocyanate P-2 obtained in Synthesis Example 1-2 was dripped over 10 minutes. After the dripping was completed, the solution was stirred for 5 minutes to obtain an encapsulated thermal latent catalyst aqueous dispersion C-2 (solid content: 30% by mass). The median particle size of the encapsulated thermal latent catalyst contained in the obtained encapsulated thermal latent catalyst aqueous dispersion C-2 was 110 nm.

[0655] Then, ion exchange water was added to the obtained encapsulated thermal latent catalyst aqueous dispersion C-2, and the solid content was diluted to 10% by mass. The centrifuge was applied at 50000 rpm × 30 minutes to separate the aqueous layer and the encapsulated thermal latent catalyst. The obtained encapsulated thermal latent catalyst was dried using a vacuum dryer at 30°C, 10 hours, and a vacuum degree of 0.1 Torr. Then, butyl acetate: 23 parts by mass was added to the obtained dried encapsulated thermal latent catalyst: 10 parts by mass, and stirred for 10 minutes to obtain an encapsulated thermal latent catalyst butyl acetate dispersion C-2SB (solid content: 30% by mass).

[0656] [Examples 1-3]

[0657] (Manufacturing of Encapsulated Thermal Latent Catalyst Aqueous Dispersion C-3 and Encapsulated Thermal Latent Catalyst Butyl Acetate Dispersion C-3SB)

[0658] Add ion exchange water: 10 parts by mass and N2320-SN: 0.25 parts by mass to a four-necked flask equipped with a stirrer, a thermometer, and a reflux condenser and stir to prepare a reaction system. Next, stir and pre-mix D1420: 1.0 parts by mass, toluene: 1.0 parts by mass, and U-600: 4.0 parts by mass to obtain an organic mixed solution, and drop the organic mixed solution into the reaction system over 5 minutes. After the dropwise addition is completed, stir for 5 minutes to disperse the organic mixed solution in water. Then, drop the water-dispersible polyisocyanate P-3 obtained in Synthesis Example 1-3: 1.4 parts by mass over 10 minutes. After the dropwise addition is completed, stir for 5 minutes to obtain an encapsulated thermal latent catalyst aqueous dispersion C-3 (solid content: 30% by mass). The median particle size of the encapsulated thermal latent catalyst contained in the obtained encapsulated thermal latent catalyst aqueous dispersion C-3 is 82nm.

[0659] Then, ion exchange water was added to the obtained encapsulated thermal latent catalyst aqueous dispersion C-3, and the solid content was diluted to 10% by mass. The centrifuge was applied at 50000 rpm × 30 minutes to separate the aqueous layer and the encapsulated thermal latent catalyst. The obtained encapsulated thermal latent catalyst was dried using a vacuum dryer at 30°C, 10 hours, and a vacuum degree of 0.1 Torr. Then, butyl acetate: 23 parts by mass was added to the obtained dried encapsulated thermal latent catalyst: 10 parts by mass, and stirred for 10 minutes to obtain an encapsulated thermal latent catalyst butyl acetate dispersion C-3SB (solid content: 30% by mass).

[0660] [Table 3]

[0661]

[0662] [Comparative Example 1-1]

[0663] (Manufacturing of Encapsulated Thermal Latent Catalyst Aqueous Dispersion C-4)

