Optical glass, preforms and optical components
By optimizing the composition ratio of La2O3, TiO2 and BaO, combined with the adjustment of SiO2 and B2O3, the problem of high manufacturing cost of high refractive index and high dispersion glass is solved, and the optical glass with high refractive index, low dispersion and low cost is achieved. It is suitable for high-refractive index, low-dispersion and low-cost optical glass. Precision optical components.
Patent Information
- Application Number
- CN202310219632.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2017-11-13
- Filing Date
- 2017-12-01
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2037-12-01
AI Technical Summary
The existing high-refractive index high-dispersion glass contains a large amount of materials such as GeO2, Nb2O5 and Ta2O5, which leads to high manufacturing costs and shows a wavelength of 5% spectral transmittance, making it difficult to achieve optical with both high refractive index, low dispersion and low cost. Glass.
By combining La2O3, TiO2 and BaO components, adjust the total amount of SiO2 and B2O3 and the mass ratio of TiO2/(TiO2+BaO) to optimize the composition of glass to obtain high refractive index and high dispersion, while reducing manufacturing costs and ensuring the display spectrum The wavelength of transmittance is 5%.
It realizes that while maintaining high refractive index and high dispersion, the manufacturing cost of optical glass is reduced, and the stability and visible light transmittance of glass are improved, and is suitable for high-precision optical component manufacturing.
Smart Images

Figure CN116332506B_ABST
Abstract
Description
[0001] This application is a divisional application of an application with a filing date of December 1, 2017, application number 201711251286.0, and invention name “Optical glass, preform and optical element”. Technical Field
[0002] The invention relates to an optical glass, a preform and an optical element. Background Art
[0003] In recent years, the digitization of instruments using optical systems or the high-definition of images and videos has been developing rapidly. In particular, the high-definition of images and videos is particularly prominent in optical instruments such as digital cameras, video cameras, and projectors. At the same time, in the optical systems included in these optical instruments, the number of optical elements such as lenses and prisms is reduced to achieve lightweight and miniaturization.
[0004] Among optical glasses used to manufacture optical elements, those with a high refractive index (n) of 1.90 or higher are particularly suitable for achieving lightweight and miniaturization of the entire optical system. d ), a low Abbe number (v d As such high refractive index and low dispersion glass, a glass composition represented by Patent Document 1 is known.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2011-178571 Summary of the invention
[0008] However, in order to promote high refractive index and high dispersion, the glass described in Patent Document 1 contains a large amount of components with high material unit price such as GeO2, Nb2O5 and Ta2O5, which has a problem of high manufacturing cost. Therefore, it is expected that there will be an optical glass having high refractive index and high dispersion, short wavelength (λ5) at which spectral transmittance is 5%, and low manufacturing cost.
[0009] In view of the above problems, an object of the present invention is to provide an optical glass having a high refractive index, a short wavelength (λ5) showing a spectral transmittance of 5%, and a low manufacturing cost, as well as a preform and an optical element using the optical glass.
[0010] In order to solve the above-mentioned problems, the inventors of the present invention have repeatedly conducted intensive experimental studies and found that by using La2O3, TiO2 and BaO components in combination while adjusting the total amount of SiO2 and B2O3 components or the mass ratio of TiO2 / (TiO2+BaO), the desired high refractive index and high dispersion can be obtained, the manufacturing cost can be suppressed, and the wavelength (λ5) showing 5% spectral transmittance can be shortened, thereby completing the present invention.
[0011] Specifically, the present invention provides the following contents.
[0012] (1) An optical glass, measured in terms of mass % based on oxides,
[0013] contain
[0014] Greater than 0% to 45.0% La2O3 content,
[0015] A TiO2 content greater than 0% to 45.0%, and
[0016] BaO content greater than 0% to 40.0%,
[0017] The total amount of SiO2 and B2O3 components contained is 5.0% or more and 30.0% or less,
[0018] The mass ratio of TiO2 / (TiO2+BaO) is 0.10 or more and 0.90 or less,
[0019] Refractive index (n d ) is above 1.90, and the Abbe number (v d ) is 30.0 or less, and the wavelength (λ5) showing a spectral transmittance of 5% is 400 nm or less.
[0020] (2) The optical glass according to (1), wherein
[0021] Measured in mass % based on oxides,
[0022] SiO2 content is 0 to 30.0%, and
[0023] The B2O3 content is 0 to 30.0%.
[0024] (3) The optical glass according to (1) or (2), wherein:
[0025] Measured in mass % based on oxides,
[0026] The ZnO content is 0 to 20.0%,
[0027] Y2O3 content is 0~15.0%,
[0028] Nb2O5 content is 0~25.0%,
[0029] The Yb2O3 content is 0 to 15.0%, and
[0030] The Gd2O3 component is 0 to 15.0%.
[0031] (4) The optical glass according to any one of (1) to (3), wherein
[0032] Measured in mass % based on oxides,
[0033] The mass sum of (La2O3+Nb2O5+Gd2O3+Yb2O3) is greater than 0% and less than 60.0%.
[0034] (5) The optical glass according to any one of (1) to (4), wherein
[0035] Measured in mass % based on oxides,
[0036] The total amount of Ln2O3 components (wherein Ln is one or more selected from the group consisting of La, Gd, Y, and Yb) is greater than 0% and less than 50.0%.
[0037] (6) The optical glass according to any one of (1) to (5), wherein
[0038] Calculated on an oxide basis,
[0039] TiO2 / BaO is greater than 0 and less than 3.00.
[0040] (7) The optical glass according to any one of (1) to (6), wherein
[0041] Measured in mass % based on oxides,
[0042] The mass sum of Rn2O components (wherein Rn is one or more selected from the group consisting of Li, Na, and K) is 15.0% or less.
[0043] (8) The optical glass according to any one of (1) to (7), wherein
[0044] Measured in mass % based on oxides,
[0045] The mass sum of RO components (wherein R is one or more selected from the group consisting of Mg, Ca, Sr, Ba, and Zn) is greater than 0% and less than or equal to 35.0%.
[0046] (9) The optical glass according to any one of (1) to (8), wherein
[0047] In terms of mass % based on oxides,
[0048] ZrO2 composition 0~20.0%,
[0049] Nb2O5 composition 0~15.0%,
[0050] WO3 component 0~10.0%,
[0051] Ta2O5 composition 0~10.0%,
[0052] MgO component 0~15.0%,
[0053] CaO content 0~15.0%,
[0054] SrO component 0~15.0%,
[0055] Li2O composition 0~15.0%,
[0056] Na2O component 0~15.0%,
[0057] K2O component 0~15.0%,
[0058] P2O5 composition 0~10.0%,
[0059] GeO2 composition 0~10.0%,
[0060] Al2O3 composition 0~15.0%,
[0061] Ga2O3 content 0~15.0%,
[0062] Bi2O3 composition 0~10.0%,
[0063] TeO2 composition 0~10.0%,
[0064] SnO2 content 0-3.0%, and
[0065] Sb2O3 content: 0~1.0%.
[0066] (10) A preform comprising the optical glass as described in any one of (1) to (9).
[0067] (11) An optical element comprising the optical glass according to any one of (1) to (9).
[0068] (12) An optical instrument comprising the optical element described in (11).
[0069] According to the present invention, it is possible to provide an optical glass having a high refractive index and high dispersion, a short wavelength (λ5) showing a spectral transmittance of 5%, and a low manufacturing cost, as well as a preform and an optical element using the optical glass. BRIEF DESCRIPTION OF THE DRAWINGS
[0070] Embodiments of the present invention will be described in detail based on the following drawings, in which:
[0071] Picture 1 The vertical axis is the partial dispersion ratio (θg, F) and the vertical axis is the Abbe number (v d ) is a schematic diagram of a normal line represented by rectangular coordinates of the horizontal axis; and
[0072] Picture 2 The partial dispersion ratio (θg, F) and the Abbe number (v d ) diagram of the relationship. DETAILED DESCRIPTION
[0073] The optical glass of the present invention contains, by mass%, more than 0% to 45.0% of La2O3, more than 0% to 45.0% of TiO2, and more than 0% to 40.0% of BaO, the total amount of SiO2 and B2O3 is 5.0% to 30.0%, the mass ratio of TiO2 / (TiO2+BaO) is 0.10 to 0.90, and the refractive index (n d ) is above 1.90, and the Abbe number (v d ) is 30.0 or less, and the wavelength (λ5) showing a spectral transmittance of 5% is 400 nm or less.
[0074] According to the present invention, by using La2O3, TiO2 and BaO together and adjusting the content of each component, it is possible to achieve high refractive index and high dispersion of glass and improve the stability of glass. Therefore, it is possible to provide an optical glass having high refractive index and high dispersion, a short wavelength (λ5) at which the spectral transmittance is 5%, and a low manufacturing cost, as well as a preform and an optical element using the optical glass.
