Multifunctional practical membrane cloth
By adding chitosan fiber, seaweed fiber and composite fiber to the facial mask cloth, the problem of single function of the facial mask cloth is solved, multifunctionality and sustainability are achieved, the fragrance release time is extended, and resource waste and environmental pollution are reduced.
Patent Information
- Application Number
- CN202310191413.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-02
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-03-02
AI Technical Summary
The existing facial mask cloth has a single function, causing environmental pollution and resource waste after use, and lacks versatility and sustainability.
It adopts multi-functional and practical membrane cloth, containing chitosan fiber, seaweed fiber and composite fiber. The composite fiber is composed of polylactic acid, polyglutamic acid, hemp straw core ultra-fine powder and aromatic microcapsules, which has significant water absorption and antibacterial properties. , slow-release aroma and biodegradable properties, suitable for facial masks, aromatherapy, wipes and potting fertilizers.
It realizes the multifunctionality of the mask cloth, prolongs the fragrance release time, promotes plant growth, reduces resource waste and environmental pollution, and conforms to the concept of green environmental protection.
Smart Images

Figure BDA0004105608420000141
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of facial masks, and more specifically, to a multifunctional and practical facial mask cloth. Background Art
[0002] With the rapid development of economy and technology, people's lives are getting better and better, and people's concepts are gradually changing. They pay more and more attention to skin care and use various cosmetics to improve their facial skin. Facial masks contain a variety of effective ingredients to improve skin condition. Therefore, facial masks have become an indispensable skin care product in people's daily lives, and the per capita consumption of facial masks is increasing year by year. At present, the main consumer of facial masks is still patch masks, and the consumption of mask cloth used for patch masks is also increasing year by year.
[0003] At present, in addition to its good ability to absorb mask liquid, facial mask cloth does not have many other practical functions. After using the mask, people basically discard it directly, which not only pollutes the environment, but also wastes resources. Therefore, it is urgent to propose a multifunctional practical mask cloth to solve the problem of the single function of the existing mask cloth, so that the mask cloth has multiple practical functions. In addition to exerting its excellent liquid absorption ability, it can also be reused as a product, actively responding to the call of green environmental protection and sustainable development concepts, and has broad market prospects. Summary of the invention
[0004] In order to solve the problem of single function of existing facial mask cloths, the present application provides a multifunctional practical mask cloth.
[0005] This application provides a multifunctional practical membrane cloth, which adopts the following technical solutions:
[0006] The multifunctional and practical membrane cloth comprises the following raw materials in parts by weight: 15-26 parts of chitosan fiber, 8-12 parts of seaweed fiber, and 30-40 parts of composite fiber;
[0007] The composite fiber comprises the following raw materials in parts by weight: 10-20 parts of polylactic acid, 5-7 parts of polyglutamic acid, 20-30 parts of ethyl acetate, 6-8 parts of superfine hemp stalk core powder, 8-10 parts of aromatic microcapsules, and 1-3 parts of sophorolipids.
[0008] By adopting the above-mentioned technical scheme, the chitosan fiber in the multifunctional practical membrane cloth of the present application has significant antibacterial function, good biodegradability, and excellent water absorption performance; due to the advantages of its own molecular structure, the seaweed fiber has the characteristics of antibacterial, moisture absorption, breathability, skin-friendly, flame retardant, radiation protection, and biodegradability; the addition of chitosan fiber and seaweed fiber makes the multifunctional practical membrane cloth have significant water absorption, antibacterial and biodegradable properties.
[0009] In addition, composite fibers are added to the multifunctional practical membrane cloth of the present application. The composite fibers are made of biodegradable materials such as polylactic acid and polyglutamic acid as main raw materials. Both are hydrophilic biodegradable materials and contain active groups in their structures. The synergistic effect of the two can effectively improve the water absorption performance of the composite fibers; and sustained-release aromatic microcapsules are added to enable the multifunctional practical membrane cloth to release aroma for a long time; at the same time, ultrafine hemp stalk core powder is added. The ultrafine hemp stalk core powder has a microporous structure, significant moisture absorption and breathability, antibacterial and adsorption properties, and can promote the slow release of aroma molecules in the aromatic microcapsules, so that the multifunctional practical membrane cloth has good biodegradability and moisture absorption properties, and can release aroma slowly.
