Plasmon metal copper-metal oxide composite structure catalyst and method for catalyzing hydrogen production from gas-phase formic acid under visible light at room temperature
Through the plasmon metal copper-metal oxide composite structure catalyst, combined with visible light catalysis, the existing technology problems of difficult catalyst recovery, large environmental impact, and limited precious metal resources have been solved, and efficient, low-cost, and stable gas-phase formic acid has been achieved. For hydrogen production reaction, the catalyst has excellent catalytic activity and stability.
Patent Information
- Application Number
- CN202310355693.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-06
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-04-06
AI Technical Summary
In the existing technology, homogeneous catalysts are difficult to recycle and use a large amount of organic matter in the preparation process, which has a great impact on the environment. However, noble metal catalyst resources are limited and the cost is high, and non-precious metal catalysts are unstable in systems with a pH less than 7. , it is difficult to develop efficient, low-cost, and stable non-precious metal catalysts.
A plasmon metal copper-metal oxide composite structure catalyst is used, which is modified by a metal salt and a copper source, and prepared by H2O2 treatment and vacuum annealing to form a copper-modified oxygen vacancy oxide catalyst, which is combined with visible light catalysis for hydrogen production from gas-phase formic acid.
It achieves high catalytic activity and selectivity for gas-phase formic acid dehydrogenation under mild conditions. The catalyst has good stability and recyclability. The reaction rate is greater than 300mmol/(g·h), the conversion rate is close to 100%, and the selectivity reaches 96.3 %, and the materials are simple and easy to obtain, suitable for large-scale production.
Smart Images

Figure CN116328778B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of copper-based plasma photocatalysts, and in particular relates to a plasmon metal copper-metal oxide composite structure catalyst and a method for catalyzing hydrogen production from gas-phase formic acid under visible light at room temperature. Background Art
[0002] In the current era of dwindling fossil fuel resources and global warming, the search for a sustainable energy source is more urgent than ever. Hydrogen (H2) is a promising intermediate energy storage alternative. Its high energy content and high efficiency make it a solution that can replace fossil fuels as a mobile energy source for transportation. However, traditional hydrogen storage methods have weight, cost and safety issues. As an alternative, chemical hydrogen storage has attracted considerable attention, and formic acid (FA) has become one of the compounds that is promising to achieve this goal. Formic acid is the simplest carboxylic acid. Due to its low toxicity, stability, high mass capacity (4.4wt%) and high volume capacity (53g / L), simple and easy source (formic acid can be easily obtained from biomass oxidation), it is an important hydrogen storage material for mobile applications. Therefore, finding a catalyst for efficient formic acid hydrogen production is crucial in hydrogen storage and application.
[0003] Efficient formic acid hydrogen production catalysts mainly include homogeneous catalysts and heterogeneous catalysts. Formic acid (FA) has attracted people to explore its hydrogen production more than 50 years ago. The homogeneous catalytic system for formic acid hydrogen production began with the study of Pt, Ru and Ir phosphine complexes reported by Coffey in 1967. It was not until the study of Laurenczy and Beller in 2008 that formic acid FA began to be used as a liquid organic hydrogen carrier. This led to various research groups developing new active homogeneous catalysts and making considerable progress. However, homogeneous catalysts are difficult to recycle and reuse, and a large amount of organic matter is used in the preparation process, which has a great impact on the environment.
[0004] Heterogeneous systems can catalyze formic acid to produce hydrogen under mild conditions. Its catalyst is mainly composed of metal oxides and supported metal nanoparticles. Precious metal-based catalysts are generally considered to be the most effective catalysts in heterogeneous systems. Compared with homogeneous catalysts, they are easier to recover and more stable. However, precious metal resources are limited and expensive, which is not conducive to large-scale use. Therefore, people are also constantly researching and developing non-precious metal catalysts. Most non-precious metal catalysts are extremely unstable in systems with a pH of less than 7, so it is very important to develop an efficient, low-cost and stable non-precious metal catalyst. Copper (Cu), which is abundant and low-cost, has a very strong and adjustable localized surface plasmon resonance effect and has excellent catalytic performance for various reactions. Combined with light harvesting ability and catalytic function, copper-based plasmon photocatalysts can serve as a promising platform for efficient light-driven chemical reactions.