[0075] [Glass composition]
[0076] The composition range of each component constituting the optical glass of the present invention is described below. In this specification, unless otherwise specified, the content of each component is expressed in mass % relative to the total mass of the glass on an oxide basis. Here, "oxide basis" means that the composition of each component contained in the glass is expressed by setting the total mass of the oxide to 100 mass % under the assumption that the oxides, composite salts, metal fluorides, etc. used as raw materials for the glass components of the present invention are all decomposed into oxides when melted.
[0077] <About essential ingredients and optional ingredients>
[0078] The La2O3 component is a component that can increase the refractive index of the glass and reduce dispersion when its content is greater than 0%. In particular, by containing more than 0% of the La2O3 component, the desired high refractive index can be obtained, and it is an essential component. Therefore, the lower limit of the content of the La2O3 component is preferably greater than 0%, more preferably 3.0%, further preferably 15.0%, further preferably 20.0%, further preferably 25.0%, and further preferably 27.0%.
[0079] On the other hand, by setting the content of La2O3 component to 45.0% or less, the devitrification resistance of glass can be improved, the increase in specific gravity of glass can be suppressed, and the manufacturing cost can be reduced. Therefore, the upper limit of the content of La2O3 component is preferably 45.0%, more preferably 40.0%, further preferably 38.0%, and further preferably 37.0%.
[0080] As the La2O3 component, La2O3, La(NO3)3.XH2O (X is an arbitrary integer) or the like can be used as a raw material.
[0081] TiO2 is an essential component that can increase the refractive index of glass, lower the Abbe number, increase the partial dispersion ratio, and improve the resistance to devitrification when its content is greater than 0%. Therefore, the lower limit of the content of TiO2 is preferably greater than 0%, preferably 5.0%, more preferably greater than 10.0%, further preferably 15.0%, further preferably 18.0%, and further preferably greater than 20.0%.
[0082] On the other hand, by setting the content of TiO2 component to 45.0% or less, the coloring of the glass can be reduced and the visible light transmittance can be improved. In addition, the devitrification caused by the excessive inclusion of TiO2 component can also be suppressed. Therefore, the upper limit of the content of TiO2 component is preferably 45.0%, more preferably 38.0%, further preferably 32.0%, further preferably 27.0%, and further preferably 25.0%.
[0083] The TiO2 component can use TiO2 or the like as a raw material.
[0084] BaO is an essential component that can improve the refractive index or devitrification resistance of glass and improve the meltability of glass raw materials when its content is greater than 0%. Therefore, the lower limit of the content of BaO is preferably greater than 0%, more preferably 5.0%, further preferably 8.0%, and further preferably 10.0%.
[0085] On the other hand, by setting the content of the BaO component to 40.0% or less, the refractive index of the glass is not easily reduced, and the devitrification of the glass can be reduced. Therefore, the upper limit of the content of the BaO component is preferably 40.0%, more preferably 35.0%, further preferably 28.0%, further preferably 23.0%, and further preferably 20.0%.
[0086] BaO component can use BaCO3, Ba(NO3)2 or the like as a raw material.
[0087] The sum (mass sum) of the contents of the B2O3 component and the SiO2 component is preferably 5.0% or more and 30.0% or less.
[0088] In particular, by setting the sum to 5.0% or more, it is possible to suppress the reduction in resistance to devitrification due to insufficient B2O3 or SiO2 components. Therefore, the lower limit of the mass sum (B2O3+SiO2) is preferably 5.0%, more preferably 7.0%, and further preferably 9.0%.
[0089] On the other hand, by setting the sum to less than 30.0%, the reduction in refractive index due to excessive inclusion of these components can be suppressed, thereby making it easy to obtain the desired high refractive index. Therefore, the upper limit of the mass sum (B2O3+SiO2) is preferably 30.0%, more preferably 23.0%, further preferably 18.0%, and further preferably 16.5%.
[0090] Here, the ratio (mass ratio) of the content of TiO2 to the sum of the contents of the TiO2 component and the BaO component is preferably 0.10 or more. Thus, a high partial dispersion ratio can be obtained while maintaining a high refractive index and a high dispersion. Therefore, the lower limit of the mass ratio TiO2 / (TiO2+BaO) is preferably 0.10, more preferably 0.30, further preferably 0.40, and further preferably 0.45.
[0091] On the other hand, by setting the mass ratio to less than 0.90, the coloring of the glass can be reduced, the visible light transmittance can be increased, and devitrification can be suppressed. Therefore, the upper limit of the mass ratio TiO2 / (TiO2+BaO) is preferably 0.90, more preferably 0.80, further preferably 0.73, and further preferably 0.68.
[0092] The SiO2 component is an arbitrary component that can improve the devitrification resistance when its content is greater than 0%. Therefore, the lower limit of the content of the SiO2 component is preferably greater than 0%, more preferably greater than 0.5%, further preferably greater than 1.0%, and further preferably greater than 2.0%.
[0093] On the other hand, by setting the content of SiO2 component to below 30.0%, SiO2 component can be easily melted in molten glass and avoided from melting at high temperature. The upper limit of the content of SiO2 component is preferably 30.0%, more preferably 23.0%, further preferably 16.0%, further preferably 11.0%, and further preferably 9.0%.
[0094] SiO2 component can use SiO2, K2SiF6, Na2SiF6 and the like as raw materials.
[0095] The B2O3 component is an arbitrary component that can form a network structure inside the glass when its content is greater than 0%, promote stable glass formation, and improve resistance to devitrification. Therefore, the lower limit of the content of the B2O3 component is preferably greater than 0%, more preferably greater than 0.5%, further preferably greater than 1.0%, and further preferably greater than 2.0%.
[0096] On the other hand, by setting the content of the B2O3 component to 30.0% or less, the decrease in the refractive index can be suppressed, the Abbe number can be reduced, and the deterioration of chemical durability can be suppressed. Therefore, the upper limit of the content of the B2O3 component is preferably 30.0% or less, more preferably 20.0%, further preferably less than 15.0%, further preferably 12.0%, and further preferably less than 10.0%.
[0097] The B2O3 component can be made of H3BO3, Na2B4O7, Na2B4O7·10H2O, BPO4, etc.
[0098] The ZnO component is an arbitrary component that can improve the meltability of glass, lower the glass transition temperature, and reduce devitrification when its content is greater than 0%. Therefore, the lower limit of the content of the ZnO component is preferably greater than 0%, more preferably greater than 0.5%, further preferably greater than 1.0%, and further preferably greater than 1.5%.
[0099] On the other hand, by setting the content of the ZnO component to 20.0% or less, the refractive index or devitrification can be reduced. In addition, since the viscosity of the molten glass can be increased, the generation of glass streaks can be reduced. Therefore, the upper limit of the content of the ZnO component is preferably 20.0%, more preferably 15.0%, further preferably 11.0%, and further preferably 8.0%.
[0100] The ZnO component can use ZnO, ZnF2, etc. as a raw material.
[0101] The Y2O3 component is an arbitrary component which can suppress an increase in the material cost of glass when the content thereof is greater than 0%.
[0102] By setting the content of the Y2O3 component to 15.0% or less, the reduction in the refractive index of the glass can be suppressed, the Abbe number can be reduced, and the devitrification resistance of the glass can be improved. Therefore, the upper limit of the content of the Y2O3 component is preferably 15.0%, more preferably 10.0%, and further preferably 5.0%.
[0103] The Y2O3 component can use Y2O3, YF3 and the like as raw materials.
[0104] The Nb2O5 component is an arbitrary component that can increase the refractive index of the glass and improve the devitrification resistance when its content is greater than 0%. Therefore, the lower limit of the content of the Nb2O5 component is preferably greater than 0%, more preferably 2.0%, and further preferably 4.0%.
[0105] On the other hand, by setting the content of the Nb2O5 component to 25.0% or less, it is possible to suppress the reduction in the devitrification resistance of the glass or the reduction in the transmittance of visible light caused by the excessive inclusion of the Nb2O5 component, and to suppress the increase in the material cost of the glass. Therefore, the upper limit of the content of the Nb2O5 component is preferably 25.0%, more preferably 20.0%, further preferably 16.0%, and further preferably 13.0%.
[0106] The Nb2O5 component can use Nb2O5 or the like as a raw material.
[0107] The Yb2O3 component is an arbitrary component that can increase the refractive index of glass when its content exceeds 0%.
[0108] On the other hand, by setting the content of the Yb2O3 component to 15.0% or less, the devitrification resistance of the glass can be improved and the Abbe number can be reduced. Therefore, the upper limit of the content of the Yb2O3 component is preferably 15.0%, more preferably 10.0%, and further preferably 5.0%.
[0109] Yb2O3 component can use Yb2O3 or the like as a raw material.
[0110] The Gd2O3 component is an arbitrary component which can increase the refractive index of the glass and the Abbe number when the content thereof is greater than 0%.
[0111] On the other hand, by reducing the particularly expensive Gd2O3 component among the rare earth elements to below 15.0%, the material cost of the glass can be reduced, thereby making it possible to produce cheaper optical glass. In addition, the rise of the Abbe number of the glass above the necessary level can be suppressed thereby. Therefore, the upper limit of the content of the Gd2O3 component is preferably 15.0%, more preferably 10.0%, and further preferably 5.0%.