[0664] In a four-necked flask equipped with a stirrer, a thermometer, and a reflux condenser, 10 parts by mass of ion exchange water and 0.25 parts by mass of anionic surfactant (manufactured by Nippon Emulsifier Co., Ltd., product name "Newcol N2320-SN") (hereinafter sometimes referred to as "N2320-SN") were added and stirred to prepare a reaction system. Next, 1.0 parts by mass of toluene, 4.0 parts by mass of a 2-ethylhexanoic acid solution containing 25% by mass of bismuth 2-ethylhexanoate (manufactured by Nitto Kasei Co., Ltd., product name "NEOSTANN U-600") (hereinafter sometimes referred to as "U-600"), and 1.0 parts by mass of diisononylcyclohexane-1,2-dicarboxylate were pre-mixed to obtain an organic mixed solution, and the organic mixed solution was added dropwise to the reaction system over 5 minutes. After the dropwise addition is completed, 0.05 parts by mass of 1,4-butanediol diacrylate, 0.25 parts by mass of methyl methacrylate, and 0.2 parts by mass of methacrylic anhydride are mixed in advance and added dropwise over 5 minutes. Then, the mixture is stirred for 40 minutes to form a stable emulsion. Then, 0.01 parts by mass of tert-butyl peroxy neodecanoate is added, and the mixture is heated to 75°C over 180 minutes and then maintained for 60 minutes. Then, 0.05 parts by mass of a 10% aqueous solution of tert-butyl hydroperoxide is added, and while cooling to 20°C, 0.13 parts by mass of a 3.85% aqueous solution of ascorbic acid is added over 60 minutes to obtain an encapsulated thermal latent catalyst aqueous dispersion C-4 (solid content: 20% by mass). The median particle size of the encapsulated thermal latent catalyst in the obtained encapsulated thermal latent catalyst aqueous dispersion C-4 is 2500 nm.

[0665] <Production of solvent-based two-component coating composition>

[0666] [Example 2-1]

[0667] (Manufacture of solvent-based two-component coating composition T-a1)

[0668] 10.0 parts by mass of acrylic polyol (manufactured by Allnex, "Setalux 1903" (trade name), hydroxyl concentration 4.5% by mass (resin basis), solid content concentration 75% by mass), 3.9 parts by mass of polyisocyanate P-1 obtained in Synthesis Example 1-1, and 8.3 parts by mass of butyl acetate were mixed and stirred. Then, 0.66 parts by mass of encapsulated heat latent catalyst butyl acetate dispersion C-1SB (solid content: 30% by mass) was added under stirring, and stirred for 5 minutes to obtain a solvent-based two-component coating composition T-a1.

[0669] [Example 2-2 and Comparative Examples 2-1 to 2-3]

[0670] (Manufacturing of solvent-based two-component coating compositions T-a2 and T-b1 to T-b3)

[0671] Each solvent-based two-component coating composition was produced by the same method as in Example 2-1 except that the composition and the blending amount were as shown in Table 4.

[0672] [Table 4]

[0673]

[0674] As can be seen from Table 4, the solvent-based two-component coating compositions T-a1 to T-a2 (Examples 2-1 to 2-2) containing an encapsulated thermal latent catalyst have good storage stability, low-temperature curing properties, and scratch resistance when forming a coating film.

[0675] On the other hand, the solvent-based two-component coating compositions T-b1 and T-b2 (Comparative Examples 2-1 and 2-2) to which a non-encapsulated catalyst was added had good low-temperature curing properties but poor storage stability.

[0676] In addition, the solvent-based two-component coating composition T-b3 (Comparative Example 2-3) to which no catalyst was added had good storage stability, but poor low-temperature curability and poor scratch resistance when forming a coating film.

[0677] <Manufacturing of solvent-based one-component coating composition>

[0678] [Example 2-3]

[0679] (Manufacture of solvent-based one-component coating composition T-a3)

[0680] 10.0 parts by mass of acrylic polyol (manufactured by Allnex, "Setalux 1767" (trade name), hydroxyl concentration 4.5% by mass (resin basis), solid content concentration 65% by mass), 8.7 parts by mass of the blocked polyisocyanate composition BL-1 obtained in Synthesis Example 2-1, and 2.9 parts by mass of butyl acetate were mixed and stirred. Then, 2.8 parts by mass of encapsulated heat latent catalyst butyl acetate dispersion C-3SB (solid content: 30% by mass) was added under stirring, and stirred for 5 minutes to obtain a solvent-based one-component coating composition T-a3 containing a polyurethane-based curing agent.

