A Co3O4-CeO2 catalyst for low-temperature CO catalytic oxidation and a preparation method thereof
Co3O4-CeO2 catalyst prepared by hydrothermal and low-temperature calcination solves the problems of low catalyst activity and difficult to control morphology in the prior art, and realizes complete CO conversion under low temperature conditions, which is suitable for hydrogen purification of automobile exhaust gas and fuel cell. , has the potential for industrial production.
Patent Information
- Application Number
- CN202311236255.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-25
- Publication Date
- 2024-11-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing Co3O4-CeO2 composite oxide catalysts have low activity in low-temperature CO catalytic oxidation and are difficult to control, so they cannot effectively deal with CO pollution in automobile exhaust and fuel cell hydrogen purification.
Co3O4-CeO2 catalyst is prepared by combining hydrothermal and low-temperature calcination. The suspension is formed by stirring cobalt salt, cerium salt and strong alkali, and then hydrothermal reaction and calcination are carried out in the presence of aluminum powder to obtain high activity and shape. Nanocomposite material with uniform appearance.
It achieves the catalytic performance of achieving complete CO conversion at -10°C. It is suitable for automotive exhaust purification and fuel cell hydrogen purification. It has a simple process and low cost, which is suitable for industrial production.
Smart Images

Figure CN117427644B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the fields of functional material synthesis and energy environment, and in particular to a preparation method and application of a Co3O4-CeO2 catalyst for low-temperature CO catalytic oxidation. Background Art
[0002] With the rapid development of social economy and the rapid growth of population, traditional energy is increasingly depleted, and the energy crisis has become an important issue concerning the people's livelihood and social and economic development of all countries. At the same time, the large-scale development and utilization of fossil energy has caused serious ecological damage and environmental pollution. CO oxidation, as a typical low-temperature oxidation model reaction, has important applications in industries such as automobile exhaust treatment, fuel cells, and H2 purification. However, the CO oxidation temperature of most catalysts currently involved is often higher than 200°C, and most pollutants in automobile exhaust are currently emitted within 30 seconds of cold start. In the field of fuel cell hydrogen purification, the CO priority oxidation reactor is connected to the water-gas conversion reactor on the upper side and the fuel cell on the lower side. The temperature of the hydrogen-rich gas after the water-gas conversion is about 200°C, and the operating temperature of the fuel cell is 80-100°C. Therefore, it is necessary to develop a highly active low-temperature CO oxidation catalyst.
[0003] Cobalt oxide and cerium dioxide-based catalysts are two materials widely used in various catalytic reactions. Cobalt oxide, as a p-type semiconductor, is often used in a composite heterojunction with other semiconductor materials for photocatalytic reactions. In addition, due to the presence of Co in Co3O4, 3+ / Co 2+ Redox couple makes it show excellent catalytic performance in many thermal catalytic reactions such as Fischer-Tropsch synthesis and various catalytic oxidation reactions. Ceria has a unique oxygen storage / release capacity (OSC) and has become an important material in catalytic fields such as methanol steam reforming, three-way catalysis, CO oxidation, water gas shift and methane dry reforming. The combination of cobalt tetroxide and cerium dioxide is expected to improve the CO catalytic performance. However, the Co3O4-CeO2 composite oxides synthesized by existing methods have poor uniformity (such as Lu Xiaolin. Research on CO preferential oxidation performance of Co3O4-CeO2 and its composite oxide catalysts [D]. Inner Mongolia: Inner Mongolia University of Technology, 2016), the morphology is difficult to control (such as Jin Xin, Feng Xilan, Liu Dapeng, etc. Preparation of Co3O4 / CeO2 nanocomposites by spontaneous redox method and structural optimization of their CO catalytic oxidation reaction [J] Journal of Chemistry in Universities, 2020, 41, 652), and the catalytic activity is low (such as patent CN 107362804B, 2020.04.28). Summary of the invention
[0004] The purpose of the embodiments of the present invention is to provide a Co3O4-CeO2 catalyst for low-temperature CO catalytic oxidation, and also to provide a method for preparing the catalyst, in order to solve the problems raised in the above-mentioned background technology.
