Preparation method and application of strip-shaped nano-barium sulfate
By adding EDTA-2Na and phosphate to barium sulfate slurry, the morphology and size of barium sulfate can be controlled, and strip-shaped barium sulfate with high aspect ratio can be synthesized. This solves the problem of insufficient mechanical improvement of hollow spherical barium sulfate nanoparticles and realizes high-purity and low-cost plastic modification applications.
Patent Information
- Application Number
- CN202310353274.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-04
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-04-04
AI Technical Summary
In existing technologies, hollow spherical nano-barium sulfate does not provide sufficient mechanical enhancement in plastic modification. Ordinary barium sulfate powder, when used as an additive, increases the density of the product, weakens the advantages of lightweighting, and is costly.
By adding EDTA-2Na and phosphate to barium sulfide slurry, the morphology and size of barium sulfate can be controlled, and the synthesis reaction rate can be controlled to form strip-shaped barium sulfate with an aspect ratio higher than 4:1. Ultrasonic vibration and silane coupling agent treatment are used to improve dispersibility and purity.
Barium sulfate nanoparticles with uniform particle size distribution and high purity were prepared, which are suitable for plastic modification, improving mechanical properties and reducing production costs.
Smart Images

Figure CN116332218B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of inorganic nano material synthesis, and in particular to a preparation method and application of strip-shaped nano barium sulfate. Background Art
[0002] Barium sulfate is one of the most important inorganic chemical products today. It is widely used in rubber, plastic, coating, medicine and other industries. It is also used as a weighting agent for oil and gas drilling mud. Barium sulfate has the characteristics of good acid and alkali resistance and corrosion resistance. Therefore, adding it to rubber and plastic products as a filler not only increases the volume, increases the volume, and reduces the cost, but also improves the mechanical strength, thermodynamic properties, and corrosion resistance and aging resistance of the products. However, the density of barium sulfate is relatively large. When ordinary barium sulfate powder is used as an additive, it often greatly increases the density of the product, weakens and reduces the lightweight advantages of plastic and rubber products, increases production costs, and greatly limits the scope of use of such products. Therefore, under the same quality, the volume and surface area of barium sulfate can be increased as much as possible, which will effectively reduce the density of rubber and plastic products, maintain the lightweight advantages, and reduce production costs.
[0003] Patent Publication No. (CN 113697838 A) discloses a method for preparing hollow spherical nano-barium sulfate, the steps of which are: 1) adding hydrochloric acid and a reaction aid to a nano-barium sulfide slurry and mixing thoroughly to obtain a pre-reaction mixture A; 2) adding hydrochloric acid to a sodium hexametaphosphate solution to prepare a pre-reaction mixture B; 3) adding the pre-reaction mixture A and the pre-reaction mixture B obtained in step 1) to a sodium sulfate solution at the same time, and stabilizing the pH value between 2.0 and 6.0 when adding; after all mixing, the pH value is between 1.5 and 1.8; 4) stirring the mixture obtained in step 3) for more than 30 minutes, adjusting the pH to 7.0 to 9.0 to terminate the reaction; 5) filtering and washing with water, and drying to obtain hollow spherical nano-barium sulfate. The method prepares hollow spherical barium sulfate, so that when barium sulfate is used as an additive, it can increase its surface area and volume in contact with the main material, thereby greatly improving the application range of barium sulfate as an additive.
[0004] However, the mechanical improvement of hollow spherical nano-barium sulfate in plastic modification applications is insufficient, and barium sulfate strips are more effective in improving the mechanical properties of plastics. Summary of the invention
[0005] In order to solve the technical problems existing in the above background technology, one of the purposes of the present invention is to provide a method for preparing strip-shaped nano barium sulfate, comprising the following steps:
[0006] S0: Add 0.05-0.6 mass parts of EDTA-2Na and 0.05-0.2 mass parts of phosphate to 10-30 mass parts of barium sulfide slurry and mix thoroughly to obtain a pre-reaction mixture, wherein the mass ratio of barium sulfide to the slurry is 10-30%;
[0007] S1: preparing 3 to 8 parts by mass of a sodium sulfate solution having a concentration of 3 to 8 wt% (parts by mass);
[0008] S2: adding 0.05-0.7 parts by mass of EDTA-2Na and 0.01-0.05 parts by mass of sodium octadecyl sulfonate or sodium octadecyl sulfate to 500-1000 parts by mass of water to prepare a bottom water mixture;
[0009] S3: adding the pre-reaction mixture and the sodium sulfate solution to the bottom water mixture;
[0010] S4: stirring the mixture in S3 to make it fully react to obtain a reacted mixture;
[0011] S5: Filter the reaction mixture, wash with water, and dry to obtain strip-shaped nano-barium sulfate.