[0112] The Gd2O3 component can use Gd2O3, GdF3 or the like as a raw material.
[0113] In addition, in the optical glass of the present invention, the sum (mass sum) of the contents of La2O3, Nb2O5, Gd2O3 and Yb2O3 is preferably 60.0% or less. Thus, the contents of these expensive components can be reduced, thereby suppressing the material cost of the glass and reducing the Abbe number. Therefore, the upper limit of the mass sum (La2O3+Nb2O5+Gd2O3+Yb2O3) is preferably 60.0%, more preferably 57.0%, further preferably 53.0%, further preferably 49.0%, and further preferably 47.0%.
[0114] On the other hand, by containing the mass sum of these components greater than 0%, the desired high refractive index can be obtained. Therefore, the lower limit of the mass sum (La2O3+Nb2O5+Gd2O3+Yb2O3) is preferably greater than 0%, more preferably 10.0%, further preferably 20.0%, further preferably 25.0%, further preferably 30.0%, and further preferably 35.0%.
[0115] The sum (mass sum) of the contents of the Ln2O3 component (Ln is one or more selected from the group consisting of La, Gd, Y, and Yb) is preferably greater than 0% to 50.0%.
[0116] In particular, by setting the mass sum to be greater than 0%, the refractive index of the glass can be increased, thereby making it easy to obtain high-refractive index glass. In addition, the coloring of the glass can be reduced. Therefore, the lower limit of the mass sum of the content of the Ln2O3 component is preferably greater than 0%, more preferably 1.0%, further preferably 3.0%, and further preferably 5.0%.
[0117] On the other hand, by setting the mass sum to 50.0% or less, the devitrification resistance can be improved and the Abbe number can be reduced. Therefore, the upper limit of the mass sum of the content of the Ln2O3 component is preferably 50.0%, more preferably less than 40.0%, further preferably 30.0%, and further preferably 25.0%.
[0118] Here, the ratio (mass ratio) of the content of TiO2 to the sum of the contents of the La2O3 component, the Nb2O5 component, the Gd2O3 component, and the Yb2O3 component is preferably greater than 0. Thus, a high partial dispersion ratio can be obtained while maintaining a high refractive index and a high dispersion, and the manufacturing cost can be reduced. Therefore, the lower limit of the mass ratio TiO2 / (La2O3+Nb2O5+Gd2O3+Yb2O3) is preferably greater than 0, more preferably 0.10, further preferably 0.20, and further preferably 0.40.
[0119] On the other hand, by setting the mass ratio to less than 2.00, the coloring of the glass can be reduced, the visible light transmittance can be increased, and devitrification can be suppressed. Therefore, the upper limit of the mass ratio TiO2 / (La2O3+Nb2O5+Gd2O3+Yb2O3) is preferably 2.00, more preferably 1.00, further preferably 0.80, and further preferably 0.66.
[0120] Here, the ratio (mass ratio) of the content of the TiO2 component to the content of the BaO component is preferably greater than 0. Thus, a high partial dispersion ratio can be obtained while maintaining a high refractive index and a high dispersion. The lower limit of the mass ratio TiO2 / BaO is preferably greater than 0, more preferably 0.10, further preferably 0.40, and further preferably 0.60.
[0121] On the other hand, by setting the mass ratio to 3.00 or less, the coloring of the glass can be reduced, the visible light transmittance can be increased, and devitrification can be suppressed. Therefore, the upper limit of the mass ratio TiO2 / BaO is preferably 3.00, more preferably 2.00, and further preferably 1.60.
[0122] Here, the ratio (mass ratio) of the sum of the contents of the TiO2 component and the WO3 component to the content of the BaO component is preferably greater than 0. Thus, a high partial dispersion ratio can be obtained while maintaining a high refractive index and a high dispersion, and the devitrification resistance can be improved. Therefore, the lower limit of the mass ratio (TiO2+WO3) / BaO is preferably greater than 0, more preferably 0.30, further preferably 0.60, further preferably 0.80, and further preferably 1.00.
[0123] On the other hand, by setting the mass ratio to 3.00 or less, the coloring of the glass can be reduced, the visible light transmittance can be increased, and devitrification can be suppressed. Therefore, the upper limit of the mass ratio (TiO2+WO3) / BaO is preferably 3.00, more preferably 2.50, and further preferably 1.90.
[0124] The sum (mass sum) of the contents of TiO2 and Nb2O5 is preferably greater than 0%. This can increase the refractive index / dispersion and improve the resistance to devitrification. Therefore, the lower limit of the mass sum (TiO2+Nb2O5) is preferably greater than 0%, more preferably greater than 10.0%, further preferably greater than 15.0%, further preferably greater than 20.0%, and further preferably greater than 25.0%.
[0125] On the other hand, by setting the content of the sum to 60.0% or less, the coloring of the glass can be reduced, the visible light transmittance can be increased, and devitrification can be suppressed. Therefore, the upper limit of the content of the mass sum is preferably 60.0%, more preferably 50.0%, further preferably 45.0%, further preferably 40.0%, further preferably 35.0%, and further preferably 33.0%.
[0126] The total amount of Rn2O components (wherein Rn is one or more selected from the group consisting of Li, Na, K, and Cs) is preferably 15.0% or less. Thus, the reduction in the refractive index of the glass can be suppressed and the resistance to devitrification can be improved. Therefore, the upper limit of the mass sum of the Rn2O components is preferably 15.0%, more preferably 10.0%, further preferably less than 5.0%, and further preferably less than 1.0%.
[0127] The sum (mass sum) of the contents of the RO component (wherein R is one or more selected from the group consisting of Mg, Ca, Sr, and Ba) is preferably 35.0% or less. Thus, devitrification caused by excessive inclusion of the RO component can be reduced, and the reduction in the refractive index can be suppressed. Therefore, the upper limit of the mass sum of the contents of the RO component is preferably 35.0%, more preferably 30.0%, further preferably 27.0%, further preferably less than 23.0%, and further preferably 20.0%.
[0128] On the other hand, by making the sum greater than 0%, the meltability of glass raw materials or the stability of glass can be improved. Therefore, the lower limit of the total content of RO components is preferably greater than 0%, more preferably 4.0%, further preferably 7.0%, and further preferably greater than 9.0%.
[0129] When the content of ZrO2 is greater than 0%, it can contribute to the high refractive index and low dispersion of the glass, and can improve the resistance of the glass to devitrification. Therefore, the lower limit of the content of ZrO2 is preferably greater than 0%, more preferably 0.5%, and further preferably 1.0%.
[0130] On the other hand, by setting the ZrO2 component to 20.0% or less, it is possible to suppress the reduction in the devitrification resistance of the glass or the increase in the Abbe number above the necessary level due to the excessive inclusion of the ZrO2 component. Therefore, the upper limit of the content of the ZrO2 component is preferably 20.0%, more preferably 16.0%, further preferably 12.0%, further preferably 9.0%, and further preferably less than 6.5%.
[0131] The ZrO2 component can use ZrO2, ZrF4, etc. as a raw material.
[0132] The WO3 component is an arbitrary component that can increase the refractive index, improve the partial dispersion ratio, and improve the resistance to devitrification of the glass while reducing the coloring of the glass caused by other high-refractive index components when its content is greater than 0%. In addition, the WO3 component is also a component that can reduce the glass transition temperature. Therefore, the lower limit of the content of the WO3 component is preferably greater than 0%, more preferably 0.1%, further preferably 0.2%, and further preferably 0.3%.
[0133] On the other hand, by setting the content of WO3 component to 10.0% or less, the coloring of the glass caused by WO3 component can be reduced and the visible light transmittance can be improved. Therefore, the upper limit of the content of WO3 component is preferably 10.0%, more preferably 5.0%, and further preferably 3.0%.
[0134] The WO3 component can use WO3 or the like as a raw material.
[0135] The Ta2O5 component is an arbitrary component which can increase the refractive index of the glass and improve the devitrification resistance when the content thereof exceeds 0%.
[0136] On the other hand, by making expensive Ta2O5 component as 10.0% or less, the material cost of glass can be reduced, thereby cheaper optical glass can be made. In addition, by making the content of Ta2O5 component as 10.0% or less, the melting temperature of raw materials can be reduced, the energy required for raw material melting can be reduced, thereby the manufacturing cost of optical glass can be reduced. Therefore, the upper limit of the content of Ta2O5 component is preferably 10.0%, more preferably 8.0%, and further preferably 5.0%. Especially, from the viewpoint of manufacturing cheaper optical glass, the upper limit of the content of Ta2O5 component is preferably 4.0%, more preferably 3.0%, and further more preferably less than 1.0%, and most preferably does not contain.
[0137] Ta2O5 component can use Ta2O5 etc. as a raw material.
[0138] The MgO component is an arbitrary component that can improve the meltability of glass raw materials or the devitrification resistance of glass when the content thereof exceeds 0%.
[0139] On the other hand, by setting the content of the MgO component to 15.0% or less, it is possible to suppress the reduction in refractive index or reduction in devitrification resistance due to excessive inclusion of these components. Therefore, the upper limit of the content of the MgO component is preferably 15.0%, more preferably 10.0%, and further preferably 5.0%.
