A method for preparing ferric chloride at low cost

The existing chlorination was solved by treating the hydrochloric acid solution obtained by electrolysis using scrap iron filings and brine, combined with tartaric acid intercalation modified magnesium-aluminum-aluminum hydrotalcite material and modified sodium alginate/chitosan porous membrane treatment of brine. The problem of excessive use of hydrochloric acid in iron preparation has achieved the preparation of low-cost and high-purity iron chloride and the improvement of raw material utilization.

CN116332241BActive Publication Date: 2024-11-08GUANGXI HUANMIAO IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310274951.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-21
Publication Date
2024-11-08
Estimated Expiration
2043-03-21

AI Technical Summary

Technical Problem

The use of large amounts of hydrochloric acid in the existing preparation methods of ferric chloride leads to high preparation costs and has an impact on the environment.

Method used

The hydrochloric acid solution prepared by electrolyzing waste iron filings was used to react with the hydrochloric acid solution obtained by electrolyzing the brine, and the brine was treated by tartaric acid intercalation modified magnesium-aluminum-ferro-based hydrotalcite material and modified sodium alginate/chitosan porous membrane, and the waste gas was collected and burned. Hydrochloric acid reduces the preparation cost of iron chloride and improves raw material utilization.

Benefits of technology

The preparation of low-cost and high-purity iron chloride is realized, which reduces the preparation cost of iron chloride, and improves the utilization rate of raw materials through the reuse of waste gas and simplifies the process flow.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a low-cost method for preparing ferric chloride, comprising the following steps: adding sodium hypochlorite solution to brine for ammonia removal; pumping the ammonia-removed brine into an adsorption column containing tartaric acid-intercalated modified magnesium aluminum iron hydrotalcite material for further treatment, and then into a separator containing a modified sodium alginate / chitosan porous membrane for further treatment; concentrating the brine after the above treatment and then electrolyzing it, burning the chlorine and hydrogen obtained from the electrolysis, and capturing the combustion gas with deionized water to obtain a hydrochloric acid solution; mixing and stirring the waste iron filings and the hydrochloric acid solution to react, filtering the reaction solution after the reaction, introducing chlorine gas into the filtrate for oxidation, and cooling and crystallizing the oxidized solution to obtain ferric chloride. This invention uses waste iron filings as the iron source and the hydrochloric acid solution obtained from the electrolytic treatment of brine as the acid solution. The waste gas collected during the preparation process can be reused, greatly reducing the preparation cost of ferric chloride.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of inorganic material preparation, and in particular to a method for preparing ferric chloride at low cost. Background Art

[0002] Ferric chloride is a covalent inorganic compound, which is black-brown crystals or flakes. It has a melting point of 306°C and a boiling point of 316°C. It is easily soluble in water and has strong water absorption. It can absorb moisture in the air and deliquesce. Ferric chloride is a very important iron salt, mainly used for metal etching and sewage treatment. Etching includes etching of copper, stainless steel, aluminum and other materials. It has the advantages of good effect and low price for treating raw water with low oil content, but it brings the disadvantage of yellowing water color. Ferric chloride is also used for printing and dyeing roller engraving, electronic industry circuit board and fluorescent digital tube production. In the construction industry, ferric chloride is often used to prepare concrete to enhance the strength, corrosion resistance and waterproofness of concrete. It can also be prepared with ferrous chloride, calcium chloride, aluminum chloride, aluminum sulfate, hydrochloric acid and other materials to make concrete waterproofing agents. In the inorganic industry, it is used to manufacture other iron salts and inks. In the metallurgical industry, it is used as a chlorination extractor for extracting gold and silver. In the organic industry, it is used as a catalyst, oxidant and chlorinating agent. In the glass industry, it is used as a hot colorant for glassware. The soap industry uses it as a coagulant to recover glycerin from soap waste liquid. Due to the wide range of uses of ferric chloride, it is in great demand in the chemical industry.