[0681] [Examples 2-4 to 2-5 and Comparative Examples 2-4 to 2-5]

[0682] (Manufacture of solvent-based one-component coating compositions T-a4 to T-a5 and T-b4 to T-b5)

[0683] Each solvent-based one-component coating composition was produced by the same method as in Example 2-3 except that the composition and the blending amount were as shown in Table 5.

[0684] [Table 5]

[0685]

[0686] As can be seen from Table 5, the solvent-based one-component coating compositions T-a3 to T-a5 (Examples 2-3 to 2-5) containing a polyurethane curing agent have good storage stability, low-temperature curability, and scratch resistance when forming a coating film.

[0687] In addition, for the solvent-based one-component coating compositions T-a3 and T-a5 (Examples 2-3 and 2-5) having different contents of encapsulated thermal latent catalysts, it was found that the lower the content of the encapsulated thermal latent catalyst, the better the low-temperature curing property and the scratch resistance when the coating film is formed.

[0688] On the other hand, the solvent-based one-component coating composition T-b4 (Comparative Example 2-4) to which a non-encapsulated catalyst was added had good low-temperature curability but poor storage stability.

[0689] In addition, the solvent-based one-component coating composition T-b5 (Comparative Example 2-5) to which no catalyst was added had good storage stability, but poor low-temperature curability and abrasion resistance when a coating film was formed.

[0690] <Production of water-based one-component coating composition>

[0691] [Example 2-6]

[0692] (Manufacture of water-based one-component coating composition T-a6)

[0693] Add ion exchange water: 2.8 parts by mass, surfactant (manufactured by Japan Emulsifier Co., Ltd., "Newcol2320SN" (trade name)) (hereinafter sometimes referred to as "N2320-SN"): 0.5 parts by mass, and stir with a stirrer. Add 6.0 parts by mass of the blocked polyisocyanate BL-3 manufactured in Synthesis Example 2-3 under stirring. After 5 minutes, add 10.0 parts by mass of acrylic dispersion (manufactured by Allnex, "SETAQUA6515" (trade name), hydroxyl concentration 3.3% by mass (resin basis), solid content concentration 45% by mass) under stirring. Then add 1.95 parts by mass of encapsulated thermal latent catalyst aqueous dispersion C-3 (solid content: 30% by mass) under stirring to obtain a water-based one-component coating composition T-a6 containing a polyurethane curing agent.

[0694] [Examples 2-7 to 2-8 and Comparative Examples 2-6 to 2-9]

[0695] (Manufacture of water-based one-component coating compositions T-a7 to T-a8 and T-b6 to T-b9)

[0696] Each one-component coating composition was produced by the same method as in Example 2-6 except that the composition and the blending amount were as shown in Table 6.

[0697] [Table 6]

[0698]

[0699] As can be seen from Table 6, the water-based one-component coating compositions T-a6 to T-a8 (Examples 2-6 to 2-8) containing a polyurethane curing agent have good storage stability, low-temperature curability, and scratch resistance when forming a coating film.

[0700] In addition, for water-based one-component coating compositions T-a6 and T-a8 (Examples 2-6 and 2-8) having different contents of encapsulated thermal latent catalysts, it was found that the lower the content of the encapsulated thermal latent catalyst, the better the low-temperature curing property and the scratch resistance when the coating film is formed.

[0701] On the other hand, for the water-based one-component coating composition T-b6 (Comparative Example 2-6) to which the catalyst (U-810) without encapsulation is added, although the storage stability is good, the low-temperature curing property and the scratch resistance when forming the coating film are not good. In addition, for the water-based one-component coating composition T-b7 (Comparative Example 2-7) to which the catalyst (U-600) without encapsulation is added, although the storage stability and low-temperature curing property are allowed, the scratch resistance when forming the coating film is not good.