[0140] The MgO component can use MgCO3, MgF2, etc. as a raw material.
[0141] The CaO component is an arbitrary component that can improve the refractive index or devitrification resistance of the glass and improve the meltability of the glass raw material when its content is greater than 0%. Therefore, the lower limit of the content of the CaO component is preferably greater than 0%, more preferably 0.5%, further preferably 1.5%, and further preferably 3.0%.
[0142] On the other hand, by setting the content of the CaO component to 15.0% or less, the refractive index of the glass is less likely to decrease, and devitrification of the glass can be reduced. Therefore, the upper limit of the content of the CaO component is preferably 15.0%, more preferably 10.0%, and further preferably 5.0%.
[0143] The CaO component can use CaCO3, CaF2, etc. as a raw material.
[0144] The SrO component is an arbitrary component that can increase the refractive index or devitrification resistance of the glass and improve the meltability of the glass raw material when its content is greater than 0%. Therefore, the lower limit of the content of the SrO component is preferably greater than 0%, more preferably 0.5%, further preferably 1.5%, and further preferably 3.0%.
[0145] On the other hand, by setting the content of the SrO component to 15.0% or less, the refractive index of the glass is less likely to decrease, and the devitrification of the glass can be reduced. Therefore, the upper limit of the content of the SrO component is preferably 15.0%, more preferably 10.0%, and further preferably 5.0%.
[0146] The SrO component can use SrCO3, SrF2, etc. as a raw material.
[0147] The Li2O component, the Na2O component, and the K2O component are arbitrary components that can improve the meltability of the glass when the content of at least any one of them is greater than 0%. In particular, the K2O component is also a component that can further increase the partial dispersion ratio of the glass.
[0148] On the other hand, by reducing the content of Li2O, Na2O or K2O, the refractive index of the glass can be suppressed from decreasing, and devitrification can be reduced. In particular, by reducing the content of Li2O, the partial dispersion ratio of the glass can be suppressed from decreasing. Therefore, the content of at least one of the Li2O, Na2O and K2O components is preferably 15.0%, more preferably less than 10.0%, further preferably less than 5.0%, and further preferably less than 1.0%.
[0149] Li2O component, Na2O component and K2O component can use Li2CO3, LiNO3, LiF, Na2CO3, NaNO3, NaF, Na2SiF6, K2CO3, KNO3, KF, KHF2, K2SiF6 and the like as raw materials.
[0150] The P2O5 component is an arbitrary component that can improve the devitrification resistance of the glass when its content is greater than 0%. In particular, by setting the content of the P2O5 component to 10.0% or less, it is possible to suppress the reduction of the chemical durability of the glass, especially the reduction of the water resistance. Therefore, the upper limit of the content of the P2O5 component is preferably 10.0%, more preferably 5.0%, and further preferably 3.0%.
[0151] The P2O5 component can use Al(PO3)3, Ca(PO3)2, Ba(PO3)2, BPO4, H3PO4 and the like as raw materials.
[0152] The GeO2 component is an arbitrary component that can increase the refractive index of the glass and improve the resistance to devitrification of the glass when its content is greater than 0%. However, since the raw material price of GeO2 is high, if the amount used is large, the material cost will increase, thereby weakening the cost reduction effect brought about by reducing the Gd2O3 component or the Ta2O5 component. Therefore, the upper limit of the content of the GeO2 component is preferably 10.0%, more preferably 5.0%, further preferably 1.0%, and most preferably not contained.
[0153] The GeO2 component can use GeO2 or the like as a raw material.
[0154] The Al 2 O 3 component and the Ga 2 O 3 component are arbitrary components that can improve the chemical durability of the glass and improve the devitrification resistance of the glass when the content thereof is greater than 0%.
[0155] On the other hand, by setting the content of each of the Al2O3 component and the Ga2O3 component to 15.0% or less, the reduction in the devitrification resistance of the glass caused by the excessive inclusion of these components can be suppressed. Therefore, the upper limit of the content of each of the Al2O3 component and the Ga2O3 component is preferably 15.0%, more preferably 8.0%, and further preferably 3.0%.
[0156] Al2O3 component and Ga2O3 component can use Al2O3, Al(OH)3, AlF3, Ga2O3, Ga(OH)3 or the like as raw materials.
[0157] The Bi2O3 component is an arbitrary component that can increase the refractive index and lower the glass transition temperature when the content thereof is greater than 0%.
[0158] On the other hand, by setting the content of Bi2O3 component to 10.0% or less, the devitrification resistance of the glass can be improved, and the coloring of the glass can be reduced to improve the visible light transmittance. Therefore, the upper limit of the content of Bi2O3 component is preferably 10.0%, more preferably 5.0%, and further preferably 3.0%.
[0159] Bi2O3 component can use Bi2O3 etc. as a raw material.
[0160] The TeO2 component is an arbitrary component that can increase the refractive index and lower the glass transition temperature when the content thereof is greater than 0%.
[0161] However, when glass raw materials are put into a platinum crucible, or when the part in contact with the molten glass is melted in a melting tank formed of platinum, there is a problem that the TeO2 component may alloy with the platinum. Therefore, the upper limit of the content of the TeO2 component is preferably 10.0%, more preferably 5.0%, further preferably 3.0%, and further more preferably not containing.
[0162] TeO2 component can use TeO2 etc. as a raw material.
[0163] The SnO2 component is an arbitrary component which can reduce oxidation of the molten glass to make the molten glass clear when the content thereof is greater than 0%, and can also prevent the light transmittance of the glass from being deteriorated.
[0164] On the other hand, by setting the content of SnO2 component to 3.0% or less, it is not easy to cause the coloring of glass or the devitrification of glass due to the reduction of molten glass. In addition, since the alloying of SnO2 component with melting equipment (especially precious metals such as Pt) is reduced, the service life of melting equipment can be extended. Therefore, the content of SnO2 component is preferably 3.0% or less, more preferably less than 2.0%, further preferably less than 1.0%, and further preferably not contained.
[0165] The SnO2 component can use SnO2, SnO2, SnF2, SnF4 and the like as raw materials.
[0166] The Sb2O3 component is an arbitrary component that can defoam the molten glass when the content thereof is more than 0%.
[0167] On the other hand, by setting the content of Sb2O3 to 1.0% or less, excessive foaming can be prevented and alloying with melting equipment (especially precious metals such as Pt) can be reduced. Therefore, the content of Sb2O3 is preferably 1.0% or less, more preferably less than 0.5%, further preferably less than 0.3%, and further preferably less than 0.1%.
[0168] The Sb2O3 component can use Sb2O3, Sb2O5, Na2H2Sb2O7·5H2O and the like as a raw material.
[0169] In addition, the component for clarifying and defoaming the glass is not limited to the above-mentioned Sb2O3 component, and a clarifier, defoamer or a combination thereof known in the field of glass manufacturing can be used.
[0170] The component F is an arbitrary component that can increase the Abbe number of glass, lower the glass transition temperature, and improve the devitrification resistance when the content thereof exceeds 0%.
[0171] However, if the content of the F component, that is, the total amount of F as fluoride substituted with a part or all of the oxides of one or more of the above-mentioned metal elements, exceeds 10.0%, the volatilization amount of the F component increases, making it difficult to obtain stable optical constants and thus to obtain homogeneous glass. In addition, the Abbe number increases to a degree that is more than necessary.
[0172] Therefore, the content of the component F is preferably 10.0% or less, more preferably less than 5.0%, further preferably less than 3.0%, further preferably less than 1.0%, and further preferably not contained.
[0173] <About ingredients that should not be contained>
[0174] Next, components that should not be contained in the optical glass of the present invention and components that are not preferably contained are described.
[0175] In the optical glass of the present invention, other components may be added as needed as long as the properties of the glass of the present invention are not impaired. However, GeO2 component improves the dispersion of the glass, so it is preferably substantially not contained.
[0176] In addition, various transition metal components other than Ti, Zr, Nb, W, La, Gd, Y, Yb, and Lu, such as Hf, N, Cr, Mn, Fe, Co, Ni, Cu, Ag, Mo, Ce, and Nd, have the property that when contained alone or in combination, even a small amount will color the glass and absorb light of specific wavelengths in the visible light region. Therefore, it is preferably not substantially contained, especially in optical glasses using wavelengths in the visible light region.
[0177] In addition, lead compounds such as PbO and arsenic compounds such as As2O3 and Th, Cd, Tl, Os, Be, Se have a tendency to be avoided as harmful chemical substances in recent years, and not only the manufacturing process of glass, but also the processing process and the treatment after productization also need measures on environmental countermeasures. Therefore, when paying attention to the impact on the environment, except for the inevitable mixing, it is preferred that these components are not substantially contained. Thus, in optical glass, materials that pollute the environment are not substantially contained. Therefore, even if the measures on special environmental countermeasures are not taken, the optical glass can be manufactured, processed and discarded.