[0003] The preparation method of ferric chloride mainly adopts hydrochloric acid and iron as raw materials to prepare at present, and the patent of application number 200910184059.X provides a kind of preparation method of ferric chloride, and the method adopts iron-containing raw material as natural iron ore above 40 meshes, and hydrochloric acid above 10wt%, and hydrochloric acid is equivalent or slightly excessive by ferric chloride molecular molar ratio, and reaction is carried out in liquid phase.Compared with prior art, it has: reaction preparation production safety, process conditions are not harsh, low requirements for production equipment, raw materials are easy to obtain, preparation cost is low, and iron ore does not contain harmful impurities substantially, and impurities in iron ore are easy to separate by precipitation, and purification is simple.Although the ferric chloride with higher purity can be obtained in the above-mentioned prior art, a large amount of hydrochloric acid needs to be used in the preparation process to increase the preparation cost of ferric chloride. Summary of the invention

[0004] The technical problem to be solved by the present invention is: in view of the shortcomings of the prior art, a method for preparing ferric chloride at a low cost is provided. The method uses scrap iron as an iron source and a hydrochloric acid solution obtained by electrolysis of brine as an acid solution. The waste gas collected during the preparation process can be reused, so that not only ferric chloride with higher purity is prepared, but also the preparation cost of ferric chloride is greatly reduced.

[0005] In order to solve the above technical problems, the technical solution of the present invention is:

[0006] A method for preparing ferric chloride at low cost comprises the following steps:

[0007] (1) adding sodium hypochlorite solution to brine to remove ammonia;

[0008] (2) the brine after ammonia removal is pumped into an adsorption column loaded with tartaric acid intercalated modified magnesium aluminum iron type hydrotalcite material for treatment, and then the brine enters a separator loaded with modified sodium alginate / chitosan porous membrane for treatment;

[0009] (3) The brine after the above treatment is concentrated and then electrolyzed, and the chlorine and hydrogen obtained by electrolysis are collected and placed in a burner for combustion treatment, and the gas after combustion is captured by deionized water to produce a hydrochloric acid solution;

[0010] (4) washing the scrap iron and mixing it with the hydrochloric acid solution prepared above, stirring and reacting, and then filtering the reaction solution after the reaction is completed, introducing chlorine gas into the filtered filtrate for oxidation, and cooling and crystallizing the oxidized solution to obtain ferric chloride.

[0011] As a preferred embodiment of the above technical solution, in step (1), the concentration of the sodium hypochlorite solution is 10-15wt%, and the flow rates of the brine and the sodium hypochlorite solution during the ammonia removal are 130-140m3, respectively. 3 / h, 200-220l / h.

[0012] As a preferred embodiment of the above technical solution, in step (2), the preparation method of the tartaric acid intercalation modified magnesium-aluminum-iron hydrotalcite material is: dissolving aluminum nitrate nonahydrate, iron nitrate nonahydrate and magnesium nitrate hexahydrate in deionized water to prepare a mixed metal salt solution, then adding potassium tartrate solution to the mixed metal salt solution, and slowly dripping sodium hydroxide solution into the mixed metal salt solution under nitrogen protection for co-precipitation and mixing, then transferring to a reactor for heating reaction, and finally cooling to room temperature for filtering, washing the filtered precipitate and drying to obtain the tartaric acid intercalation modified magnesium-aluminum-iron hydrotalcite material.

[0013] As a preferred embodiment of the above technical solution, in the mixed metal salt solution, the concentrations of aluminum nitrate nonahydrate, ferric nitrate nonahydrate and magnesium nitrate hexahydrate are 0.1-0.2 mol / L, 0.3-0.5 mol / L and 0.3-0.5 mol / L respectively; the concentration of the potassium tartrate solution is 0.4 mol / L, and the mass ratio of the mixed metal salt aqueous solution to the potassium tartrate solution is 2:(3-4).