[0005] To achieve the above objectives, the embodiments of the present invention provide the following technical solutions:
[0006] The preparation method of the Co3O4-CeO2 catalyst for low-temperature CO catalytic oxidation of the present invention comprises the following steps:
[0007] Step S1: Add cobalt salt, cerium salt and deionized water into a beaker, and stir for a period of time at a certain temperature to obtain a light pink solution;
[0008] Step S2: adding a strong base and deionized water into a beaker, stirring for a period of time at a certain temperature to obtain a transparent solution;
[0009] Step S3: adding the solution obtained in step S2 dropwise to the solution obtained in step S1 under stirring, and continuing stirring to obtain a turbid solution;
[0010] Step S4: transferring the suspension obtained in step S3 to a reaction kettle, adding aluminum powder, and then placing it in an oven for reaction. The precipitate obtained by the reaction is washed with deionized water and ethanol, and dried in an oven to obtain a Co3O4-CeO2 nanocomposite material precursor;
[0011] Step S5: The precursor obtained in step S4 is placed in a muffle furnace for calcination, and then further calcined in a tube furnace to obtain a Co3O4-CeO2 catalyst suitable for room temperature CO catalytic oxidation.
[0012] Preferably, the cobalt / cerium molar ratio of the Co3O4-CeO2 nanocomposite material is 1 to 10, the cobalt salt is selected from one of cobalt chloride, cobalt nitrate, cobalt sulfate or cobalt acetate, the cerium salt is selected from one of cerium chloride, cerium nitrate or cerium acetate, and the strong base is selected from one of sodium hydroxide or potassium hydroxide.
[0013] Furthermore, in the step S1, the dissolution temperature is room temperature-60°C, and the stirring time is 10-60 minutes. In the step S2, the dissolution temperature is 0-40°C, and the stirring time is 10-60 minutes. In the step S4, the hydrothermal temperature range of the suspension is 100-200°C, and the time is 12-48 hours. In the step S5, the muffle furnace calcination temperature is 200-600°C, and the heating rate is 1-10°C / minute; the tubular furnace calcination temperature is 200-600°C, the calcination atmosphere is compressed air, N2, Ar or He, the time is 2-6 hours, and the heating rate is 1-10°C / minute.
[0014] The Co3O4-CeO2 catalyst of the present invention can be used for CO oxidation elimination in low temperature and room temperature environments, and complete CO conversion can be achieved at -10°C. The CO oxidation reaction performance test is carried out in a U-shaped quartz tube fixed bed with an outer diameter of 8 mm, the reaction mixture is 1% CO, 20% O2 and 79% He, the mass of the catalyst used in the test is 50 mg, and the evaluation temperature of the catalytic activity is -40 to 400°C.
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] 1. The present invention combines hydrothermal and low-temperature calcination to synthesize the Co3O4-CeO2 catalyst for low-temperature CO catalytic oxidation. Compared with the previously reported Co3O4-CeO2 composite oxide synthesis method, the catalyst prepared by this method has the characteristics of highly dispersed active components and uniform and controllable morphology. The entire synthesis process is simple and easy, with strong controllability, no need for advanced instruments, low cost, and suitable for industrial production.
[0017] 2. The Co3O4-CeO2 composite oxide provided by the present invention is applied to CO catalytic oxidation reaction. Compared with the current metal oxide catalysts, it has excellent performance under the reaction atmosphere and can achieve complete CO conversion at -10°C, which is of great significance for automobile exhaust purification and fuel cell hydrogen purification under actual conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 These are the X-ray powder diffraction patterns (XRD) of 1-1Co3O4-CeO2, 3-1Co3O4-CeO2 and 5-1Co3O4-CeO2.
[0019] Figure 2 These are the X-ray powder diffraction patterns (XRD) of 5-1Co3O4-CeO2, 5-1Co3O4-CeO2-N2 and 5-1Co3O4-CeO2-Air.
[0020] Figure 3 Scanning electron microscope (SEM) images of 1-1Co3O4-CeO2, 3-1Co3O4-CeO2 and 5-1Co3O4-CeO2.
[0021] Figure 4 These are the transmission electron microscope (TEM) images of Comparative Example 1, Comparative Example 2, 5-1Co3O4-CeO2, 5-1Co3O4-CeO2-N2 and 5-1Co3O4-CeO2-Air.
[0022] Figure 5 This is the CO catalytic oxidation activity diagram of Comparative Example 3, 5-1Co3O4-CeO2, 5-1Co3O4-CeO2-N2 and 5-1Co3O4-CeO2-Air. DETAILED DESCRIPTION
[0023] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments. The illustrative embodiments and descriptions of the present invention are used to explain the present invention but are not intended to limit the present invention.