[0010] The membrane cloth of the present application has excellent comprehensive performance and can be used as a facial mask cloth. After use, it can be made into aromatherapy, rags, and fertilizer for potted plants. The membrane cloth of the present application can play a variety of practical functions and has positive significance for green environmental protection and sustainable development.
[0011] Preferably, the composite fiber is prepared by the following method:
[0012] Polylactic acid and polyglutamic acid are dissolved in ethyl acetate at 50-60°C and a rotation speed of 1100-1500r / min for 0.5-1h, and then hemp stalk core ultrafine powder, aromatic microcapsules and sophorolipids are added and ultrasonically dispersed for 10-20min to form a spinning solution; the spinning solution is wet-spun to obtain composite fibers.
[0013] By adopting the above-mentioned technical scheme, the present application dissolves polylactic acid and polyglutamic acid in ethyl acetate, and then adds hemp stalk core ultrafine powder and aromatic microcapsules, which are evenly dispersed under the action of sophora biosurfactant; and the present application controls various process parameters to make the hygroscopic properties and sustained-release properties of the composite fiber more excellent, thereby making the comprehensive performance of the membrane cloth of the present application better and having broad market prospects.
[0014] Preferably, the aromatic microcapsules are prepared by the following method:
[0015] S1. Add essence and PEG-60 hydrogenated castor oil into water, stir for 10-60 min at a temperature of 40-60° C. and a rotation speed of 600-800 r / min to mix evenly, and obtain a capsule core emulsion;
[0016] S2, treating the capsule core emulsion obtained in step S1 with the first capsule wall solution by ultrasonic treatment at 50-70° C. for 30-40 min, and uniformly mixing them to form a microcapsule solution; and then spray drying to obtain a primary product;
[0017] S3, subjecting the primary product obtained in step S2 to adsorption treatment with the second capsule wall solution at room temperature for 10-30 minutes; and then freeze-drying to obtain aromatic microcapsules.
[0018] Preferably, the mass ratio of the essence, PEG-60 hydrogenated castor oil and water is 8-12:1-2:20; the mass ratio of the capsule core emulsion to the first capsule wall solution is 1:1.2-1.6; and the mass ratio of the primary product to the second capsule wall solution is 1:1.1-1.5.
[0019] Preferably, the essence is one of sweet orange essential oil, osmanthus essential oil, jasmine essential oil and lavender essential oil.
[0020] By adopting the above technical scheme, the aromatic microcapsule of the present application uses essence as the capsule core, forms two layers of capsule wall on the surface of the capsule core, and controls various process parameters, so that the aromatic microcapsule has a regular structure, uniform size, and good aroma sustained release function.
[0021] Preferably, the first capsule wall solution is prepared by the following method:
[0022] Firstly, the modified chitosan is dissolved in a succinic acid solution with a concentration of 5-20wt% to obtain a modified chitosan solution; then the modified chitosan solution is fully mixed with tea tree oil, and homogenized and emulsified at a speed of 20000-25000rpm for 30-60s to obtain a first capsule wall solution.
[0023] Preferably, the mass ratio of the modified chitosan, succinic acid solution and tea tree oil is 20:40-60:5-7.
[0024] By adopting the above-mentioned technical scheme, the present application uses modified chitosan, succinic acid and tea tree oil as raw materials to form a first capsule wall solution. The modified chitosan is protonated under the acidic action of succinic acid, and under the action of tea tree oil, a porous modified chitosan solution is formed. The first capsule wall solution is used as the aqueous phase to coat the oil phase capsule core, and a hydrophilic microporous film is formed on the surface of the flavor, which is beneficial to the sustained release of the aroma.