[0014] As a preferred embodiment of the above technical solution, the concentration of the sodium hydroxide solution is 1-2 mol / L, the dropping speed is 5-6 ml / min, and the sodium hydroxide solution is added dropwise until the pH value of the solution reaches 11; the temperature of the coprecipitation mixing is room temperature, the time is 2-3 h, and the temperature of the temperature rising reaction is 110° C., and the time is 5-6 h.

[0015] As a preferred embodiment of the above technical solution, in step (2), the preparation method of the modified sodium alginate / chitosan porous membrane is: cellulose nanofibers, biochar and deionized water are mixed and stirred to disperse uniformly to obtain a dispersion, polyethylene glycol 400 and sodium alginate are added to the dispersion and stirred at room temperature, then chitosan acetic acid solution is added to mix uniformly, allowed to stand, and finally the mixture is placed in a mold for drying, and then calcium chloride solution is added dropwise to the mold for cross-linking reaction, and then after the reaction is completed, deionized water is used for washing and drying to obtain a porous gel membrane.

[0016] As a preferred embodiment of the above technical solution, the mass concentrations of cellulose nanofibers and biochar in the dispersion are 0.3-0.5wt% and 0.5-1wt% respectively; the mass ratio of the cellulose nanofibers, polyethylene glycol 400, and sodium alginate is 1:(10-11):(5-6); the acetic acid solution of chitosan is prepared by dissolving 1g of chitosan in 50ml of 1wt% acetic acid aqueous solution; the mass ratio of the acetic acid solution of chitosan to sodium alginate is 50:(1-2).

[0017] As a preferred embodiment of the above technical solution, the rotation speed of the continuous stirring treatment at room temperature is 500-800 rpm, and the time is 5-6 hours; the temperature of the static treatment is room temperature, and the time is 8-10 hours; the concentration of the calcium chloride solution is 5-6wt%, the mass ratio of the calcium chloride solution to the acetic acid solution of chitosan is (5-10):1, and the temperature of the cross-linking reaction is room temperature, and the time is 1-2 hours.

[0018] As a preferred embodiment of the above technical solution, in step (3), the temperature of the combustion treatment is 700° C., and the concentration of the hydrochloric acid solution is 30-35wt%.

[0019] As a preferred embodiment of the above technical solution, in step (4), chlorine is introduced into the filtered filtrate for oxidation, and the unreacted chlorine and the gas generated when the scrap iron and the hydrochloric acid solution react are used in the combustion treatment process in step (3); the mass ratio of the scrap iron and the hydrochloric acid solution is 1:(3-4); the reaction is stirred until the pH of the solution is 4-5 to terminate the reaction; the oxidation time is 1-2h, and the amount of chlorine introduced is 4-7wt% of the mass of the filtrate.

[0020] Due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0021] The invention uses brine as a raw material, then performs ammonia removal treatment on the brine, then performs impurity removal to remove metal ions in the brine, performs electrolysis treatment on the impurity-removed brine to prepare chlorine and hydrogen, reacts the collected chlorine and hydrogen to generate hydrogen chloride and prepares a hydrochloric acid solution, and finally mixes the hydrochloric acid solution with waste iron filings to react to prepare ferric chloride; the method is simple to operate and has a low preparation cost; waste gas in the preparation process of ferric chloride can also be reused in the preparation of hydrochloric acid, thereby greatly improving the utilization rate of the raw materials.

[0022] The present invention sequentially uses tartaric acid intercalation modified magnesium aluminum iron hydrotalcite material and porous gel membrane for treatment when removing impurities from brine. The tartaric acid intercalation modified magnesium aluminum iron hydrotalcite material has a multilayer structure, is environmentally friendly and non-toxic, and can effectively remove metal ions in brine through ion exchange and complexation of surface active groups with metal ions. Tartaric acid intercalation modification effectively improves the complexation of layered hydrotalcite material with metal ions, further improving the removal effect of metal ions. The porous gel membrane used in the present invention is based on a double network gel formed by sodium alginate and chitosan, and then modified by cellulose nanofibers and biochar. The synergistic addition of biochar and cellulose nanofibers can improve the mechanical properties of the porous gel membrane on the one hand, and on the other hand, can improve the interception ability of the porous gel membrane to pollutants, improve the service life of the porous gel membrane, and further reduce the preparation cost of ferric chloride. DETAILED DESCRIPTION

[0023] The present invention will be further described below in conjunction with the examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention.