[0012] Among them, EDTA-2Na is a chelating agent that can form a stable complex with barium ions, making barium ions more easily dispersed in aqueous solution, while preventing sulfate ions from combining with barium ions to form unstable precipitation. Phosphate can adjust the pH value and ionic strength of the reaction system, and has a certain effect on controlling the morphology of barium sulfate. The barium sulfide selected in the present invention is because sulfide ions can jointly regulate the morphology and size of barium sulfate with EDTA-2Na and phosphate, the synthesis reaction rate is controllable, the crystallization trend of the formed particles is consistent, the shape of the synthesis is uniform, and finally a strip of nanoscale barium sulfate is formed.
[0013] As a preferred embodiment, 3 to 10 parts by mass of barium chloride are further added to S0.
[0014] As a preferred embodiment, 1 to 5 parts by mass of strontium sulfide is further added to S0, and the mass parts of barium sulfide slurry is 10 to 15.
[0015] As a preferred solution, between S2 and S4, the mixture in S3 is treated by ultrasonic oscillation at 40-60 degrees Celsius, wherein the power is 100-300 W and the oscillation time is 10-30 minutes.
[0016] As a preferred embodiment, in S0, the phosphate is trisodium phosphate, and the mass ratio of EDTA-2Na to trisodium phosphate is 1:1.25.
[0017] As a preferred embodiment, in S3, stirring is started and the temperature is raised to 40-50°C before the pre-reaction mixture and the sodium sulfate solution are added dropwise.
[0018] As a preferred embodiment, in S5, the reaction mixture is filtered, washed with water, re-slurried, 0.1 to 1.0 parts by mass of a silane coupling agent is added, the pH value is adjusted to 4.0 to 5.0, stirred for 1 to 2 hours, and then dehydrated and dried to obtain strip-shaped nano-barium sulfate.
[0019] In order to solve the above technical problems, the second purpose of the present invention is to provide the application of the strip-shaped nano-barium sulfate prepared by the above preparation method in plastic modification.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] (1) Compared with other existing technologies, the reaction mechanism of the present invention is that barium sulfide reacts with EDTA and phosphate in a certain ratio to form a complex, and then reacts with sodium sulfate to synthesize barium sulfate, wherein sulfide ions, EDTA-2Na and phosphate are combined to control the morphology and size of barium sulfate, thereby preparing strip-shaped nano-barium sulfate with an aspect ratio higher than 4:1, the synthesis reaction rate is controllable, the crystallization trend of the formed particles is consistent, and the synthesized shape is uniform;
[0022] (2) This method has low cost, simple process, concentrated and uniform product particle size distribution, can control the size and properties of strip-shaped nano barium sulfate particles, and is suitable for industrial production and application;
[0023] (3) The prepared strip-shaped nano-barium sulfate has high purity and concentrated distribution, and can be effectively used as a reinforcing and toughening raw material for plastic modification. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a SEM scanning electron microscope image of the strip-shaped nano-barium sulfate obtained in Example 4;
[0025] Figure 2 This is the particle size distribution diagram of the strip-shaped nano-barium sulfate obtained in Example 4.
[0026] Figure 3 This is a SEM scanning electron microscope image of the strip-shaped nano-barium sulfate obtained in Example 2;
[0027] Figure 4 This is the particle size distribution diagram of the strip-shaped nano-barium sulfate obtained in Example 2. DETAILED DESCRIPTION
[0028] The present invention is further described below in conjunction with examples. These examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually carried out according to conventional conditions in the art or according to the conditions recommended by the manufacturer; the raw materials, reagents, etc. used, unless otherwise specified, are all raw materials and reagents that can be obtained from commercial channels such as conventional markets. Any non-substantial changes and substitutions made by those skilled in the art on the basis of the present invention belong to the scope of protection claimed by the present invention.
[0029] Unless otherwise specified, the sources of raw materials in the embodiments and comparative examples of the present invention are conventional raw materials, including the following 7 embodiments and 2 comparative examples.