[0024] Example 1
[0025] Preparation of sample #1 Co3O4-CeO2 catalyst with a cobalt / cerium molar ratio of 1:1
[0026] 9.6 g of NaOH was dissolved in 25 mL of deionized water to form solution A. At the same time, 6 mmol of Co(NO3)2·6H2O and 6 mmol of Ce(NO3)3·6H2O were dissolved in 15 mL of deionized water to form solution B. The above solution A was added dropwise to solution B under stirring at a rate of about 1 mL min -1 After the addition was completed, the mixture was stirred for one hour, 10 mmol of aluminum powder was added, and the mixture was transferred to a reactor for hydrothermal reaction at 100 °C for 24 h. After cooling to room temperature, the mixture was washed with deionized water and anhydrous ethanol, dried at 60 °C, and then calcined in a muffle furnace at 200 °C for 2 h, with a heating rate of 2 °C·min -1 The X-ray diffraction pattern of the Co3O4-CeO2 catalyst prepared in this example is as follows: Figure 1 shown.
[0027] Example 2
[0028] Preparation of sample #2 Co3O4-CeO2 catalyst with a cobalt / cerium molar ratio of 3:1
[0029] 9.6 g of NaOH was dissolved in 25 mL of deionized water to form solution A. Meanwhile, 9 mmol of Co(NO3)2·6H2O and 3 mmol of Ce(NO3)3·6H2O were dissolved in 15 mL of deionized water to form solution B. The above solution A was added dropwise to solution B under stirring at a rate of about 1 mL min -1 After the addition was completed, the mixture was stirred for one hour, 10 mmol of aluminum powder was added, and the mixture was transferred to a reactor for hydrothermal reaction at 100 °C for 24 h. After cooling to room temperature, the mixture was washed with deionized water and anhydrous ethanol, dried at 60 °C, and then calcined in a muffle furnace at 200 °C for 2 h, with a heating rate of 2 °C·min -1 The X-ray diffraction pattern of the Co3O4-CeO2 catalyst prepared in this example is as follows: Figure 1 shown.
[0030] Example 3
[0031] Preparation of sample #3 Co3O4-CeO2 catalyst with a cobalt / cerium molar ratio of 5:1
[0032] 9.6 g of NaOH was dissolved in 25 mL of deionized water to form solution A. Meanwhile, 10 mmol of Co(NO3)2·6H2O and 2 mmol of Ce(NO3)3·6H2O were dissolved in 15 mL of deionized water to form solution B. The above solution A was added dropwise to solution B under stirring at a rate of about 1 mL min -1 After the addition was completed, the mixture was stirred for one hour, 10 mmol of aluminum powder was added, and the mixture was transferred to a reactor for hydrothermal reaction at 100 °C for 24 h. After cooling to room temperature, the mixture was washed with deionized water and anhydrous ethanol, dried at 60 °C, and then calcined in a muffle furnace at 200 °C for 2 h, with a heating rate of 2 °C·min -1 The X-ray diffraction pattern of the Co3O4-CeO2 catalyst prepared in this example is as follows: Figure 1 shown.
[0033] Example 4
[0034] Preparation of sample #4 Co3O4-CeO2-N2 catalyst with a cobalt / cerium molar ratio of 5:1 and calcined in N2 atmosphere
[0035] 9.6 g of NaOH was dissolved in 25 mL of deionized water to form solution A. Meanwhile, 10 mmol of Co(NO3)2·6H2O and 2 mmol of Ce(NO3)3·6H2O were dissolved in 15 mL of deionized water to form solution B. The above solution A was added dropwise to solution B under stirring at a rate of about 1 mL min -1 After the addition was completed, the mixture was stirred for one hour, 10 mmol of aluminum powder was added, and the mixture was transferred to a reactor for hydrothermal reaction at 100 °C for 24 h. After cooling to room temperature, the mixture was washed with deionized water and anhydrous ethanol, dried at 60 °C, and then calcined in a muffle furnace at 200 °C for 2 h, with a heating rate of 2 °C·min -1 The obtained powder was further heated in N2 atmosphere at 2℃·min -1 The temperature was raised at 400°C for 2 h. The X-ray diffraction pattern of the Co3O4-CeO2-N2 catalyst prepared in this example is shown in FIG. Figure 2 shown.