[0024] Example 1

[0025] 0.1 mol of aluminum nitrate nonahydrate, 0.3 mol of ferric nitrate nonahydrate and 0.3 mol of magnesium nitrate hexahydrate were dissolved in 1 L of deionized water to prepare a mixed metal salt solution, and then 1.5 L of a potassium tartrate solution with a concentration of 0.4 mol / L was added to the mixed metal salt solution, and a sodium hydroxide solution with a concentration of 1.5 mol / L was slowly dripped into the mixed metal salt solution under nitrogen protection to adjust the solution pH to 11, and co-precipitation was mixed for 2 hours, and then the mixture was transferred to a reactor and heated to 110° C. for reaction for 5 hours, and finally cooled to room temperature for filtration, and the filtered precipitate was washed and dried to obtain a tartaric acid intercalation modified magnesium aluminum iron hydrotalcite material;

[0026] 0.5 g of cellulose nanofibers, 0.8 g of biochar and 100 ml of deionized water were mixed and stirred to disperse uniformly to obtain a dispersion, 5 g of polyethylene glycol 400 and 2.5 g of sodium alginate were added to the dispersion, and the mixture was stirred at room temperature and a speed of 500 rpm for 5 h, then 125 g of chitosan acetic acid solution was added and mixed uniformly, and the mixture was allowed to stand at room temperature for 8 h, and finally the mixture was placed in a mold for drying, and then 650 g of 5 wt% calcium chloride solution was added dropwise to the mold for cross-linking reaction for 1 h, and then after the end, the mixture was washed and dried with deionized water to obtain a porous gel membrane;

[0027] A 10 wt% sodium hypochlorite solution was added to the brine for ammonia removal. The flow rates of the brine and the sodium hypochlorite solution were 130 m3 and 130 m4, respectively. 3 / h, 200l / h; the brine after ammonia removal is pumped into an adsorption column loaded with tartaric acid intercalated modified magnesium aluminum iron type hydrotalcite material for treatment, and then the brine enters a separator loaded with modified sodium alginate / chitosan porous membrane for treatment; the brine after the above treatment is concentrated and then electrolyzed, and the chlorine and hydrogen obtained by electrolysis are collected and placed in a burner at 700°C for combustion treatment, and the gas after combustion is captured by deionized water to obtain a hydrochloric acid solution with a concentration of 30wt%;

[0028] The washed scrap iron was mixed with the hydrochloric acid solution prepared above at a mass ratio of 1:3, and stirred to react until the pH of the solution reached 4-5 to terminate the reaction. The reaction solution was filtered, and chlorine gas was introduced into the filtered filtrate for oxidation for 1 hour. The amount of chlorine introduced was 4wt% of the mass of the filtrate. The oxidized solution was cooled and crystallized to obtain ferric chloride.

[0029] Example 2

[0030] 0.2 mol of aluminum nitrate nonahydrate, 0.5 mol of ferric nitrate nonahydrate and 0.5 mol of magnesium nitrate hexahydrate were dissolved in 1 L of deionized water to prepare a mixed metal salt solution, and then 1.5 L of a potassium tartrate solution with a concentration of 0.4 mol / L was added to the mixed metal salt solution, and a sodium hydroxide solution with a concentration of 2 mol / L was slowly dripped into the mixed metal salt solution under nitrogen protection to adjust the solution pH to 11, and co-precipitation was mixed for 3 hours, and then the mixture was transferred to a reactor and heated to 110° C. for reaction for 6 hours, and finally cooled to room temperature for filtration, and the filtered precipitate was washed and dried to obtain a tartaric acid intercalation modified magnesium aluminum iron hydrotalcite material;