[0005] Photocatalytic hydrogen production from formic acid is a current research hotspot. It uses green and abundant sunlight as energy to efficiently produce hydrogen at room temperature. The present invention proposes a low-cost, high-efficiency, simple and easy-to-obtain non-precious metal copper-based plasmon photocatalyst for photocatalytic hydrogen production from gas-phase formic acid. Summary of the invention
[0006] The purpose of the present invention is to provide a plasmonic metal copper-metal oxide composite structure catalyst and a method for catalyzing formic acid to produce hydrogen under visible light at room temperature in view of the deficiencies in the prior art. The plasmonic metal copper-metal oxide composite structure catalyst has good catalytic activity, selectivity and stability, and realizes gas-phase formic acid dehydrogenation under mild conditions.
[0007] The present invention discloses a plasmonic copper-metal oxide composite structure catalyst, which uses a metal salt (zinc chloride, etc.) as a source of a metal oxide semiconductor, uses a copper source (copper chloride, etc.) to modify the metal oxide, and performs H2O2 treatment and vacuum annealing to make the metal oxide generate a large number of oxygen vacancies, thereby obtaining a plasmonic copper-metal oxide composite structure catalyst.
[0008] The plasmon metal copper-metal oxide composite structure catalyst of the present invention is prepared by the following steps:
[0009] (1) adding an alkali solution to a mixed solution of a water-soluble metal salt and a water-soluble copper salt, wherein the concentration of the alkali in the alkali solution is 2M, the sum of the concentrations of the metal salt and the copper salt in the mixed solution of the water-soluble metal salt and the water-soluble copper salt is 2M, and the molar ratio of the metal salt to the copper salt is 0.2 to 5:100; stirring at room temperature for 0.5 to 4 hours to allow the mixture to fully react to generate a metal hydroxide precipitate, filtering and separating the precipitate, and washing with distilled water to remove impurities;
[0010] (2) dispersing the precipitate obtained in step (1) in a 1M H2O2 aqueous solution, then keeping it in an oil bath at 70-90°C for 1-4 hours, and then separating the precipitate by suction filtration to obtain a copper-doped peroxide powder; annealing the obtained copper-doped peroxide powder under vacuum conditions at 200-600°C for 1-4 hours, thereby obtaining a copper-modified oxygen vacancy oxide catalyst (Cu-ZnO-Vo, Cu-ZrO-Vo, Cu-CeO-Vo, etc.), that is, a plasmonic metal copper-metal oxide composite structure catalyst.
[0011] Among them, the alkaline solution is sodium hydroxide (NaOH), potassium hydroxide (KOH), etc., the water-soluble metal salts are zinc chloride (ZnCl2), zinc sulfate (ZnSO4), zinc nitrate (Zn(NO3)2), zirconium oxynitrate (ZrO(NO3)2), zirconium oxychloride (ZrOCl2), cerium nitrate (Ce(NO3)2), etc., and the water-soluble copper salts are copper chloride (CuCl2), copper sulfate (CuSO4), copper nitrate (Cu(NO3)2), etc.
[0012] The plasmonic copper-metal oxide composite structure catalyst (Cu-ZnO-Vo) of the present invention is most preferably a CuCl2 / ZnCl2 molar ratio of 2:100, that is, a Cu:Zn molar ratio of 2:100, and is annealed in a vacuum atmosphere at 400°C for 2h. The obtained plasmonic copper-metal oxide composite structure catalyst has excellent catalytic activity for hydrogen production from formic acid: 10mg of the catalyst can catalyze 10uL (265.217umol) of formic acid with a conversion rate of nearly 100% within 5 minutes, a selectivity of 96.3%, a hydrogen production rate of greater than 300mmol / (g·h), and the catalyst can be recycled.
[0013] The method for producing hydrogen from gas-phase formic acid using a copper-based plasmon photocatalyst under visible light at room temperature described in the present invention specifically comprises placing a plasmon metal copper-metal oxide composite structure catalyst in a gas-phase reactor, controlling the reaction at room temperature by a constant temperature water bath, then vaporizing formic acid and adding it to the reactor, and irradiating the gas-phase reactor with visible light (λ>400nm) from above to react, thereby obtaining product hydrogen.