[0702] In addition, although the storage stability of the aqueous one-component coating composition T-b8 (Comparative Example 2-8) to which no catalyst was added was good, the low-temperature curing property and the scratch resistance when the coating film was formed were poor.

[0703] In addition, for the water-based one-component coating composition T-b9 (Comparison Example 2-9) using an encapsulated catalyst encapsulated by an acrylic polymer film, although the storage stability is good, the dispersibility of the encapsulated catalyst in the water-based coating is insufficient, the low-temperature curing property is poor, and it is not a urea film, so the scratch resistance is poor.

[0704] Industrial Applicability

[0705] According to the polyurethane curing agent of the present embodiment, a coating composition with excellent storage stability and low temperature curing property can be obtained, and a coating film with excellent scratch resistance can be obtained. The coating composition of the present embodiment contains the aforementioned polyurethane curing agent, and is excellent in storage stability and low temperature curing property, and a coating film with excellent scratch resistance can be obtained. The coating composition of the present embodiment is suitably used as a primer, a middle coating or a top coating for raw materials such as metals, plastics, and inorganic materials. The coating composition of the present embodiment is suitably used in order to give aesthetics, weather resistance, acid resistance, rust resistance, chipping resistance, adhesion, etc. to the pre-coated metal containing rust-proof steel plate, the coating part of the automobile, the coating part of the plastic, etc. The coating composition of the present embodiment is also useful as a carbamate raw material such as an adhesive, a bonding agent, an elastomer, a foam, a surface treatment agent, etc.

Claims

1. A polyurethane curing agent comprising a first polyisocyanate and an encapsulated thermal latent catalyst, wherein the encapsulated thermal latent catalyst is covered with a polyurea film derived from a polyamine compound and a second polyisocyanate, The content ratio of the first polyisocyanate and the encapsulated thermal latent catalyst when the solid content is 100% by mass, that is, the mass ratio of the first polyisocyanate: the encapsulated thermal latent catalyst is 96:4 to 80:20, The encapsulated thermolatent catalyst comprises a metal compound covered by the polyurea membrane, The content of the metal compound is 10% by mass or more and 40% by mass or less relative to the total mass of the solid content of the encapsulated thermal latent catalyst.

2. The polyurethane curing agent according to claim 1, in, The metal compound is a metal carboxylate or a metal acetylacetonate.

3. The polyurethane curing agent according to claim 1, in, The content of the metal compound is 20% by mass or more and 35% by mass or less relative to the total mass of the solid content of the encapsulated thermal latent catalyst.

4. The polyurethane curing agent according to claim 1 or 2, in, The median particle size of the encapsulated thermal latent catalyst is 10 nm or more and 3 μm or less.

5. The polyurethane curing agent according to claim 1 or 2, in, The median particle size of the encapsulated thermal latent catalyst is 50 nm or more and 200 nm or less.

6. The polyurethane curing agent according to claim 1 or 2, in, The first polyisocyanate is a blocked polyisocyanate derived from a polyisocyanate and a blocking agent.

7. The polyurethane curing agent according to claim 1 or 2, in, The first polyisocyanate is a hydrophilic blocked polyisocyanate derived from a polyisocyanate, a hydrophilic compound and a blocking agent. 8 . A two-component coating composition kit comprising the polyurethane curing agent according to claim 1 and a polyvalent active hydrogen compound.

9. A solvent-based one-component coating composition comprising the polyurethane-based curing agent according to claim 6 and a polyvalent active hydrogen compound.

10. The solvent-based one-component coating composition according to claim 9, in, The mass of the metal compound contained in the encapsulated thermal latent catalyst is 0.01 mass % or more and 10.0 mass % or less relative to the total mass of the solid content of the coating composition.

11. The solvent-based one-component coating composition according to claim 9 or 10, in, The mass of the metal compound contained in the encapsulated thermal latent catalyst is 0.5 mass % or more and 2.0 mass % or less relative to the total mass of the solid content of the coating composition.