[0031] 0.5 g of cellulose nanofibers, 0.8 g of biochar and 100 ml of deionized water were mixed and stirred to disperse uniformly to obtain a dispersion, 5 g of polyethylene glycol 400 and 2.5 g of sodium alginate were added to the dispersion, and the mixture was stirred at room temperature and 800 rpm for 6 h, then 125 g of chitosan acetic acid solution was added and mixed uniformly, and the mixture was allowed to stand at room temperature for 10 h, and finally the mixture was placed in a mold for drying, and then 650 g of 6 wt % calcium chloride solution was added dropwise to the mold for cross-linking reaction for 2 h, and then after the end, the mixture was washed and dried with deionized water to obtain a porous gel membrane;

[0032] A 15 wt% sodium hypochlorite solution was added to the brine to remove ammonia. The flow rates of the brine and the sodium hypochlorite solution were 140 m 3 / h, 220l / h; the brine after ammonia removal is pumped into an adsorption column equipped with tartaric acid intercalated modified magnesium aluminum iron type hydrotalcite material for treatment, and then the brine enters a separator loaded with modified sodium alginate / chitosan porous membrane for treatment; the brine after the above treatment is concentrated and then electrolyzed, and the chlorine and hydrogen obtained by electrolysis are collected and placed in a burner at 700°C for combustion treatment, and the gas after combustion is captured with deionized water to obtain a hydrochloric acid solution with a concentration of 30wt%;

[0033] The cleaned scrap iron was mixed with the hydrochloric acid solution prepared above at a mass ratio of 1:4, and stirred to react until the pH of the solution reached 4-5 to terminate the reaction. The reaction solution was filtered, and chlorine gas was introduced into the filtered filtrate for oxidation for 2 hours. The amount of chlorine introduced was 7wt% of the mass of the filtrate. The oxidized solution was cooled and crystallized to obtain ferric chloride.

[0034] Example 3

[0035] 0.15 mol of aluminum nitrate nonahydrate, 0.35 mol of ferric nitrate nonahydrate and 0.35 mol of magnesium nitrate hexahydrate were dissolved in 1 L of deionized water to prepare a mixed metal salt solution, and then 1.5 L of a potassium tartrate solution with a concentration of 0.4 mol / L was added to the mixed metal salt solution, and a sodium hydroxide solution with a concentration of 1.5 mol / L was slowly dripped into the mixed metal salt solution under nitrogen protection to adjust the solution pH to 11, and co-precipitation was mixed for 2 hours, and then the mixture was transferred to a reactor and heated to 110° C. for reaction for 5 hours, and finally cooled to room temperature for filtration, and the filtered precipitate was washed and dried to obtain a tartaric acid intercalation modified magnesium aluminum iron hydrotalcite material;

[0036] 0.5 g of cellulose nanofibers, 0.8 g of biochar and 100 ml of deionized water were mixed and stirred to disperse uniformly to obtain a dispersion, 5 g of polyethylene glycol 400 and 2.5 g of sodium alginate were added to the dispersion, and the mixture was stirred at room temperature and a speed of 500 rpm for 5.5 h, and then 125 g of chitosan acetic acid solution was added to mix uniformly, and the mixture was allowed to stand at room temperature for 8 h. Finally, the mixture was placed in a mold for drying, and then 650 g of 5.5 wt% calcium chloride solution was added dropwise to the mold for cross-linking reaction for 1 h. After the reaction was completed, the mixture was washed and dried with deionized water to obtain a porous gel membrane.