[0014] Compared with the prior art, the present invention has the following beneficial effects:
[0015] 1. The present invention uses soluble zinc salt ZnCl2 as a precursor and then treats it with hydrogen peroxide to synthesize zinc oxide rich in oxygen vacancies. On the basis of zinc oxide catalyst rich in vacancies, the catalyst is improved to synthesize copper-modified oxygen vacancy zinc oxide catalyst, that is, a plasmon metal copper-metal oxide composite structure catalyst. During the reaction process, the copper co-catalyst exists on the surface of the metal oxide semiconductor as stable metal particles. The hot electrons generated by copper excited by light cross the Schottky barrier of the interface and transfer electrons to the semiconductor. The metal and the metal oxide semiconductor synergistically catalyze formic acid to produce hydrogen. The catalyst material has good electron transfer performance and light induction, and also realizes the utilization of SPR photothermal effect.
[0016] 2. The present invention adopts a coprecipitation method of a water-soluble metal salt and an alkaline solution and a vacuum annealing method to prepare a catalyst. First, a metal hydroxide is synthesized by a coprecipitation method, and then a 1M H2O2 aqueous solution is used to treat the precipitate to obtain a metal peroxide. The dispersed solution is kept in a 75°C oil bath for 2 hours, and then the precipitate is separated by suction filtration to obtain a copper-doped metal peroxide powder, which is then annealed at 400°C in vacuum for 2 hours to obtain a copper-modified oxygen vacancy oxide catalyst. The catalyst has high activity and selectivity under the action of visible light. The catalyst is used to carry out a visible light catalytic formic acid hydrogen production reaction, and still shows good catalytic activity at room temperature (20°C), with a conversion rate of nearly 100%, a selectivity of 96.3%, and a hydrogen production rate of more than 300mmol / (g·h). The catalyst preparation method is simple, the required raw materials are simple and easy to obtain, and can be mass-produced. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 The powder X-ray diffraction spectra of the products obtained in Examples 1, 2, 3, 4 and 5 are compared with the zinc oxide standard card (JCPDS: 36-1451), proving that the products are zinc oxide.
[0018] Figure 2 The mapping diagram of the 2% Cu-ZnO-Vo product obtained by implementing Example 4 shows that the product contains zinc and copper elements, confirming that copper is doped into the oxygen vacancy zinc oxide.
[0019] Figure 3 This is a high-resolution transmission electron microscope (HRTEM) of the 2% Cu-ZnO-Vo product obtained in Example 4 before and after the photocatalytic formic acid hydrogen production reaction. Figure 3 (a) TEM image of 2% Cu-ZnO-Vo before reaction, measuring the lattice spacing of zinc oxide It is attributed to the (100) plane of wurtzite ZnO; Figure 3 (b) is the HRTEM of the 2% Cu-ZnO-Vo product after the reaction, where copper nanoparticles can be clearly seen, confirming that copper participates in the reaction in the form of stable copper nanoparticles during the reaction.
[0020] Figure 4 The electron paramagnetic resonance (EPR) diagram of the 2% Cu-ZnO-Vo product obtained in Example 4 before and after the photocatalytic formic acid hydrogen production reaction, 2% Cu-ZnO-Vo has strong EPR signal peaks at the splitting factors g = 1.961, g = 2.002 and g = 2.044, and the signal peaks correspond to the Zn in the 2% Cu-ZnO-Vo that captures the conduction electrons. 2+ , oxygen vacancies and Cu 2+ , proving that the product before the reaction contains oxygen vacancies and Cu 2+After the reaction, the 2% Cu-ZnO-Vo, i.e., 2% Cu-ZnO-Vo-Used, had a splitting factor of only g=2.002, confirming that the copper substance existed in the form of zero-valent copper nanoparticles after the reaction.
[0021] Figure 5 The photocatalytic formic acid hydrogen production performance bar chart obtained in Examples 1, 2, 3, 4, and 5 confirms that the photocatalytic formic acid hydrogen production performance is best when the molar ratio of Cu:Zn is 2:100.