[0025] Preferably, the modified chitosan is prepared by the following method:
[0026] S11, dissolving chitosan in a citric acid solution with a concentration of 3-5wt%, fully dissolving to obtain a chitosan citric acid aqueous solution; dissolving octadecyl alcohol in ethanol at 50-60°C, mixing evenly, obtaining an octadecyl alcohol ethanol solution;
[0027] S12, first uniformly mix the chitosan citric acid aqueous solution obtained in step S11 and the octadecyl alcohol ethanol solution to form a mixed solution; then add concentrated sulfuric acid with a concentration of 98wt% to the obtained mixed solution, mix evenly, and stir at 100-120°C and a speed of 600-800r / min to react for 8-10h; then adjust the pH to 8-11, let stand for 10-30min, filter, wash, and dry to obtain modified chitosan.
[0028] Preferably, the modified chitosan comprises the following raw materials in parts by weight: 11-15 parts of chitosan, 30-50 parts of citric acid solution, 5-9 parts of octadecyl alcohol, 10-30 parts of ethanol, and 6-12 parts of concentrated sulfuric acid.
[0029] By adopting the above technical scheme, the modified chitosan of the present application is mainly modified by octadecyl alcohol, and the modified chitosan has hydrophilicity and lipophilicity, so that the modified chitosan has good adsorption performance and can fully adsorb flavor molecules, thereby allowing the flavor to be completely coated in the first layer of capsule wall to form a primary product with stable structure.
[0030] Preferably, the second capsule wall solution is prepared by the following method:
[0031] According to weight, 1-3 parts of porous starch and 10-14 parts of carboxymethyl-β-cyclodextrin are added to 20-30 parts of water, and stirred at 50-60° C. and 600-800 r / min for 10-30 min to obtain a second capsule wall solution.
[0032] By adopting the above-mentioned technical scheme, the second capsule wall solution of the present application includes porous starch and carboxymethyl-β-cyclodextrin, which are combined in the form of hydrogen bonds to form a network macromolecular structure on the surface of the primary product, forming the second capsule wall of the aromatic microcapsule. The second capsule wall has strong hygroscopic properties and will form a loose and porous structure after absorbing moisture, which is beneficial to the internal first capsule wall to absorb water and expand. The microporous structure of the modified chitosan will become larger, thereby allowing the capsule core essence to be slowly released, thereby achieving the purpose of sustained-release aroma of the aromatic microcapsule.
[0033] Preferably, the multifunctional practical membrane cloth is prepared by the following method:
[0034] Chitosan fiber, seaweed fiber and composite fiber are combed, laid into a net and reinforced with hydroentanglement to produce a multifunctional and practical membrane cloth.
[0035] By adopting the above technical scheme, the preparation method of the multifunctional practical membrane cloth of the present application has simple steps, low preparation cost, and is suitable for industrial production, so that the multifunctional practical membrane cloth has broad application prospects.
[0036] In summary, this application has the following beneficial effects:
[0037] 1. The multifunctional and practical membrane cloth of the present application is composed of chitosan fiber, seaweed fiber, and composite fiber; and the raw materials of the composite fiber include polylactic acid, polyglutamic acid, hemp stalk core ultrafine powder, aromatic microcapsules, and sophora biosurfactant; the membrane cloth of the present application has excellent water absorption performance and can release aroma slowly, and has broad application prospects.
[0038] 2. The aromatic microcapsules of the present application have a double-layer structure, with essence as the capsule core, the first layer of the capsule wall being porous modified chitosan, and the second layer of the capsule wall being a complex of porous starch and carboxymethyl-β-cyclodextrin. The aromatic microcapsules of the present application have good hygroscopic properties, and can thus achieve the function of sustained release of aroma.
[0039] 3. The multifunctional and practical membrane cloth of the present application is a good choice of mask cloth material, with good liquid absorption capacity, and the addition of aromatic microcapsules has the function of slow-release fragrance; after being used as a mask cloth, it can be washed with clean water, dried, and made into aromatherapy, spraying a small amount of water, and it can release fragrance for a long time until the essence evaporates; the water absorption function of the membrane cloth can be used to make it into a rag; the degradable properties of the membrane cloth can also be used to lay the membrane cloth at the bottom of the potted plant to supply nutrients for the plant. The membrane cloth of the present application has multiple practical functions, and the method of use is simple, which can effectively solve the problem of direct disposal of the mask cloth after use, causing environmental pollution and waste of resources. DETAILED DESCRIPTION
[0040] The present application is further described in detail below with reference to the embodiments.