12. The solvent-based one-component coating composition according to claim 9 or 10, in, The solid content of the polyvalent active hydrogen compound in the coating composition is 10 mass % or more and 50 mass % or less relative to the total mass of the coating composition.

13. The solvent-based one-component coating composition according to claim 9 or 10, in, The solid content of the polyvalent active hydrogen compound in the coating composition is 23 mass % or more and 35 mass % or less relative to the total mass of the coating composition.

14. A water-based one-component coating composition comprising the polyurethane curing agent according to claim 7 and a polyvalent active hydrogen compound.

15. The water-based one-component coating composition according to claim 14, in, The mass of the metal compound contained in the encapsulated thermal latent catalyst is 0.01 mass % or more and 10.0 mass % or less relative to the total mass of the solid content of the coating composition.

16. The water-based one-component coating composition according to claim 14 or 15, in, The mass of the metal compound contained in the encapsulated thermal latent catalyst is 0.5 mass % or more and 2.0 mass % or less relative to the total mass of the solid content of the coating composition.

17. The water-based one-component coating composition according to claim 14 or 15, in, The solid content of the polyvalent active hydrogen compound in the coating composition is 10 mass % or more and 50 mass % or less relative to the total mass of the coating composition.

18. The water-based one-component coating composition according to claim 14 or 15, in, The solid content of the polyvalent active hydrogen compound in the coating composition is 23 mass % or more and 35 mass % or less relative to the total mass of the coating composition.

19. A coating film formed by curing a two-component coating composition comprising the polyurethane curing agent according to any one of claims 1 to 5 and a polyvalent active hydrogen compound. 20 . A coating film formed by curing the solvent-based one-component coating composition according to claim 9 .

21. A coating film formed by curing the water-based one-component coating composition according to any one of claims 14 to 18. 22 . A coated article comprising the coating film according to claim 19 .

23. An encapsulated thermolatent catalyst covered with a polyurea film derived from a polyamine compound and a second polyisocyanate, The encapsulated thermal latent catalyst comprises a metal compound covered by a polyurea film, wherein the metal compound is a metal carboxylate or a metal acetylacetonate, and the content of the metal compound is 10 mass % or more and 40 mass % or less relative to the total mass of the solid component of the encapsulated thermal latent catalyst.

24. The encapsulated thermal latent catalyst according to claim 23, in, The content of the metal compound is 20% by mass or more and 35% by mass or less relative to the total mass of the solid content of the encapsulated thermal latent catalyst.

25. The encapsulated thermal latent catalyst according to claim 23 or 24, in, The second polyisocyanate is a water-dispersible polyisocyanate.

26. A method for producing an encapsulated thermal latent catalyst, in, The encapsulated thermal latent catalyst comprises a metal compound covered by a polyurea film, wherein the metal compound is a metal carboxylate or a metal acetylacetonate, and the content of the metal compound is 10% by mass or more and 40% by mass or less relative to the total mass of the solid component of the encapsulated thermal latent catalyst. The manufacturing method comprises: A step of mixing a polyamine compound and a metal compound to prepare a mixture; a step of dispersing the mixture in water to prepare a dispersion; and A step of adding a water-dispersible polyisocyanate dropwise to the dispersion to form a polyurea film derived from the polyamine compound and the water-dispersible polyisocyanate by an interfacial polymerization method, and covering the metal compound with the polyurea film.

Citation Information

Patent Citations

  • Curable fluoroolefin copolymer and its production

    JP1986275311A

  • Thermolatently catalysed two-component system

    WO2017182429A1

  • Microcapsule-type latent curing agent for epoxy resin and process for production thereof, and one-pack-type epoxy resin composition and cured product thereof

    CN101802050A

  • Microcapsule type curable resin composition

    CN105555807A

  • Multi-layer coating structure having a thermally latent catalyst

    CN108472684A