[0036] Example 5
[0037] Preparation of sample #5 Co3O4-CeO2-Air catalyst with a cobalt / cerium molar ratio of 5:1 and calcined in air atmosphere
[0038] 9.6 g of NaOH was dissolved in 25 mL of deionized water to form solution A. Meanwhile, 10 mmol of Co(NO3)2·6H2O and 2 mmol of Ce(NO3)3·6H2O were dissolved in 15 mL of deionized water to form solution B. The above solution A was added dropwise to solution B under stirring at a rate of about 1 mL min -1 After the addition was completed, the mixture was stirred for one hour, 10 mmol of aluminum powder was added, and the mixture was transferred to a reactor for hydrothermal reaction at 100 °C for 24 h. After cooling to room temperature, the mixture was washed with deionized water and anhydrous ethanol, dried at 60 °C, and then calcined in a muffle furnace at 200 °C for 2 h, with a heating rate of 2 °C·min -1 The obtained powder was further heated in compressed air at 2 °C min -1 The temperature was raised at 400°C for 2 h. The X-ray diffraction pattern of the Co3O4-CeO2-Air catalyst prepared in this example is shown in FIG. Figure 2 shown.
[0039] Example 6
[0040] Sample structure and morphology characterization
[0041] X-ray diffraction (XRD) analysis was performed on samples #1 to #5. Figure 1 and Figure 2 As shown. The XRD spectra of samples #1 to #5 are well matched with the standard PDF (PDF#34-0394, PDF#43-1003) cards, indicating that the phases of samples #1 to #5 are Co3O4 and CeO2. Figure 1 It can be seen that as the Co / Ce feed molar ratio gradually increases from 1:1 to 5:1, the diffraction peak intensity of Co3O4 in the sample also gradually increases, indicating that the phase content of Co3O4 in the sample increases and the phase content of CeO2 decreases. By performing scanning electron microscopy (SEM) and transmission electron microscopy (TEM) analysis on samples #1 to #5, Figure 3 and Figure 4 As shown. When the Co / Ce feed molar ratio is 1:1 (sample #1), it is mainly composed of stacked nanowires and nanosheets. As the Co / Ce feed molar ratio gradually increases from 1:1 to 5:1, the nanowires on its surface gradually decrease, and the nanosheets gradually transform into regular hexagonal morphology. When sample #3 is further calcined in compressed air and N2 atmosphere, its morphology remains unchanged ( Figure 4 ).
[0042] Example 7
[0043] Characterization of sample CO catalytic oxidation performance
[0044] The catalyst was tested for CO oxidation activity using a fixed bed microreactor. The test conditions were: 50 mg catalyst, 1% CO, 20% O2 and 79% He mixed gas, and a total gas flow rate of 19.6 ml / min. The CO catalytic oxidation performance of samples #3 to #5 is shown in Figure 2. Figure 5 The test results show that the catalytic oxidation performance of the Co3O4-CeO2 nanocomposite can be greatly improved after further calcination in a tube furnace. When the calcination atmosphere is N2, the Co3O4-CeO2 nanocomposite can achieve complete CO conversion at room temperature. When the calcination atmosphere is compressed air, it can achieve complete CO conversion at -10°C.
[0045] Comparative Example 1
[0046] A certain amount of Ce(NO3)3·6H2O and Co(NO3)2·6H2O were uniformly mixed in a specific ratio, and a mixed solution of 0.9434M sodium carbonate and sodium hydroxide was used as a precipitant for parallel titration. During this process, the pH value of the precipitate was controlled within the range of 9.5-10.5. The precipitate was stirred at room temperature for 3 hours, then washed twice with deionized water at room temperature, washed twice with anhydrous ethanol, dried in an oven at 85°C for 12 hours, and finally calcined at 350°C in a muffle furnace for 5 hours to obtain the 8Co3O4-1CeO2 catalyst.
[0047] Comparative Example 2
[0048] First, 0.134 g of (Co(NH3)6)Cl3 and 1.09 g of Ce(NO3)3·6H2O were ultrasonically dispersed in 100 mL of deionized water and stirred for 10 min. Then, NaOH solution (9 mL, 1 mmol / L) was added. The orange solution was heated at 40°C for 1 h, cooled to room temperature and centrifuged (at a speed of 8000 r / min). The obtained product was dried in a vacuum oven at 60°C, and then calcined in air at 500°C for 2 h (at a heating rate of 10°C / min).
[0049] Comparative Example 3
[0050] First, 4mmol Co(NO3)2·6H2O and 8mmol 2-methylimidazole were dissolved in 100mL anhydrous methanol, and then the obtained solution was transferred to a 100mL screw-capped bottle and allowed to stand at room temperature for 24 hours to obtain a solid-liquid mixture. The obtained solid-liquid mixture was filtered and vacuum dried at 80℃ for 12h to obtain the precursor ZIF-67. 0.5g Ce(NO3)3·6H2O was weighed and dissolved in 10mL anhydrous ethanol, and 0.5g dried ZIF-67 was added to the mixed solution, stirred and mixed at room temperature for 5h, and then solid-liquid separation was performed, and the separated solid was collected and dried in an 80℃ drying oven for 12h. The obtained solid powder was calcined at 400℃ in air for 3 hours (heating rate of 5℃ / min) to obtain a flower-like Co3O4-CeO2 composite oxide.