[0022] Figure 6 This is a bar chart of the photocatalytic formic acid hydrogen production performance of the 2% Cu-ZnO-Vo product in Example 4 obtained under annealing at 200°C to 600°C, which confirms that the photocatalytic formic acid hydrogen production performance of the product is the best under vacuum annealing at 400°C.
[0023] Figure 7 This is a cycle performance curve of the photocatalytic formic acid hydrogen production reaction of the 2% Cu-ZnO-Vo product in Example 4, which proves that the product can be recycled for no less than 30 times. Specific implementation methods
[0024] The present invention is further described in detail below by way of examples, which however do not constitute a limitation of the present invention.
[0025] Example 1
[0026] Catalyst preparation process
[0027] 1.363g zinc chloride (ZnCl2) was weighed and dissolved in 25mL aqueous solution, 0.4g sodium hydroxide (NaOH) was weighed and dissolved in 25mL aqueous solution, the NaOH solution was added to the ZnCl2 solution, stirred at room temperature for 2h, and fully reacted to generate Zn(OH)2 precipitate, the precipitate was separated by filtration, and impurities were removed by washing with distilled water; the obtained precipitate was dispersed in 1M, 100mL H2O2 aqueous solution, the dispersed solution was kept in a 75℃ oil bath for 2 hours, and then the precipitate was separated by suction filtration to obtain zinc peroxide powder. Subsequently, the obtained powder was annealed at 400℃ under vacuum conditions for 2 hours, and the obtained catalyst sample was represented as ZnO-Vo.
[0028] Dehydrogenation reaction process
[0029] 10 mg of the prepared ZnO-Vo catalyst was loaded into the reactor, and the reaction was controlled by a constant temperature water bath at 20°C. Then, formic acid was vaporized and added to the reactor. Visible light of λ>400 nm was irradiated from above the gas phase reactor to react to obtain product hydrogen. The reaction gas was collected. After the reaction, the selectivity of hydrogen was measured to be 83.3%, the conversion rate of formic acid was 9.1%, and the hydrogen production rate of the reaction was 30 mmol / (g·h).
[0030] Example 2
[0031] Catalyst preparation process
[0032] 1.363g zinc chloride (ZnCl2) and 0.0034g copper chloride (CuCl2) were weighed and dissolved in 25mL aqueous solution, 0.4g sodium hydroxide (NaOH) was weighed and dissolved in 25mL aqueous solution, the NaOH solution was added to the mixed solution of ZnCl2 and CuCl2, and stirred at room temperature for 2h to allow it to fully react to generate metal hydroxide precipitate, the precipitate was separated by filtration, and impurities were removed by washing with distilled water; the obtained precipitate was dispersed in 1M, 100mL H2O2 aqueous solution, the dispersed solution was kept in a 75℃ oil bath for 2h, and then the precipitate was separated by suction filtration to obtain copper-doped metal peroxide powder, and then the obtained Cu / ZnO2 powder was annealed at 400℃ under vacuum conditions for 2h, and the obtained catalyst sample was expressed as 0.2% Cu-ZnO-Vo (the molar ratio of Cu:Zn is 2:1000).
[0033] Dehydrogenation reaction process
[0034] 10 mg of the prepared 0.2% Cu-ZnO-Vo catalyst was loaded into a gas phase reactor, and the reaction was controlled by a constant temperature 20°C water bath. Then, formic acid was vaporized and added to the reactor, and visible light of λ>400nm was irradiated from above the gas phase reactor to react and obtain hydrogen as a product. The reaction gas was collected, and after the reaction, the selectivity of hydrogen was measured to be 94.76%, the conversion rate of formic acid was 26.3%, and the hydrogen generation rate of the reaction was 83.64 mmol / (g·h).