[0178] [Manufacturing method]
[0179] The optical glass of the present invention can be produced, for example, as follows. That is, the above raw materials are uniformly mixed in such a manner that each component is within a prescribed content range, the prepared mixture is put into a platinum crucible, a quartz crucible or an alumina crucible for rough melting, and then put into a gold crucible, a platinum crucible, a platinum alloy crucible or an iridium crucible, and melted at a temperature range of 900 to 1400° C. for 1 to 5 hours, stirred to make it uniform and defoamed, etc., and then cooled to below 1300° C., and then stirred in the final stage to remove the streaks, and then formed using a forming mold, thereby producing it. Here, as a method for obtaining glass formed using a forming mold, a method of pulling out the formed glass from the other end of the forming mold while flowing the molten glass into one end of the forming mold, or a method of casting the molten glass into a mold and then slowly cooling it.
[0180] [physical properties]
[0181] The optical glass of the present invention preferably has a high refractive index and high dispersion.
[0182] In particular, the refractive index (n d The lower limit of the refractive index is preferably 1.90, more preferably 1.95, and further preferably 1.98. The upper limit of the refractive index is preferably 2.20, more preferably 2.15, and further preferably 2.10. In addition, the Abbe number (v) of the optical glass of the present invention is preferably 1.90, more preferably 1.95, and further preferably 1.98. d ) has a lower limit of preferably 15.0, more preferably 18.0, further preferably 20.0, and an upper limit thereof is preferably 30.0, more preferably 28.0, further preferably 27.0.
[0183] By having such a high refractive index, a large amount of light refraction can be obtained even if the optical element is thinned. In addition, by having such a high dispersion, when combined with an optical element with low dispersion (high Abbe number), high imaging characteristics can be achieved.
[0184] Therefore, the optical glass of the present invention is useful in optical design, and in particular, can realize miniaturization of the optical system while achieving high imaging characteristics, thereby expanding the degree of freedom of optical design.
[0185] The optical glass of the present invention preferably has a high visible light transmittance, particularly a high transmittance of light on the short wavelength side of visible light, and has little coloration.
[0186] In particular, when the optical glass of the present invention is expressed in terms of glass transmittance, the wavelength (λ 70 ) is preferably 500 nm, more preferably 490 nm, further preferably 480 nm.
[0187] In the optical glass of the present invention, the upper limit of the shortest wavelength (λ5) showing a spectral transmittance of 5% in a sample having a thickness of 10 mm is preferably 400 nm, more preferably 390 nm.
[0188] Thus, the absorption edge of the glass is positioned near the ultraviolet region, and the transparency of the glass to visible light can be improved. Therefore, the optical glass can be preferably used for optical elements that transmit light, such as lenses.
[0189] The optical glass of the present invention preferably has a high partial dispersion ratio (θg, F). More specifically, the lower limit of the partial dispersion ratio (θg, F) of the optical glass of the present invention is preferably 0.570, more preferably 0.580, further preferably 0.595, further preferably 0.605, and further preferably 0.612.
[0190] In addition, the partial dispersion ratio (θg, F) and the Abbe number (v d ) preferably satisfies the relationship between (-0.00162v d +0.645)≤(θg,F)≤(-0.00162v d +0.680). As a result, since an optical glass having a small partial dispersion ratio (θg, F) can be obtained, the optical glass can contribute to reducing chromatic aberration of an optical element or the like.
[0191] Therefore, the lower limit of the partial dispersion ratio (θg, F) of the optical glass of the present invention is preferably (-0.00162v d +0.645, more preferably (-0.00162v d +0.650).
[0192] On the other hand, the upper limit of the partial dispersion ratio (θg, F) of the optical glass of the present invention is preferably (-0.00162v d +0.675, more preferably (-0.00162v d +0.670).
[0193] In the rectangular coordinate system with the partial dispersion ratio as the vertical axis and the Abbe number as the horizontal axis, the above partial dispersion ratio (θg, F) and the Abbe number (v d ) is represented by a straight line parallel to the normal line. The normal line represents the relationship between the partial dispersion ratio (θg, F) and the Abbe number (v d ) is observed between the partial dispersion ratio (θg, F) and the Abbe number (v d ) is the rectangular coordinate with the horizontal axis, and is represented by a straight line obtained by connecting the two points where the partial dispersion ratio and Abbe number of NSL7 and PBM2 are plotted (see Picture 1). Moreover, the relationship between the partial dispersion ratio and the Abbe number of conventionally known glasses roughly overlaps with the normal line.
[0194] Here, NSL7 and PBM2 are optical glasses manufactured by Ohara Co., Ltd., and the Abbe number (v d ) is 36.3, the partial dispersion ratio (θg, F) is 0.5828, and the Abbe number of NSL7 (v d ) is 60.5, and the partial dispersion ratio (θg, F) is 0.5436.
[0195] [Preforms and optical components]
[0196] The glass molded body can be produced from the produced optical glass by a grinding method, or a molding method such as re-hot pressing molding, precision stamping molding, etc. That is, the glass molded body can be produced by mechanical processing such as grinding and polishing the optical glass, or by re-hot pressing a preform made of optical glass and then grinding it, or by precision stamping a preform produced by grinding or a preform molded by known float molding. It should be noted that the method of producing the glass molded body is not limited to the above method.
[0197] As described above, the glass molded body formed from the optical glass of the present invention is useful for various optical elements and optical designs, and is particularly preferably used for optical elements such as lenses and prisms. By improving the stability of the glass, a large-diameter glass molded body can be formed, so that while the optical element is enlarged, high-definition and high-precision imaging characteristics and projection characteristics can be achieved when using optical instruments such as cameras and projectors.
[0198] Example
[0199] The glass compositions of the embodiments (No. 1 to No. 52) of the present invention and the refractive index (n d ), Abbe number (v d ), transmittance (λ5, λ 70 ) and the values of the partial dispersion ratio (θg, F) are shown in Tables 1 to 10. It should be noted that the following examples are for illustrative purposes only and the present invention is not limited to these examples.
[0200] In the glass of the embodiment, the raw materials of each component are high-purity raw materials used in ordinary optical glass, such as corresponding oxides, hydroxides, carbonates, nitrates, fluorides, hydroxides, metaphosphate compounds, etc., which are selected. After being weighed and evenly mixed, they are put into a platinum crucible and melted in an electric furnace at a temperature range of 1280-1340°C for 2.5 hours. When the glass raw materials are melted, the molten glass raw materials are defoamed by stirring, cooled to 1180-1250°C, stirred again to make it uniform, and then cast into a mold and slowly cooled to make glass.
[0201] The refractive index of the glass of the embodiment (n d ) and the Abbe number (v d ) is expressed as a measured value relative to the d line (587.56 nm) of a helium lamp. In addition, the refractive index of the d line and the refractive index of the F line (486.13 nm) of a hydrogen lamp are used. F ), the refractive index (n) relative to the C line (656.27nm) C ) value, according to the Abbe number (v d )=[(n d -1) / (n F -n C )] to calculate the Abbe number (v d ).
[0202] Measure the refractive index n in C line (wavelength 656.27nm) C , refractive index n in F line (wavelength 486.13nm) F , the refractive index n in the g line (wavelength 435.835nm) g , according to (θg, F) = (n g -n F ) / (n F -n C ) is used to calculate the partial dispersion ratio.
[0203] The transmittance of the glass of the embodiment is measured according to the standard of Japan Optical Glass Industry Association JOGIS02-2003. In addition, in the present invention, the presence or absence of glass coloration and the degree of coloration are determined by measuring the transmittance of the glass. Specifically, according to JIS Z8722, the spectral transmittance of 200 to 800 nm is measured for a parallel polished product with a thickness of 10 ± 0.1 mm, and λ5 (the wavelength at which the transmittance is 5%) and λ 70 (Wavelength when transmittance is 70%).
[0204] In addition, the glass used in this measurement was treated in a slow cooling furnace at a slow temperature drop rate of -25°C / hr.