[0041] Preparation Examples 1-5 provide modified chitosan and preparation methods thereof.
[0042] Preparation Example 1
[0043] The modified chitosan comprises the following raw materials: 11 g chitosan, 30 g citric acid solution, 5 g octadecyl alcohol, 10 g ethanol and 6 g concentrated sulfuric acid.
[0044] Modified chitosan is prepared by the following method:
[0045] S11, dissolving chitosan in a 3wt% citric acid solution, fully dissolving to obtain a chitosan citric acid aqueous solution; dissolving octadecyl alcohol in 50°C ethanol, mixing evenly to obtain an octadecyl alcohol ethanol solution;
[0046] S12, first uniformly mix the chitosan citric acid aqueous solution and the octadecyl alcohol ethanol solution obtained in step S11 to form a mixed solution; then add concentrated sulfuric acid with a concentration of 98wt% to the obtained mixed solution, mix evenly, and stir at 100°C and a speed of 600r / min for 10h; then adjust the pH to 8, let it stand for 10min, filter, wash, and dry to obtain modified chitosan.
[0047] Preparation Example 2
[0048] The modified chitosan comprises the following raw materials: 14 g chitosan, 35 g citric acid solution, 6 g octadecyl alcohol, 15 g ethanol and 7 g concentrated sulfuric acid.
[0049] Modified chitosan is prepared by the following method:
[0050] S11, dissolving chitosan in a 3.5wt% citric acid solution, fully dissolving to obtain a chitosan citric acid aqueous solution; dissolving octadecyl alcohol in 52°C ethanol, mixing evenly to obtain an octadecyl alcohol ethanol solution;
[0051] S12, first uniformly mix the chitosan citric acid aqueous solution and the octadecyl alcohol ethanol solution obtained in step S11 to form a mixed solution; then add concentrated sulfuric acid with a concentration of 98wt% to the obtained mixed solution, mix evenly, and stir at 105°C at a speed of 650r / min for 9.5h; then adjust the pH to 8.5, let stand for 15min, filter, wash, and dry to obtain modified chitosan.
[0052] Preparation Example 3
[0053] The modified chitosan comprises the following raw materials: 13 g chitosan, 40 g citric acid solution, 7 g octadecyl alcohol, 20 g ethanol and 8 g concentrated sulfuric acid.
[0054] Modified chitosan is prepared by the following method:
[0055] S11, dissolving chitosan in a 4 wt % citric acid solution, fully dissolving to obtain a chitosan citric acid aqueous solution; dissolving octadecyl alcohol in 55° C. ethanol, mixing evenly to obtain an octadecyl alcohol ethanol solution;
[0056] S12, first uniformly mix the chitosan citric acid aqueous solution and the octadecyl alcohol ethanol solution obtained in step S11 to form a mixed solution; then add concentrated sulfuric acid with a concentration of 98wt% to the obtained mixed solution, mix evenly, and stir at 110°C and a speed of 700r / min for 9h; then adjust the pH to 9, let it stand for 20min, filter, wash, and dry to obtain modified chitosan.
[0057] Preparation Example 4
[0058] The modified chitosan comprises the following raw materials: 14 g chitosan, 45 g citric acid solution, 8 g octadecyl alcohol, 25 g ethanol and 11 g concentrated sulfuric acid.
[0059] Modified chitosan is prepared by the following method:
[0060] S11, dissolving chitosan in a 4.5wt% citric acid solution, fully dissolving to obtain a chitosan citric acid aqueous solution; dissolving octadecyl alcohol in 58°C ethanol, mixing evenly to obtain an octadecyl alcohol ethanol solution;
[0061] S12, first uniformly mix the chitosan citric acid aqueous solution and the octadecyl alcohol ethanol solution obtained in step S11 to form a mixed solution; then add concentrated sulfuric acid with a concentration of 98wt% to the obtained mixed solution, mix evenly, and stir at 115°C and a speed of 750r / min for 8.5h; then adjust the pH to 10, let it stand for 25min, filter, wash, and dry to obtain modified chitosan.