[0035] Example 3
[0036] Catalyst preparation process
[0037] 1.363g zinc chloride ZnCl2 and 0.0171g copper chloride CuCl2 were weighed and dissolved in 25mL of aqueous solution, 0.4g sodium hydroxide NaOH was weighed and dissolved in 25mL of aqueous solution, the NaOH solution was added to the mixed solution of ZnCl2 and CuCl2, and stirred at room temperature for 2h to make it fully react to generate metal hydroxide precipitate, the precipitate was separated by filtration, and impurities were removed by washing with distilled water; the obtained precipitate was dispersed in 1M, 100mL H2O2 aqueous solution, the dispersed solution was kept in a 75℃ oil bath for 2h, and then the precipitate was separated by suction filtration to obtain copper-doped metal peroxide powder, and then the obtained Cu / ZnO2 powder was annealed at 400℃ under vacuum conditions for 2h, and the obtained catalyst sample was expressed as 1% Cu-ZnO-Vo (the molar ratio of Cu:Zn is 1:100).
[0038] Dehydrogenation reaction process
[0039] 10 mg of the prepared 1% Cu-ZnO-Vo catalyst was loaded into the reactor, and the reaction was controlled by a constant temperature water bath at 20°C. Then, formic acid was vaporized and added to the reactor, and visible light of λ>400 nm was irradiated from above the gas phase reactor to react and obtain hydrogen as a product. The reaction gas was collected, and after the reaction, the selectivity of hydrogen was measured to be 95.3%, the conversion rate of formic acid was 69.6%, and the hydrogen generation rate of the reaction was 221.5 mmol / (g·h).
[0040] Example 4
[0041] Catalyst preparation process
[0042] 1.363g zinc chloride ZnCl2 and 0.0341g copper chloride CuCl2 are weighed and dissolved in 25mL of aqueous solution, 0.4g sodium hydroxide NaOH is weighed and dissolved in 25mL of aqueous solution, the NaOH solution is added to the mixed solution of ZnCl2 and CuCl2, and stirred at room temperature for 2h to fully react to generate metal hydroxide precipitate, the precipitate is separated by filtration, and impurities are removed by washing with distilled water; the obtained precipitate is dispersed in 1M, 100mL H2O2 aqueous solution, the dispersed solution is kept in a 75℃ oil bath for 2h, and then the precipitate is separated by suction filtration, copper-doped metal peroxide powder is obtained, and then the Cu / ZnO2 powder is annealed at 400℃ under vacuum conditions for 2h, and the obtained catalyst sample is expressed as 2% Cu-ZnO-Vo (the molar ratio of Cu:Zn is 2:100).
[0043] Dehydrogenation reaction process
[0044] 10 mg of the prepared 2% Cu-ZnO-Vo catalyst was loaded into the reactor, and the reaction was controlled by a constant temperature 20°C water bath. Then, formic acid was vaporized and added to the reactor, and visible light of λ>400nm was irradiated from above the gas phase reactor to react and obtain hydrogen as a product. The reaction gas was collected, and after the reaction, the selectivity of hydrogen was measured to be 96.3%, the conversion rate of formic acid was 97.2%, and the hydrogen generation rate of the reaction was 309.4 mmol / (g·h), which can be recycled for at least 30 times.
[0045] Example 5
[0046] Catalyst preparation process
[0047] 1.363g zinc chloride ZnCl2 and 0.08525g copper chloride CuCl2 were weighed and dissolved in 25mL of aqueous solution, 0.4g sodium hydroxide NaOH was weighed and dissolved in 25mL of aqueous solution, the NaOH solution was added to the mixed solution of ZnCl2 and CuCl2, and stirred at room temperature for 2h to allow it to fully react to generate metal hydroxide precipitate, the precipitate was separated by filtration, and impurities were removed by washing with distilled water; the obtained precipitate was dispersed in 1M, 100mL H2O2 aqueous solution, the dispersed solution was kept in a 75°C oil bath for 2 hours, and then the precipitate was separated by suction filtration to obtain copper-doped metal peroxide powder, and then the Cu / ZnO2 powder was annealed at 400°C under vacuum conditions for 2 hours, and the obtained catalyst sample represented 5% Cu-ZnO-Vo (the molar ratio of Cu:Zn was 5:100).
[0048] Dehydrogenation reaction process
[0049] 10 mg of the prepared 5% Cu-ZnO-Vo catalyst was loaded into the reactor, and the reaction was controlled by a constant temperature 20°C water bath, and then formic acid was vaporized and added to the reactor, and visible light of λ>400nm was irradiated from the top of the gas phase reactor to react to obtain hydrogen as a product. The reaction gas was collected, and the selectivity of hydrogen after the reaction was measured to be 94.4%, the conversion rate of formic acid was 93.1%, and the hydrogen generation rate of the reaction was 296.25 mmol / (g·h). The hydrogen selectivity and hydrogen generation rate at this molar ratio were both lower than those of the 2% Cu-ZnO-Vo catalyst prepared in Example 4.