[0205] Table 1
[0206] wt% 1 2 3 4 5 6 <![CDATA[SiO2]]> 6.01 6.01 6.01 5.43 5.01 5.01 <![CDATA[B2O3]]> 6.95 6.95 6.95 7.60 6.95 6.95 <![CDATA[La2O3]]> 31.99 32.00 33.27 31.72 32.00 33.98 <![CDATA[Y2O3]]> <![CDATA[Gd2O3]]> <![CDATA[Yb2O3]]> <![CDATA[ZrO2]]> 6.39 6.39 6.39 6.37 6.39 4.39 <![CDATA[TiO2]]> 21.70 21.70 21.70 21.89 22.70 21.70 <![CDATA[Nb2O5]]> 7.31 7.31 7.31 8.78 7.31 8.31 <![CDATA[WO3]]> 0.77 0.77 0.77 0.77 0.77 0.77 ZnO 1.27 1.27 1.27 1.27 <![CDATA[Li2O]]> <![CDATA[Na2O]]> <![CDATA[K2O]]> MgO CaO SrO BaO 17.60 17.60 17.60 17.45 17.60 17.60 <![CDATA[Sb2O3]]> 0.01 0.00 0.00 0.00 0.00 0.02 total 100.00 100.00 100.00 100.00 100.00 100.00 Si+B 12.96 12.96 12.96 13.03 11.96 11.96 Ti / (Ti+Ba) 0.55 0.55 0.55 0.56 0.56 0.55 La+Nb+Gd+Yb 39.30 39.31 40.58 40.50 39.31 42.29 Ti / Ba 1.23 1.23 1.23 1.25 1.29 1.23 <![CDATA[Rn2O]]> 0.00 0.00 0.00 0.00 0.00 0.00 RO 17.60 17.60 17.60 17.45 17.60 17.60 Ln 31.99 32.00 33.27 31.72 32.00 33.98 Ti+Nb 29.01 29.01 29.01 30.66 30.01 30.01 (Ti+W) / Ba 1.28 1.28 1.28 1.30 1.33 1.28 La / (Nb+Gd+Yb) 4.38 4.38 4.55 3.62 4.38 4.09 <![CDATA[n d ]]> 2.012 2.012 2.012 2.018 2.025 2.020 <![CDATA[v d ]]> 24.9 24.9 25.0 24.5 24.4 24.7 θg,F 0.6156 0.6155 0.6138 0.6168 0.6167 0.6150 <![CDATA[λ 70 ]]> 447 448 447 459 451 454 <![CDATA[λ5]]> 373 372 372 375 373 374
[0207] Table 2
[0208] wt% 7 8 9 10 11 12 <![CDATA[SiO2]]> 5.01 5.51 5.51 5.51 5.51 5.51 <![CDATA[B2O3]]> 6.95 7.45 7.45 7.45 7.45 7.45 <![CDATA[La2O3]]> 32.48 29.48 30.08 30.08 30.08 29.58 <![CDATA[Y2O3]]> <![CDATA[Gd2O3]]> <![CDATA[Yb2O3]]> <![CDATA[ZrO2]]> 5.89 5.89 5.89 5.89 5.89 5.79 <![CDATA[TiO2]]> 21.70 21.70 21.70 21.70 21.70 21.70 <![CDATA[Nb2O5]]> 8.31 10.31 10.31 10.61 10.61 10.31 <![CDATA[WO3]]> 0.77 0.77 0.77 0.77 0.77 0.77 ZnO 1.27 1.27 0.67 0.67 3.67 1.27 <![CDATA[Li2O]]> <![CDATA[Na2O]]> <![CDATA[K2O]]> MgO CaO SrO BaO 17.60 17.60 17.60 17.30 14.30 17.60 <![CDATA[Sb2O3]]> 0.02 0.02 0.02 0.02 0.02 0.02 total 100.00 100.00 100.00 100.00 100.00 100.00 Si+B 11.96 12.96 12.96 12.96 12.96 12.96 Ti / (Ti+Ba) 0.55 0.55 0.55 0.56 0.60 0.55 La+Nb+Gd+Yb 40.79 39.79 40.39 40.69 40.69 39.89 Ti / Ba 1.23 1.23 1.23 1.25 1.52 1.23 <![CDATA[Rn2O]]> 0.00 0.00 0.00 0.00 0.00 0.00 RO 17.60 17.60 17.60 17.30 14.30 17.60 Ln 32.48 29.48 30.08 30.08 30.08 29.58 Ti+Nb 30.01 32.01 32.01 32.31 32.31 32.01 (Ti+W) / Ba 1.28 1.28 1.28 1.30 1.57 1.28 La / (Nb+Gd+Yb) 3.91 2.86 2.92 2.84 2.84 2.87 <![CDATA[n d ]]> 2.022 2.021 2.021 2.023 2.027 2.020 <![CDATA[v d ]]> 24.6 24.2 24.2 24.1 24.0 24.2 θg,F 0.6157 <![CDATA[λ 70 ]]> 468 459 457.5 463 462 467 <![CDATA[λ5]]> 376 377 377 377.5 378 378
[0209] Table 3
[0210] wt% 13 14 15 <![CDATA[SiO2]]> 5.51 5.51 5.51 <![CDATA[B2O3]]> 7.45 7.45 7.45 <![CDATA[La2O3]]> 31.48 29.48 33.48 <![CDATA[Y2O3]]> <![CDATA[Gd2O3]]> <![CDATA[Yb2O3]]> <![CDATA[ZrO2]]> 5.89 5.89 5.89 <![CDATA[TiO2]]> 21.70 21.70 21.70 <![CDATA[Nb2O5]]> 10.31 10.31 10.31 <![CDATA[WO3]]> 0.77 0.77 0.77 ZnO 1.27 1.27 1.27 <![CDATA[Li2O]]> <![CDATA[Na2O]]> <![CDATA[K2O]]> MgO CaO SrO BaO 15.60 17.60 13.60 <![CDATA[Sb2O3]]> 0.02 0.02 0.02 total 100.00 100.00 100.00 Si+B 12.96 12.96 12.96 Ti / (Ti+Ba) 0.58 0.55 0.61 La+Nb+Gd+Yb 41.79 39.79 43.79 Ti / Ba 1.39 1.23 1.60 <![CDATA[Rn2O]]> 0.00 0.00 0.00 RO 15.60 17.60 13.60 Ln 31.48 29.48 33.48 Ti+Nb 32.01 32.01 32.01 (Ti+W) / Ba 1.44 1.28 1.65 La / (Nb+Gd+Yb) 3.05 2.86 3.25 <![CDATA[n d ]]> 2.026 2.021 2.031 <![CDATA[v d ]]> 24.2 24.2 24.2 θg,F <![CDATA[λ 70 ]]> 467 467 470 <![CDATA[λ5]]> 379 378 380
[0211] Table 4
[0212] wt% 16 17 18 19 20 21 <![CDATA[SiO2]]> 6.01 6.01 6.01 6.01 6.01 6.01 <![CDATA[B2O3]]> 7.70 7.70 7.70 7.70 7.70 7.70 <![CDATA[La2O3]]> 33.03 33.03 33.03 32.53 33.53 33.03 <![CDATA[Y2O3]]> <![CDATA[Gd2O3]]> <![CDATA[Yb2O3]]> <![CDATA[ZrO2]]> 6.39 6.39 6.39 6.89 5.89 6.39 <![CDATA[TiO2]]> 20.90 20.90 20.90 20.90 20.90 20.90 <![CDATA[Nb2O5]]> 6.91 7.31 6.71 6.71 6.71 6.91 <![CDATA[WO3]]> 0.77 0.77 0.77 0.77 0.77 0.77 ZnO 1.27 1.27 1.27 1.27 1.27 1.27 <![CDATA[Li2O]]> <![CDATA[Na2O]]> <![CDATA[K2O]]> MgO CaO SrO BaO 17.00 16.60 17.20 17.20 17.20 17.00 <![CDATA[Sb2O3]]> 0.02 0.02 0.02 0.02 0.02 0.02 total 100.00 100.00 100.00 100.00 100.00 100.00 Si+B 13.71 13.71 13.71 13.71 13.71 13.71 Ti / (Ti+Ba) 0.55 0.56 0.55 0.55 0.55 0.55 La+Nb+Gd+Yb 39.94 40.34 39.74 39.24 40.24 39.94 Ti / Ba 1.23 1.26 1.22 1.22 1.22 1.23 <![CDATA[Rn2O]]> 0.00 0.00 0.00 0.00 0.00 0.00 RO 17.00 16.60 17.20 17.20 17.20 17.00 Ln 33.03 33.03 33.03 32.53 33.53 33.03 Ti+Nb 27.81 28.21 27.61 27.61 27.61 27.81 (Ti+W) / Ba 1.27 1.31 1.26 1.26 1.26 1.27 La / (Nb+Gd+Yb) 4.78 4.52 4.92 4.85 5.00 4.78 <![CDATA[n d ]]> 2.001 2.003 2.000 2.001 1.999 2.001 <![CDATA[v d ]]> 25.4 25.3 25.5 25.4 25.5 25.4 θg,F 0.6141 0.6137 0.6133 0.6132 0.6133 0.6136 <![CDATA[λ 70 ]]> 446 450 458 451 450 449 <![CDATA[λ5]]> 373 374 374 373 373 373
[0213] Table 5
[0214] wt% 22 23 24 25 26 27 <![CDATA[SiO2]]> 6.01 6.01 6.01 6.01 6.01 6.01 <![CDATA[B2O3]]> 7.70 7.70 7.70 7.70 7.70 7.70 <![CDATA[La2O3]]> 33.03 33.03 33.03 33.03 33.03 38.03 <![CDATA[Y2O3]]> <![CDATA[Gd2O3]]> <![CDATA[Yb2O3]]> <![CDATA[ZrO2]]> 6.39 6.39 6.39 6.39 6.39 6.39 <![CDATA[TiO2]]> 20.90 20.90 20.90 20.90 20.90 20.90 <![CDATA[Nb2O5]]> 6.91 6.91 6.91 6.91 6.91 6.91 <![CDATA[WO3]]> 0.77 0.77 0.77 0.77 0.77 0.77 ZnO 6.27 0.77 2.27 4.27 1.27 <![CDATA[Li2O]]> <![CDATA[Na2O]]> <![CDATA[K2O]]> MgO CaO SrO BaO 18.27 12.00 17.50 16.00 14.00 12.00 <![CDATA[Sb2O3]]> 0.02 0.02 0.02 0.02 0.02 0.02 total 100.00 100.00 100.00 100.00 100.00 100.00 Si+B 13.71 13.71 13.71 13.71 13.71 13.71 Ti / (Ti+Ba) 0.53 0.64 0.54 0.57 0.60 0.64 La+Nb+Gd+Yb 39.94 39.94 39.94 39.94 39.94 44.94 Ti / Ba 1.14 1.74 1.19 1.31 1.49 1.74 <![CDATA[Rn2O]]> 0.00 0.00 0.00 0.00 0.00 0.00 RO 18.27 12.00 17.50 16.00 14.00 12.00 Ln 33.03 33.03 33.03 33.03 33.03 38.03 Ti+Nb 27.81 27.81 27.81 27.81 27.81 27.81 (Ti+W) / Ba 1.19 1.81 1.24 1.35 1.55 1.81 La / (Nb+Gd+Yb) 4.78 4.78 4.78 4.78 4.78 5.50 <![CDATA[n d ]]> 1.998 2.009 2.000 2.003 2.006 2.014 <![CDATA[v d ]]> 25.5 25.2 25.5 25.4 25.3 25.4 θg,F 0.6133 0.6153 0.6132 0.6138 0.6136 0.6130 <![CDATA[λ 70 ]]> 462 459 451 459 453 454 <![CDATA[λ5]]> 375 375 373 375 374 375