[0030] Example 1
[0031] A method for preparing strip-shaped nano-barium sulfate comprises the following steps:
[0032] Step 1: Add 0.05 parts by mass of EDTA-2Na and 0.625 parts by mass of trisodium phosphate to 10 parts by mass of 1 mol / L barium sulfide slurry and mix well to obtain a pre-reaction mixture;
[0033] Step 2: preparing 3 parts by mass of a sodium sulfate solution having a concentration of 8 wt % (parts by mass);
[0034] Step 3: Add 0.05 parts by mass of EDTA-2Na and 0.05 parts by mass of sodium octadecyl sulfate to 50 parts by mass of water to prepare a bottom water mixture;
[0035] Step 4: adding the pre-reaction mixture and the sodium sulfate solution dropwise to the bottom water mixture;
[0036] Step 5: After the dropwise addition is completed, the mixture is stirred at room temperature for 30 minutes to fully stir the mixture to react sufficiently to obtain a reaction mixture;
[0037] Step 6: Filter and wash the reaction mixture, and then dry it to obtain strip-shaped nano-barium sulfate.
[0038] Example 2
[0039] A method for preparing strip-shaped nano-barium sulfate, wherein each step and the reagents and process parameters used in each step are the same as those in Example 1, except that in step 1, 5 parts by mass of strontium sulfide are also added, while the mass parts of the barium sulfide slurry is 15.
[0040] Example 3
[0041] A method for preparing strip-shaped nano-barium sulfate, wherein each step and the reagents and process parameters used in each step are the same as those in Example 2, except that the mixture between step 4 and step 5 is subjected to ultrasonic oscillation at 60 degrees Celsius, wherein the power is 300 W and the oscillation time is 20 minutes.
[0042] Example 4
[0043] A method for preparing strip-shaped nano-barium sulfate, wherein each step and the reagents and process parameters used in each step are the same as those in Example 1, except that in step 1, 8 parts by mass of barium chloride are further added, and the pH is adjusted to 4.5.
[0044] Example 5
[0045] A method for preparing strip-shaped nano-barium sulfate comprises the following steps:
[0046] Step 1: Take 30 parts by mass of 1 mol / L barium sulfide slurry, add 0.6 parts by mass of EDTA-2Na and 0.2 parts by mass of sodium hexametaphosphate and 1.5 parts by mass of hydrochloric acid, mix well, and obtain a pre-reaction mixture;
[0047] Step 2: preparing 8 parts by mass of a 3 wt% concentration (parts by mass) sodium sulfate solution;
[0048] Step 3: Add 0.7 parts by mass of EDTA-2Na and 0.01 parts by mass of sodium octadecyl sulfate to 100 parts by mass of water to prepare a bottom water mixture;
[0049] Step 4: adding the pre-reaction mixture and the sodium sulfate solution dropwise to the bottom water mixture;
[0050] Step 5: After the dropwise addition is completed, the mixture is stirred at room temperature for 30 minutes to fully stir the mixture to react sufficiently to obtain a reaction mixture;
[0051] Step 6: Filter and wash the reaction mixture, and then dry it to obtain strip-shaped nano-barium sulfate.
[0052] Example 6
[0053] A method for preparing strip-shaped nano-barium sulfate, wherein each step, the reagents used in each step, and the process parameters are the same as those in Example 1, except that the reaction mixture is filtered and washed, then re-slurried, 1.0 parts by mass of a silane coupling agent is added, the pH value is adjusted to 4.0-5.0, stirred for 1-2 hours, and then dehydrated and dried to obtain strip-shaped nano-barium sulfate.
[0054] Example 7
[0055] A method for preparing strip-shaped nano-barium sulfate, wherein each step, the reagents used in each step, and the process parameters are the same as those in Example 1, except that stirring is started before the pre-reaction mixture and the sodium sulfate solution are added dropwise and the temperature is raised to 40-50°C.
[0056] Comparative Example 1
[0057] Ordinary barium sulfate was used as Comparative Example 1.
[0058] Comparative Example 2
[0059] The spherical hollow nano-barium sulfate obtained in Example 1 of the prior art (CN 113697838 A).
[0060] The products of the above embodiments and comparative examples were subjected to performance testing, and the results are as follows:
[0061] Table 1 - Performance test results of Examples 1-7 and Comparative Examples 1-2
[0062] Test items Whiteness L value Particle size D50 / nm Dispersion / um Aspect Ratio Example 1 99.32 160 25 5:1 Example 2 99.38 270 20 4:1 Example 3 99.23 110 30 4.5:1 Example 4 99.65 95 35 12:1 Example 5 99.54 120 25 8:1 Example 6 99.44 150 25 9:1 Example 7 99.37 190 20 6:1 Comparative Example 1 99.21 460 50 1.5:1 Comparative Example 2 99.30 98 - -
[0063] Each embodiment of the present invention prepares strip-shaped nano-barium sulfate. Figure 1 and Figure 2 The SEM scanning electron microscope image and particle size distribution diagram of the nano-scale strip-shaped nano-barium sulfate obtained in Example 4 are as follows: Figure 3 and Figure 4 The SEM scanning electron microscope image and particle size distribution diagram of the nano-scale strip-shaped nano-barium sulfate obtained in Example 2.