[0051] The above are only preferred embodiments of the present invention. It should be pointed out that, for those skilled in the art, several modifications and improvements can be made without departing from the concept of the present invention. These should also be regarded as the protection scope of the present invention. These will not affect the effect of the implementation of the present invention and the practicality of the patent.
Claims
1. A method for preparing a Co3O4-CeO2 catalyst for low-temperature CO catalytic oxidation, characterized in that: The following steps are involved: Step S1: Add cobalt salt, cerium salt and deionized water into a beaker, and stir for a period of time at a certain temperature to obtain a light pink solution; Step S2: adding a strong base and deionized water into a beaker, stirring for a period of time at a certain temperature to obtain a transparent solution; Step S3: adding the solution obtained in step S2 dropwise to the solution obtained in step S1 under stirring, and continuing stirring to obtain a turbid solution; Step S4: transferring the suspension obtained in step S3 to a reaction kettle, adding aluminum powder, and then placing it in an oven for reaction. The precipitate obtained by the reaction is washed with deionized water and ethanol, and dried in an oven to obtain a Co3O4-CeO2 nanocomposite material precursor; Step S5: calcining the precursor obtained in step S4 in a muffle furnace, and then further calcining it in a tube furnace to obtain a Co3O4-CeO2 catalyst for CO catalytic oxidation; The cobalt salt is selected from one of cobalt chloride, cobalt nitrate, cobalt sulfate or cobalt acetate, the cerium salt is selected from one of cerium chloride, cerium nitrate or cerium acetate, and the strong base is selected from one of sodium hydroxide or potassium hydroxide; In step S5, the calcination temperature of the muffle furnace is 200-600°C, and the heating rate is 1-10°C / min; the calcination temperature of the tubular furnace is 200-600°C, the calcination atmosphere is compressed air, the time is 2-6 hours, and the heating rate is 1-10°C / min.
2. The method for preparing the Co3O4-CeO2 catalyst for low-temperature CO catalytic oxidation according to claim 1, characterized in that: The cobalt / cerium molar ratio of the Co3O4-CeO2 nanocomposite material is 1-10.
3. The method for preparing the Co3O4-CeO2 catalyst for low-temperature CO catalytic oxidation according to claim 1, characterized in that: In the step S1, for the dissolution of the cobalt salt and the cerium salt, the dissolution temperature is room temperature-60° C., and the stirring time is 10-60 minutes.
4. The method for preparing the Co3O4-CeO2 catalyst for low-temperature CO catalytic oxidation according to claim 1, characterized in that: In the step S2, for the dissolution of the strong base, the dissolution temperature is 0-40° C. and the stirring time is 10-60 minutes.
5. The method for preparing the Co3O4-CeO2 catalyst for low-temperature CO catalytic oxidation according to claim 1, characterized in that: In step S4, the suspension is hydrothermally heated at a temperature ranging from 100 to 200° C. for a time period of 12 to 48 hours.
6. A Co3O4-CeO2 catalyst for low-temperature CO catalytic oxidation, characterized in that: The method is prepared by any one of claims 1 to 5.
7. Use of a Co3O4-CeO2 catalyst for low-temperature CO catalytic oxidation obtained according to the method of any one of claims 1 to 5, characterized in that: The Co3O4-CeO2 catalyst is used for CO oxidation reaction performance testing.
8. The use of the Co3O4-CeO2 catalyst for low-temperature CO catalytic oxidation according to claim 7, characterized in that: The CO oxidation reaction performance test was carried out in a U-shaped quartz tube fixed bed with an outer diameter of 8 mm. The composition of the reaction gas was 1% CO, 20% O2 and 79% He.
Citation Information
Patent Citations
Cerium-based composite oxide catalyst for catalyzing and purifying nitric oxide
CN102000560A
Modified Co-Ce core-shell structure catalyst for carbon monoxide (CO) low-temperature oxidation
CN105148930A
Preparing method for flake-feature nano-composite metal oxide catalyst CeO2-Co3O4
CN105597769A
Cerium dioxide-loaded cobalt-based catalyst for hydrogen production by autothermal reforming of acetic acid
CN111450834A
Cobalt-based composite oxide catalyst for CO low-temperature oxidation and preparation method thereof
CN113996304A
Cited By
CO catalytic oxidation catalyst and preparation method thereof
CN122141695A