[0215] Table 6
[0216] wt% 28 29 30 31 32 33 <![CDATA[SiO2]]> 6.01 6.01 6.01 6.01 6.01 6.01 <![CDATA[B2O3]]> 7.70 7.70 7.70 7.70 7.70 7.70 <![CDATA[La2O3]]> 34.03 36.03 34.83 34.83 34.83 34.83 <![CDATA[Y2O3]]> <![CDATA[Gd2O3]]> <![CDATA[Yb2O3]]> <![CDATA[ZrO2]]> 6.39 6.39 6.39 6.39 6.39 6.39 <![CDATA[TiO2]]> 20.90 20.90 20.10 20.10 20.10 20.10 <![CDATA[Nb2O5]]> 6.91 6.91 6.91 5.91 6.91 5.91 <![CDATA[WO3]]> 0.77 0.77 0.77 1.77 0.77 1.77 ZnO 1.27 1.27 1.27 1.27 1.27 1.27 <![CDATA[Li2O]]> <![CDATA[Na2O]]> <![CDATA[K2O]]> MgO CaO SrO BaO 16.00 14.00 16.00 16.00 16.00 16.00 <![CDATA[Sb2O3]]> 0.02 0.02 0.02 0.02 0.02 0.02 total 100.00 100.00 100.00 100.00 100.00 100.00 Si+B 13.71 13.71 13.71 13.71 13.71 13.71 Ti / (Ti+Ba) 0.57 0.60 0.56 0.56 0.56 0.56 La+Nb+Gd+Yb 40.94 42.94 41.74 40.74 41.74 40.74 Ti / Ba 1.31 1.49 1.26 1.26 1.26 1.26 <![CDATA[Rn2O]]> 0.00 0.00 0.00 0.00 0.00 0.00 RO 16.00 14.00 16.00 16.00 16.00 16.00 Ln 34.03 36.03 34.83 34.83 34.83 34.83 Ti+Nb 27.81 27.81 27.01 26.01 27.01 26.01 (Ti+W) / Ba 1.35 1.55 1.30 1.37 1.30 1.37 La / (Nb+Gd+Yb) 4.92 5.21 5.04 5.89 5.04 5.89 <![CDATA[n d ]]> 2.003 2.008 1.999 1.999 1.999 1.999 <![CDATA[v d ]]> 25.4 25.4 25.8 25.8 25.8 25.8 θg,F 0.6137 0.6137 0.6124 0.6124 0.6119 0.6118 <![CDATA[λ 70 ]]> 453 451 442 445 <![CDATA[λ5]]> 374 374 372 372
[0217] Table 7
[0218] wt% 34 35 36 37 38 39 <![CDATA[SiO2]]> 6.01 6.01 6.01 6.01 6.01 6.01 <![CDATA[B2O3]]> 7.70 7.70 7.70 7.70 7.70 7.70 <![CDATA[La2O3]]> 34.84 34.84 34.84 34.14 33.64 34.64 <![CDATA[Y2O3]]> <![CDATA[Gd2O3]]> <![CDATA[Yb2O3]]> <![CDATA[ZrO2]]> 6.39 6.39 6.39 6.39 6.89 5.89 <![CDATA[TiO2]]> 20.10 20.10 20.10 20.80 20.80 20.80 <![CDATA[Nb2O5]]> 6.91 6.91 6.91 6.91 6.91 6.91 <![CDATA[WO3]]> 0.77 0.77 0.77 0.77 0.77 0.77 ZnO 1.27 1.27 1.27 1.27 1.27 1.27 <![CDATA[Li2O]]> <![CDATA[Na2O]]> <![CDATA[K2O]]> MgO CaO SrO BaO 16.00 16.00 16.00 16.00 16.00 16.00 <![CDATA[Sb2O3]]> 0.01 0.01 0.01 0.01 0.01 0.01 total 100.00 100.00 100.00 100.00 100.00 100.00 Si+B 13.71 13.71 13.71 13.71 13.71 13.71 Ti / (Ti+Ba) 0.56 0.56 0.56 0.57 0.57 0.57 La+Nb+Gd+Yb 41.75 41.75 41.75 41.05 40.55 41.55 Ti / Ba 1.26 1.26 1.26 1.30 1.30 1.30 <![CDATA[Rn2O]]> 0.00 0.00 0.00 0.00 0.00 0.00 RO 16.00 16.00 16.00 16.00 16.00 16.00 Ln 34.84 34.84 34.84 34.14 33.64 34.64 Ti+Nb 27.01 27.01 27.01 27.71 27.71 27.71 (Ti+W) / Ba 1.30 1.30 1.30 1.35 1.35 1.35 La / (Nb+Gd+Yb) 5.04 5.04 5.04 4.94 4.87 5.01 <![CDATA[n d ]]> 1.999 1.999 1.999 2.003 2.003 2.002 <![CDATA[v d ]]> 25.8 25.8 25.8 25.5 25.4 25.5 θg,F 0.6116 0.6116 0.6119 0.6139 0.6137 0.6131 <![CDATA[λ 70 ]]> 444.5 454 448.5 <![CDATA[λ5]]> 371.5 373 372
[0219] Table 8
[0220] wt% 40 41 42 43 44 45 <![CDATA[SiO2]]> 6.21 6.01 6.01 6.01 6.01 6.01 <![CDATA[B2O3]]> 7.85 8.02 7.70 8.02 8.02 8.02 <![CDATA[La2O3]]> 33.33 33.82 34.34 33.83 33.83 33.83 <![CDATA[Y2O3]]> <![CDATA[Gd2O3]]> <![CDATA[Yb2O3]]> <![CDATA[ZrO2]]> 6.39 6.39 6.19 6.39 6.39 6.39 <![CDATA[TiO2]]> 20.90 21.10 20.80 21.10 21.10 21.10 <![CDATA[Nb2O5]]> 6.91 6.61 6.91 6.61 6.61 6.61 <![CDATA[WO3]]> 0.77 0.77 0.77 0.77 0.77 0.77 ZnO 1.27 1.27 1.27 1.27 1.27 1.27 <![CDATA[Li2O]]> <![CDATA[Na2O]]> <![CDATA[K2O]]> MgO CaO SrO BaO 16.35 16.00 16.00 16.00 16.00 16.00 <![CDATA[Sb2O3]]> 0.02 0.01 0.01 0.00 0.00 0.00 total 100.00 100.00 100.00 100.00 100.00 100.00 Si+B 14.06 14.03 13.71 14.03 14.03 14.03 Ti / (Ti+Ba) 0.56 0.57 0.57 0.57 0.57 0.57 La+Nb+Gd+Yb 40.24 40.43 41.25 40.44 40.44 40.44 Ti / Ba 1.28 1.32 1.30 1.32 1.32 1.32 <![CDATA[Rn2O]]> 0.00 0.00 0.00 0.00 0.00 0.00 RO 16.35 16.00 16.00 16.00 16.00 16.00 Ln 33.33 33.82 34.34 33.83 33.83 33.83 Ti+Nb 27.81 27.71 27.71 27.71 27.71 27.71 (Ti+W) / Ba 1.33 1.37 1.35 1.37 1.37 1.37 La / (Nb+Gd+Yb) 4.82 5.12 4.97 5.12 5.12 5.12 <![CDATA[n d ]]> 1.999 2.001 2.002 2.000 2.001 2.001 <![CDATA[v d ]]> 25.5 25.4 25.5 25.4 25.4 25.4 θg,F 0.6138 0.6131 0.6128 0.6135 0.6126 0.6132 <![CDATA[λ 70 ]]> 460 447 447 450 452 <![CDATA[λ5]]> 375 372 372 372 373
[0221] Table 9
[0222] wt% 46 47 48 49 50 51 <![CDATA[SiO2]]> 6.21 6.12 6.63 7.87 6.55 8.14 <![CDATA[B2O3]]> 7.85 8.02 10.10 10.02 9.98 10.43 <![CDATA[La2O3]]> 33.41 33.73 41.27 37.39 31.49 36.13 <![CDATA[Y2O3]]> <![CDATA[Gd2O3]]> <![CDATA[Yb2O3]]> <![CDATA[ZrO2]]> 6.39 6.39 6.37 6.68 5.51 6.85 <![CDATA[TiO2]]> 20.83 21.08 16.68 18.48 14.30 16.76 <![CDATA[Nb2O5]]> 6.91 6.61 6.34 5.56 13.88 2.39 <![CDATA[WO3]]> 0.77 0.77 0.82 5.19 2.48 ZnO 1.27 1.27 1.36 1.61 1.34 2.20 <![CDATA[Li2O]]> <![CDATA[Na2O]]> <![CDATA[K2O]]> MgO CaO SrO BaO 16.35 16.00 10.43 12.38 11.75 14.61 <![CDATA[Sb2O3]]> 0.01 0.01 0.01 0.01 0.01 0.01 total 99.99 100.00 100.00 100.00 100.00 100.00 Si+B 14.06 14.14 16.73 17.89 16.53 18.57 Ti / (Ti+Ba) 0.56 0.57 0.62 0.60 0.55 0.53 La+Nb+Gd+Yb 40.32 40.34 47.61 42.96 45.36 38.52 Ti / Ba 1.27 1.32 1.60 1.49 1.22 1.15 <![CDATA[Rn2O]]> 0.00 0.00 0.00 0.00 0.00 0.00 RO 16.35 16.00 10.43 12.38 11.75 14.61 Ln 33.41 33.73 41.27 37.39 31.49 36.13 Ti+Nb 27.74 27.69 23.02 24.04 28.18 19.15 (Ti+W) / Ba 1.32 1.37 1.68 1.49 1.66 1.32 La / (Nb+Gd+Yb) 4.83 5.10 6.51 6.72 2.27 15.10 <![CDATA[n d ]]> 1.999 2.000 1.968 1.961 1.976 1.934 <![CDATA[v d ]]> 25.5 25.5 27.8 27.4 26.1 28.8 θg,F 0.6131 0.6134 0.6053 0.6081 0.6115 0.6040 <![CDATA[λ 70 ]]> 455 444 440 428 436 420 <![CDATA[λ5]]> 375 372 369 369 373 367
[0223] Table 10