[0062] Preparation Example 5
[0063] The modified chitosan comprises the following raw materials: 15 g chitosan, 50 g citric acid solution, 9 g octadecyl alcohol, 30 g ethanol and 12 g concentrated sulfuric acid.
[0064] Modified chitosan is prepared by the following method:
[0065] S11, dissolving chitosan in a 5wt% citric acid solution, fully dissolving to obtain a chitosan citric acid aqueous solution; dissolving octadecyl alcohol in 60°C ethanol, mixing evenly to obtain an octadecyl alcohol ethanol solution;
[0066] S12, first uniformly mix the chitosan citric acid aqueous solution and the octadecyl alcohol ethanol solution obtained in step S11 to form a mixed solution; then add concentrated sulfuric acid with a concentration of 98wt% to the obtained mixed solution, mix evenly, and stir at 120°C and a speed of 800r / min for 8h; then adjust the pH to 11, let it stand for 30min, filter, wash, and dry to obtain modified chitosan.
[0067] Preparation Examples 6-10 and Comparative Preparation Examples 1 and 2 provide methods for preparing the first capsule wall solution.
[0068] Preparation Example 6
[0069] The first capsule wall solution is prepared by the following method:
[0070] First, 20 g of modified chitosan was dissolved in 40 g of succinic acid solution with a concentration of 20 wt % to obtain a modified chitosan solution; then, the modified chitosan solution was fully mixed with 5 g of tea tree oil, and homogenized and emulsified at a speed of 20000 rpm for 60 seconds to obtain a first capsule wall solution;
[0071] Wherein, the modified chitosan is prepared by Preparation Example 1.
[0072] Preparation Example 7
[0073] The first capsule wall solution is prepared by the following method:
[0074] First, 20 g of modified chitosan was dissolved in 45 g of 16 wt% succinic acid solution to obtain a modified chitosan solution; then the modified chitosan solution was fully mixed with 5.5 g of tea tree oil, and homogenized and emulsified at a speed of 21500 rpm for 55 seconds to obtain a first capsule wall solution; wherein the modified chitosan was prepared by Preparation Example 2.
[0075] Preparation Example 8
[0076] The first capsule wall solution is prepared by the following method:
[0077] First, 20 g of modified chitosan was dissolved in 50 g of 12 wt% succinic acid solution to obtain a modified chitosan solution; then, the modified chitosan solution was fully mixed with 6 g of tea tree oil, and homogenized and emulsified at a speed of 23000 rpm for 50 seconds to obtain a first capsule wall solution;
[0078] Among them, the modified chitosan is prepared by Preparation Example 3.
[0079] Preparation Example 9
[0080] The first capsule wall solution is prepared by the following method:
[0081] First, 20 g of modified chitosan was dissolved in 55 g of 8 wt % succinic acid solution to obtain a modified chitosan solution; then the modified chitosan solution was fully mixed with 6.5 g of tea tree oil, and homogenized and emulsified at a speed of 24,000 rpm for 40 seconds to obtain a first capsule wall solution; wherein the modified chitosan was prepared by Preparation Example 4.
[0082] Preparation Example 10
[0083] The first capsule wall solution is prepared by the following method:
[0084] First, 20 g of modified chitosan was dissolved in 60 g of 5 wt% succinic acid solution to obtain a modified chitosan solution; then the modified chitosan solution was fully mixed with 7 g of tea tree oil, and homogenized and emulsified at a speed of 25,000 rpm for 30 seconds to obtain a first capsule wall solution; wherein the modified chitosan was prepared by Preparation Example 5.
[0085] Comparative Preparation Example 1
[0086] Comparative Preparation Example 1 is the same as Preparation Example 6, except that the modified chitosan is replaced by chitosan.
[0087] Comparative Preparation Example 2
[0088] Comparative Preparation Example 2 is the same as Preparation Example 6, except that the tea tree oil is replaced by soybean oil.
[0089] Preparation Examples 11-15 and Comparative Preparation Examples 3 and 4 provide methods for preparing the second capsule wall solution.