[0064] From the data in Table 1, it can be seen that the nano barium sulfate of each embodiment of the present invention has a higher whiteness L value than ordinary barium sulfate, and the particle size is also smaller and the aspect ratio is larger. After experimental testing, the strip-shaped nano barium sulfate of this embodiment is more excellent in improving the mechanics of plastics than the hollow spherical nano barium sulfate and ordinary barium sulfate.
[0065] When strontium sulfide is added to the reaction components, the inventors found that the addition of strontium sulfide can affect the morphology and structure of the crystal, thereby affecting the morphology and structure of the final nano-stripe nano-barium sulfate. From the data of Example 2, it can be seen that it is specifically manifested in that it is conducive to the growth of crystals, the particle size increases, and the aspect ratio is reduced.
[0066] When the mixture was treated with ultrasonic vibration at 60 degrees Celsius, the inventors found that ultrasonic treatment increased the dispersion in the system, thereby appropriately inhibiting the growth of crystals. From the data of Example 3, it can be seen that the particle size of the strip-shaped nano-barium sulfate was reduced.
[0067] It can be seen from the data of Example 4 that after adding barium chloride and maintaining an acidic environment, the reaction rate can be further slowed down, making the synthesis reaction rate more controllable, and then forming a complex salt with the complex is conducive to better dispersion and conversion into strip-shaped nano-barium sulfate. The specific data are reflected in the further reduction of the particle size of the strip-shaped nano-barium sulfate and the further improvement of the dispersion, and finally less impurities are generated, the whiteness is better, and the aspect ratio has a significant increase.
[0068] It can be seen from the data of Example 6 that when the reaction mixture is filtered and washed, and then re-slurried and then the silane coupling agent is added, it is beneficial to improve the dispersibility, and the addition of the silane coupling agent is beneficial to the downstream modification effect, so that the surface interaction between the polymer and the strip-shaped nano-barium sulfate is closer, the mechanical properties are further improved, and the aspect ratio has a certain increase.
[0069] From the data of Example 7, it can be seen that the stabilization temperature has a controlling effect on the formed morphology and can slightly reduce the particle size and bulk density.
[0070] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing strip-shaped nano-barium sulfate, characterized in that: The following steps are involved: S0: Add 0.05-0.6 mass parts of EDTA-2Na and 0.05-0.2 mass parts of phosphate to 10-30 mass parts of barium sulfide slurry and mix thoroughly to obtain a pre-reaction mixture, wherein the mass ratio of barium sulfide to the slurry is 10-30%; S1: preparing 3 to 8 parts by weight of a sodium sulfate solution having a concentration of 3 to 8 wt %; S2: adding 0.05-0.7 parts by mass of EDTA-2Na and 0.01-0.05 parts by mass of sodium octadecyl sulfonate or sodium octadecyl sulfate to 50-100 parts by mass of water to prepare a bottom water mixture; S3: adding the pre-reaction mixture and the sodium sulfate solution into the bottom water mixture; S4: stirring the mixture in S3 to make it fully react to obtain a reacted mixture; S5: filtering, washing and drying the reaction mixture to obtain strip-shaped nano-barium sulfate.
2. The preparation method according to claim 1, characterized in that: 3 to 10 parts by mass of barium chloride are further added to S0.
3. The preparation method according to claim 1, characterized in that: In S0, 1 to 5 parts by mass of strontium sulfide is also added, and the mass parts of the barium sulfide slurry is 10 to 15.
4. The preparation method according to claim 3, characterized in that: Between S2 and S4, the mixture in S3 is treated by ultrasonic oscillation at 40-60 degrees Celsius, wherein the power is 100-300 W and the oscillation time is 10-30 minutes.
5. The preparation method according to claim 1, characterized in that: In S0, the phosphate is trisodium phosphate, and the mass ratio of the EDTA-2Na to the trisodium phosphate is 1:1.
25.
6. The preparation method according to claim 1, characterized in that: In S3, before the pre-reaction mixture and the sodium sulfate solution are added dropwise, stirring is started and the temperature is raised to 40-50°C.
7. The preparation method according to claim 1, characterized in that: In S5, the reaction mixture is filtered, washed with water, and then re-slurried, and 0.1 to 1.0 parts by mass of a silane coupling agent is added, the pH value is adjusted to 4.0 to 5.0, stirred for 1 to 2 hours, and then dehydrated and dried to obtain strip-shaped nano-barium sulfate.
8. Use of strip-shaped nano-barium sulfate prepared by the preparation method according to any one of claims 1 to 7 in plastic modification.