[0037] A sodium hypochlorite solution with a concentration of 11 wt% was added to the brine for ammonia removal. The flow rates of the brine and the sodium hypochlorite solution were 130 m 3 / h, 220l / h; the brine after ammonia removal is pumped into an adsorption column equipped with tartaric acid intercalated modified magnesium aluminum iron type hydrotalcite material for treatment, and then the brine enters a separator loaded with modified sodium alginate / chitosan porous membrane for treatment; the brine after the above treatment is concentrated and then electrolyzed, and the chlorine and hydrogen obtained by electrolysis are collected and placed in a burner at 700°C for combustion treatment, and the gas after combustion is captured with deionized water to obtain a hydrochloric acid solution with a concentration of 30wt%;

[0038] The cleaned scrap iron was mixed with the hydrochloric acid solution prepared above at a mass ratio of 1:3, and stirred until the pH of the solution reached 4-5 to terminate the reaction. The reaction solution was filtered, and chlorine gas was introduced into the filtered filtrate for oxidation for 2 hours. The amount of chlorine gas introduced was 5wt% of the mass of the filtrate. The oxidized solution was cooled and crystallized to obtain ferric chloride.

[0039] Example 4

[0040] 0.2 mol of aluminum nitrate nonahydrate, 0.4 mol of ferric nitrate nonahydrate and 0.4 mol of magnesium nitrate hexahydrate were dissolved in 1 L of deionized water to prepare a mixed metal salt solution, and then 1.5 L of a potassium tartrate solution with a concentration of 0.4 mol / L was added to the mixed metal salt solution, and a sodium hydroxide solution with a concentration of 1.5 mol / L was slowly dripped into the mixed metal salt solution under nitrogen protection to adjust the solution pH to 11, and co-precipitation was mixed for 2.5 hours, and then the mixture was transferred to a reactor and heated to 110° C. for reaction for 5 hours, and finally cooled to room temperature for filtration, and the filtered precipitate was washed and dried to obtain a tartaric acid intercalation modified magnesium aluminum iron hydrotalcite material;

[0041] 0.5 g of cellulose nanofibers, 0.8 g of biochar and 100 ml of deionized water were mixed and stirred to disperse uniformly to obtain a dispersion, 5 g of polyethylene glycol 400 and 2.5 g of sodium alginate were added to the dispersion, and the mixture was stirred at room temperature and a speed of 700 rpm for 5 h, then 125 g of chitosan acetic acid solution was added and mixed uniformly, and the mixture was allowed to stand at room temperature for 9 h, and finally the mixture was placed in a mold for drying, and then 650 g of 5 wt% calcium chloride solution was added dropwise to the mold for cross-linking reaction for 2 h, and then after the end, the mixture was washed and dried with deionized water to obtain a porous gel membrane;

[0042] A 12 wt% sodium hypochlorite solution was added to the brine for ammonia removal. The flow rates of the brine and the sodium hypochlorite solution were 130 m 3 / h, 200l / h; the brine after ammonia removal is pumped into an adsorption column loaded with tartaric acid intercalated modified magnesium aluminum iron type hydrotalcite material for treatment, and then the brine enters a separator loaded with modified sodium alginate / chitosan porous membrane for treatment; the brine after the above treatment is concentrated and then electrolyzed, and the chlorine and hydrogen obtained by electrolysis are collected and placed in a burner at 700°C for combustion treatment, and the gas after combustion is captured by deionized water to obtain a hydrochloric acid solution with a concentration of 30wt%;

[0043] The cleaned scrap iron was mixed with the hydrochloric acid solution prepared above at a mass ratio of 1:3, and stirred until the pH of the solution reached 4-5 to terminate the reaction. The reaction solution was filtered, and chlorine gas was introduced into the filtered filtrate for oxidation for 1 hour. The amount of chlorine introduced was 5wt% of the mass of the filtrate. The oxidized solution was cooled and crystallized to obtain ferric chloride.