[0050] The above content is a further detailed description of the present invention in combination with a specific preferred embodiment. It cannot be determined that the specific embodiments of the present invention are limited to this. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions and substitutions can be made without departing from the concept of the present invention, which should be regarded as belonging to the scope of protection of the patent determined by the submitted claims of the present invention.
Claims
1. A plasmonic metal copper-metal oxide composite catalyst for catalyzing hydrogen production from gas-phase formic acid under visible light at room temperature, characterized in that: The catalyst is used for catalyzing gas-phase formic acid to produce hydrogen under visible light at room temperature, and is prepared by the following steps: (1) adding an alkali solution to a mixed solution of a water-soluble metal salt and a water-soluble copper salt, wherein the concentration of the alkali in the alkali solution is 2M, the sum of the concentrations of the metal salt and the copper salt in the mixed solution of the water-soluble metal salt and the water-soluble copper salt is 2M, and the molar ratio of the metal salt to the copper salt is 0.2-5:100; stirring at room temperature to allow the mixture to react fully to generate a metal hydroxide precipitate, filtering and separating the precipitate, and washing with distilled water to remove impurities; (2) dispersing the precipitate obtained in step (1) in a 1M H2O2 aqueous solution, and then maintaining it in an oil bath at 70-90°C for 1-4 hours, and then separating the precipitate by suction filtration to obtain a copper-doped peroxide powder; annealing the obtained copper-doped peroxide powder under vacuum conditions at 200-600°C for 1-4 hours, thereby obtaining a copper-doped oxygen vacancy oxide catalyst, i.e., a plasmonic metal copper-metal oxide composite structure catalyst.
2. The plasmonic metal copper-metal oxide composite catalyst for catalyzing gas-phase formic acid to produce hydrogen under visible light at room temperature as claimed in claim 1, characterized in that: The alkali is one or more of NaOH and KOH, the water-soluble metal salt is one or more of ZnCl2, ZnSO4, Zn(NO3)2, ZrO(NO3)2, ZrOCl2, Ce(NO3)2; the water-soluble copper salt is one or more of CuCl2, CuSO4, Cu(NO3)2.
3. The plasmonic metal copper-metal oxide composite catalyst for catalyzing hydrogen production from gas-phase formic acid under visible light at room temperature as claimed in claim 2, characterized in that: The water-soluble metal salt is ZnCl2, and the water-soluble copper salt is CuCl2.
4. The plasmonic metal copper-metal oxide composite catalyst for catalyzing hydrogen production from gas-phase formic acid under visible light at room temperature as claimed in claim 3, characterized in that: The molar ratio of CuCl2 and ZnCl2 is 2:100, and the plasmonic metal copper-metal oxide composite structure catalyst is obtained by annealing in a vacuum atmosphere at 400°C for 2 h.
5. A method for producing hydrogen from gas-phase formic acid using a plasmonic copper-metal oxide composite catalyst under visible light at room temperature, characterized in that: The method comprises placing a plasmonic metal copper-metal oxide composite structure catalyst for catalyzing gas-phase formic acid to produce hydrogen under visible light at room temperature as described in any one of claims 1 to 4 in a gas-phase reactor, controlling the reaction at room temperature by a constant temperature water bath, then vaporizing formic acid and adding it to the reactor, and irradiating the gas-phase reactor with visible light from above to react, thereby obtaining product hydrogen.
Citation Information
Patent Citations
Preparation method for CuO / ZnO composite photocatalyst
CN108579752A
Method for preparing biomass carbon-based metal-modified self-doped vacancy-rich tin oxide nano-composite photocatalytic materials
CN109126821A
Method for decomposing formic acid through photocatalysis
CN109553067A
Photocatalytic metal dissolution method
CN111809063A
High-dispersion ruthenium-modified oxygen-defect-rich semiconductor photocatalyst as well as preparation method and application thereof