[0224] wt% 52 <![CDATA[SiO2]]> 6.21 <![CDATA[B2O3]]> 7.85 <![CDATA[La2O3]]> 33.41 <![CDATA[Y2O3]]> <![CDATA[Gd2O3]]> YbO3 <![CDATA[ZrO2]]> 6.39 <![CDATA[TiO2]]> 20.83 <![CDATA[Nb2O5]]> 6.91 <![CDATA[WO3]]> 0.77 ZnO 1.27 <![CDATA[Li2O]]> 0.10 <![CDATA[Na2O]]> <![CDATA[K2O]]> MgO CaO SrO BaO 16.35 <![CDATA[Sb2O3]]> total 100.08 Si+B 14.06 Ti / (Ti+Ba) 0.56 La+Nb+Gd+Yb 40.32 Ti / Ba 1.27 <![CDATA[Rn2O]]> 0.10 RO 16.35 Ln 33.41 Ti+Nb 27.74 (Ti+W) / Ba 1.32 La / (Nb+Gd+Yb) 4.83 <![CDATA[n d ]]> 1.999 <![CDATA[v d ]]> 25.5 θg,F 0.6130 <![CDATA[λ 70 ]]> 449 <![CDATA[λ5]]> 372
[0225] As shown in the table, the optical glasses of the embodiments of the present invention are all of the following: d ) is greater than 1.90, and the refractive index (n d ) is 2.20 or less, and more specifically, 2.10 or less, both of which are within the desired range.
[0226] In addition, the optical glasses of the embodiments of the present invention are all of Abbe number (v d ) is 30.0 or less, more specifically 28.0 or less, and the Abbe number (v d ) is 15.0 or more, more specifically, 20.0 or more, both of which are within the desired range.
[0227] In addition, the λ of the optical glass of the embodiment of the present invention is 70(wavelength at a transmittance of 70%) was 500 nm or less, more specifically 490 nm or less. In addition, the λ5 (wavelength at a transmittance of 5%) of the optical glasses of the examples of the present invention was 400 nm or less, more specifically 390 nm or less.
[0228] In addition, the partial dispersion ratio (θg, F) of the optical glasses of the embodiments of the present invention is (-0.00162v d +0.645) or more, more specifically (-0.00162v d In contrast, the partial dispersion ratio of the optical glass of the embodiment of the present invention is (-0.00162v d +0.680) or less, more specifically (-0.00162v d +0.670) or less. It can be seen from this that these partial dispersion ratios (θg, F) are within the desired range.
[0229] Therefore, it is clear that the optical glass of the embodiment of the present invention has a refractive index and an Abbe number within a desired range, is easy to manufacture, and is less colored.
[0230] In addition, the optical glass obtained in the embodiment of the present invention is subjected to re-hot pressing and then ground and polished to be processed into lens and prism shapes. In addition, the optical glass of the embodiment of the present invention is used to form a preform for precision stamping, and the preform for precision stamping is precision stamped. In either case, the glass after heating and softening does not have problems such as milky whitening and devitrification, so that it can be stably processed into various lens and prism shapes.
[0231] The present invention has been described in detail above for the purpose of illustration. However, this embodiment is only for the purpose of illustration, and those skilled in the art should understand that various changes can be made without departing from the concept and scope of the present invention.
Claims
1. An optical glass, characterized in that: In terms of mass % based on oxides, Greater than 0% to 45.0% La2O3 content, TiO2 content greater than 0% to 45.0%, BaO content greater than 0% to 40.0%, and 0~6.01% SiO2 content, The total amount of SiO2 and B2O3 is 5.0% or more and 30.0% or less. The mass sum of RO components is greater than 0% and less than 14.30%, wherein R is one or more selected from the group consisting of Mg, Ca, Sr, and Ba, The mass ratio of TiO2 / (TiO2+BaO) is 0.60 or more and 0.90 or less, The mass ratio of TiO2 / (La2O3+Nb2O5+Gd2O3+Yb2O3) is above 0.52, Refractive index (n d ) is above 1.90, and the Abbe number (v d ) is 30.0 or less, and the wavelength (λ5) showing a spectral transmittance of 5% is 400 nm or less.
2. The optical glass according to claim 1, characterized in that: Measured in mass % based on oxides, The B2O3 content is 0 to 30.0%.
3. The optical glass according to claim 1 or 2, characterized in that: Measured in mass % based on oxides, The ZnO content is 0 to 20.0%, Y2O3 content is 0~15.0%, Nb2O5 content is 0~25.0%, The Yb2O3 content is 0 to 15.0%, and The Gd2O3 component is 0 to 15.0%.
4. The optical glass according to claim 1 or 2, characterized in that: Measured in mass % based on oxides, The mass sum of (La2O3+Nb2O5+Gd2O3+Yb2O3) is greater than 0% and less than 60.0%.
5. The optical glass according to claim 1 or 2, characterized in that: Measured in mass % based on oxides, The total amount of Ln2O3 components is greater than 0% and less than 50.0%, Here, Ln is one or more selected from the group consisting of La, Gd, Y, and Yb.
6. The optical glass according to claim 1 or 2, characterized in that: Calculated on an oxide basis, TiO2 / BaO is greater than 0 and less than 3.
00.
7. The optical glass according to claim 1 or 2, characterized in that: Measured in mass % based on oxides, The mass sum of Rn2O components is less than 15.0%, Here, Rn is one or more selected from the group consisting of Li, Na, and K.
8. The optical glass according to claim 1 or 2, characterized in that: The content of ZrO2 is 0-20.0% based on the mass % of the oxide. WO3 component 0~10.0%, Ta2O5 composition 0~10.0%, MgO component 0~15.0%, CaO content 0~15.0%, SrO component 0~15.0%, Li2O composition 0~15.0%, Na2O component 0~15.0%, K2O component 0~15.0%, P2O5 composition 0~10.0%, GeO2 composition 0~10.0%, Al2O3 composition 0~15.0%, Ga2O3 content 0~15.0%, Bi2O3 composition 0~10.0%, TeO2 composition 0~10.0%, SnO2 content 0-3.0%, and Sb2O3 content: 0~1.0%.
9. A preform, characterized in that: The optical glass comprising any one of claims 1 to 8.
10. An optical element, characterized in that: The optical glass comprising any one of claims 1 to 8.
11. An optical instrument, characterized in that: A method of manufacturing the optical device according to claim 10.