[0090] Preparation Example 11
[0091] The second capsule wall solution is prepared by the following method:
[0092] 1 g of porous starch and 10 g of carboxymethyl-β-cyclodextrin were added to 20 g of water, and the mixture was stirred at 50° C. and 600 r / min for 30 min to obtain a second capsule wall solution.
[0093] Preparation Example 12
[0094] The second capsule wall solution is prepared by the following method:
[0095] 1.5 g of porous starch and 11 g of carboxymethyl-β-cyclodextrin were added into 22 g of water, and stirred at 52° C. and 650 r / min for 25 min to obtain a second capsule wall solution.
[0096] Preparation Example 13
[0097] The second capsule wall solution is prepared by the following method:
[0098] 2 g of porous starch and 12 g of carboxymethyl-β-cyclodextrin were added to 25 g of water, and the mixture was stirred at 55° C. and 700 r / min for 20 min to obtain a second capsule wall solution.
[0099] Preparation Example 14
[0100] The second capsule wall solution is prepared by the following method:
[0101] 2.5 g of porous starch and 13 g of carboxymethyl-β-cyclodextrin were added into 28 g of water, and stirred at 58° C. and 750 r / min for 10-30 min to obtain a second capsule wall solution.
[0102] Preparation Example 15
[0103] The second capsule wall solution is prepared by the following method:
[0104] 3 g of porous starch and 14 g of carboxymethyl-β-cyclodextrin were added into 30 g of water, and stirred at 800 r / min at 60° C. for 10 min to obtain a second capsule wall solution.
[0105] Comparative Preparation Example 3
[0106] Comparative Preparation Example 3 is the same as Preparation Example 11, except that the porous starch is replaced by carboxymethyl-β-cyclodextrin.
[0107] Comparative Preparation Example 4
[0108] Comparative Preparation Example 4 is the same as Preparation Example 11, except that carboxymethyl-β-cyclodextrin is replaced by porous starch.
[0109] Preparation Examples 16-23 and Comparative Preparation Examples 5-8 provide methods for preparing aromatic microcapsules.
[0110] Preparation Example 16
[0111] Aroma microcapsules are prepared by the following method:
[0112] S1, add 8g of essence and 1g of PEG-60 hydrogenated castor oil to 20g of water, stir for 60min at a temperature of 40°C and a rotation speed of 600r / min to mix evenly, and obtain a capsule core emulsion;
[0113] S2, taking 20g of the capsule core emulsion obtained in step S1 and 24g of the first capsule wall solution, ultrasonically treating at 50°C for 40min, and uniformly mixing to form a microcapsule solution; then, at an inlet air temperature of 110°C and an inlet air volume of 26m 3 / min, feed at a uniform rate of 200mL / h, spray drying is performed to obtain the initial product;
[0114] S3, taking 20g of the initial product obtained in step S2 and 22g of the second capsule wall solution, and performing adsorption treatment at room temperature for 10min; then cooling to -20°C at a cooling rate of 2°C / min and freeze-drying for 3h to obtain aromatic microcapsules;
[0115] Wherein, the essence is jasmine essential oil; the first capsule wall solution is prepared by Preparation Example 6; and the second capsule wall solution is prepared by Preparation Example 11.
[0116] Preparation Example 17
[0117] Aroma microcapsules are prepared by the following method:
[0118] S1. Add 9 g of essence and 1.5 g of PEG-60 hydrogenated castor oil to 20 g of water, stir for 50 min at a temperature of 45° C. and a rotation speed of 650 r / min to mix evenly, to obtain a capsule core emulsion;
[0119] S2, taking 20g of the capsule core emulsion obtained in step S1 and 26g of the first capsule wall solution, ultrasonically treating at 55°C for 38min, and uniformly mixing to form a microcapsule solution; then, at an inlet air temperature of 120°C and an inlet air volume of 27m 3 / min, feed at a uniform rate of 300mL / h, spray drying is performed to obtain the initial product;
[0120] S3, taking 20g of the initial product obtained in step S2 and 22g of the second capsule wall solution for adsorption treatment, adsorbing for 15min at room temperature; then cooling to -25°C at a cooling rate of 3°C / min and freeze-drying for 2.8h to obtain aromatic microcapsules;
[0121] Among them, the essence is jasmine essential oil; the first capsule wall solution is prepared by Preparation Example 7; and the second capsule wall solution is prepared by Preparation Example 12.