[0044] Example 5

[0045] 0.15 mol of aluminum nitrate nonahydrate, 0.5 mol of ferric nitrate nonahydrate and 0.4 mol of magnesium nitrate hexahydrate were dissolved in 1 L of deionized water to prepare a mixed metal salt solution, and then 1.5 L of a potassium tartrate solution with a concentration of 0.4 mol / L was added to the mixed metal salt solution, and a sodium hydroxide solution with a concentration of 2 mol / L was slowly dripped into the mixed metal salt solution under nitrogen protection to adjust the solution pH to 11, and co-precipitation and mixing were performed for 3 hours, and then the mixture was transferred to a reactor and heated to 110° C. for reaction for 5 hours, and finally cooled to room temperature and filtered, and the filtered precipitate was washed and dried to obtain a tartaric acid intercalation modified magnesium aluminum iron hydrotalcite material;

[0046] 0.5 g of cellulose nanofibers, 0.8 g of biochar and 100 ml of deionized water were mixed and stirred to disperse uniformly to obtain a dispersion, 5 g of polyethylene glycol 400 and 2.5 g of sodium alginate were added to the dispersion, and the mixture was stirred at room temperature and 800 rpm for 5 h, then 125 g of chitosan acetic acid solution was added and mixed uniformly, and the mixture was allowed to stand at room temperature for 9 h, and finally the mixture was placed in a mold for drying, and then 650 g of 5.5 wt% calcium chloride solution was added dropwise to the mold for cross-linking reaction for 1 h, and then after the end, the mixture was washed and dried with deionized water to obtain a porous gel membrane;

[0047] A 14 wt% sodium hypochlorite solution was added to the brine for ammonia removal. The flow rates of the brine and the sodium hypochlorite solution were 130 m 3 / h, 200l / h; the brine after ammonia removal is pumped into an adsorption column loaded with tartaric acid intercalated modified magnesium aluminum iron type hydrotalcite material for treatment, and then the brine enters a separator loaded with modified sodium alginate / chitosan porous membrane for treatment; the brine after the above treatment is concentrated and then electrolyzed, and the chlorine and hydrogen obtained by electrolysis are collected and placed in a burner at 700°C for combustion treatment, and the gas after combustion is captured by deionized water to obtain a hydrochloric acid solution with a concentration of 30wt%;

[0048] The cleaned scrap iron was mixed with the hydrochloric acid solution prepared above at a mass ratio of 1:4, and stirred to react until the pH of the solution reached 4-5 to terminate the reaction. The reaction solution was filtered, and chlorine gas was introduced into the filtered filtrate for oxidation for 1 hour. The amount of chlorine introduced was 6wt% of the mass of the filtrate. The oxidized solution was cooled and crystallized to obtain ferric chloride.

[0049] In addition, it should be understood that after reading the contents of the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.

Claims

1. A method for preparing ferric chloride at low cost, It is characterized in that The following steps are involved: (1) Adding sodium hypochlorite solution to the brine to remove ammonia; (2) The brine after ammonia removal is pumped into an adsorption column loaded with tartaric acid intercalated modified magnesium aluminum iron hydrotalcite material for treatment, and then enters a separator loaded with modified sodium alginate / chitosan porous membrane for treatment; (3) The brine after the above treatment is concentrated and then electrolyzed. The chlorine and hydrogen obtained by electrolysis are collected and placed in a burner for combustion. The gas after combustion is captured by deionized water to produce a hydrochloric acid solution; (4) washing the scrap iron and mixing it with the hydrochloric acid solution prepared above, stirring and reacting, filtering the reaction solution after the reaction, introducing chlorine gas into the filtered filtrate for oxidation, cooling and crystallizing the oxidized solution to obtain ferric chloride; the unreacted chlorine gas when introducing chlorine gas into the filtered filtrate for oxidation and the gas generated when the scrap iron and the hydrochloric acid solution react are reused in the combustion treatment process in step (3); The modified sodium alginate / chitosan porous membrane is prepared by mixing and stirring cellulose nanofibers, biochar and deionized water to obtain a dispersion, adding polyethylene glycol 400 and sodium alginate to the dispersion and continuing to stir at room temperature, then adding chitosan acetic acid solution to mix evenly, standing, and finally placing the mixture in a mold for drying, then dropping calcium chloride solution into the mold for cross-linking reaction, and then washing and drying with deionized water after the reaction is completed to obtain a porous gel membrane.

2. A method for preparing ferric chloride at low cost according to claim 1, It is characterized in that In step (1), the concentration of the sodium hypochlorite solution is 10-15wt%, and the flow rates of the brine and the sodium hypochlorite solution during the ammonia removal are 130-140m 3 / h, 200-220L / h.

3. A method for preparing ferric chloride at low cost according to claim 1, It is characterized in that In step (2), the preparation method of the tartaric acid intercalation modified magnesium-aluminum-iron hydrotalcite material is as follows: aluminum nitrate nonahydrate, iron nitrate nonahydrate and magnesium nitrate hexahydrate are dissolved in deionized water to prepare a mixed metal salt solution, and then potassium tartrate solution is added to the mixed metal salt solution, and sodium hydroxide solution is slowly dripped into the mixed metal salt solution under nitrogen protection for co-precipitation and mixing, and then the mixture is transferred to a reactor for heating and reaction, and finally cooled to room temperature and filtered, and the filtered precipitate is washed and dried to obtain the tartaric acid intercalation modified magnesium-aluminum-iron hydrotalcite material.

4. A method for preparing ferric chloride at low cost according to claim 3, It is characterized in that In the mixed metal salt solution, the concentrations of aluminum nitrate nonahydrate, iron nitrate nonahydrate and magnesium nitrate hexahydrate are 0.1-0.2 mol / L, 0.3-0.5 mol / L and 0.3-0.5 mol / L respectively; the concentration of the potassium tartrate solution is 0.4 mol / L, and the mass ratio of the mixed metal salt solution to the potassium tartrate solution is 2:(3-4).

5. A method for preparing ferric chloride at low cost according to claim 3, It is characterized in that The concentration of the sodium hydroxide solution is 1-2 mol / L, and the dropping speed is 5-6 ml / min. The sodium hydroxide solution is added until the pH value of the solution reaches 11; the coprecipitation mixing temperature is room temperature, the time is 2-3 hours, and the temperature of the temperature rising reaction is 110° C., and the time is 5-6 hours.

6. A method for preparing ferric chloride at low cost according to claim 1, It is characterized in that The mass concentrations of cellulose nanofibers and biochar in the dispersion are 0.3-0.5wt% and 0.5-1wt% respectively; the mass ratio of the cellulose nanofibers, polyethylene glycol 400 and sodium alginate is 1:(10-11):(5-6); the acetic acid solution of chitosan is prepared by dissolving 1g of chitosan in 50ml of 1wt% acetic acid aqueous solution; the mass ratio of the acetic acid solution of chitosan to sodium alginate is 50:(1-2).

7. A method for preparing ferric chloride at low cost according to claim 1, It is characterized in that The rotation speed of the stirring treatment at room temperature is 500-800 rpm, and the time is 5-6 hours; the temperature of the static treatment is room temperature, and the time is 8-10 hours; the concentration of the calcium chloride solution is 5-6wt%, the mass ratio of the calcium chloride solution to the acetic acid solution of chitosan is (5-10):1, and the temperature of the cross-linking reaction is room temperature, and the time is 1-2 hours.

8. A method for preparing ferric chloride at low cost according to claim 1, It is characterized in that In step (3), the temperature of the combustion treatment is 700° C., and the concentration of the hydrochloric acid solution is 30-35 wt %.

9. A method for preparing ferric chloride at low cost according to claim 1, It is characterized in that In step (4), the mass ratio of the scrap iron and the hydrochloric acid solution is 1:(3-4); the reaction is stirred until the pH value of the solution reaches 4-5 to terminate the reaction; the oxidation time is 1-2h, and the amount of chlorine introduced is 4-7wt% of the mass of the filtrate.