[0122] Preparation Example 18
[0123] Aroma microcapsules are prepared by the following method:
[0124] S1. Add 10 g of essence and 2 g of PEG-60 hydrogenated castor oil to 20 g of water, stir for 35 min at a temperature of 50° C. and a rotation speed of 700 r / min to mix evenly, to obtain a capsule core emulsion;
[0125] S2, taking 20g of the capsule core emulsion obtained in step S1 and 28g of the first capsule wall solution, ultrasonically treating at 55°C for 35min, and uniformly mixing to form a microcapsule solution; then, heating at an inlet air temperature of 130°C and an inlet air volume of 28m 3 / min, feed at a uniform rate of 400mL / h, spray drying is performed to obtain the initial product;
[0126] S3, taking 20g of the initial product obtained in step S2 and 26g of the second capsule wall solution for adsorption treatment, adsorbing for 20min at room temperature; then cooling to -30°C at a cooling rate of 4°C / min and freeze-drying for 2.5h to obtain aromatic microcapsules;
[0127] Among them, the essence is jasmine essential oil; the first capsule wall solution is prepared by Preparation Example 8; and the second capsule wall solution is prepared by Preparation Example 13.
[0128] Preparation Example 19
[0129] Aroma microcapsules are prepared by the following method:
[0130] S1. Add 11 g of essence and 1.8 g of PEG-60 hydrogenated castor oil into water, stir for 20 min at a temperature of 55° C. and a rotation speed of 750 r / min to mix evenly, and obtain a capsule core emulsion;
[0131] S2, taking 20g of the capsule core emulsion obtained in step S1 and 30g of the first capsule wall solution, ultrasonically treating at 65°C for 32min, and uniformly mixing to form a microcapsule solution; then, heating at an inlet air temperature of 140°C and an inlet air volume of 29m 3 / min, feed at a uniform rate of 500mL / h, spray drying is performed to obtain the initial product;
[0132] S3, taking 20g of the initial product obtained in step S2 and 28g of the second capsule wall solution for adsorption treatment, adsorbing at room temperature for 25min; then cooling to -35°C at a cooling rate of 5°C / min and freeze-drying for 2.2h to obtain aromatic microcapsules;
[0133] Among them, the essence is jasmine essential oil; the first capsule wall solution is prepared by Preparation Example 9; and the second capsule wall solution is prepared by Preparation Example 14.
[0134] Preparation Example 20
[0135] Aroma microcapsules are prepared by the following method:
[0136] S1. Add 12 g of essence and 2 g of PEG-60 hydrogenated castor oil into water, stir for 10 min at 60° C. and 800 r / min to obtain a capsule core emulsion;
[0137] S2, taking 20g of the capsule core emulsion obtained in step S1 and 32g of the first capsule wall solution, ultrasonically treating at 70°C for 30min, and uniformly mixing to form a microcapsule solution; then, at an inlet air temperature of 150°C and an inlet air volume of 30m 3 / min, feed at a uniform rate of 600mL / h, spray drying is performed to obtain the initial product;
[0138] S3, taking 20g of the initial product obtained in step S2 and 30g of the second capsule wall solution for adsorption treatment, adsorbing for 30min at room temperature; then cooling to -40°C at a cooling rate of 6°C / min and freeze-drying for 2h to obtain aromatic microcapsules;
[0139] Among them, the essence is jasmine essential oil; the first capsule wall solution is prepared by Preparation Example 10; and the second capsule wall solution is prepared by Preparation Example 15.
[0140] Preparation Example 21
[0141] Preparation Example 21 is the same as Preparation Example 16, except that the essence is sweet orange essential oil.
[0142] Preparation Example 22
[0143] Preparation Example 22 is the same as Preparation Example 16, except that the essence is osmanthus essential oil.
[0144] Preparation Example 23
[0145] Preparation Example 23 is the same as Preparation Example 16, except that the essence is lavender essential oil.
[0146] Comparative Preparation Example 5
[0147] Comparative Preparation Example 5 is the same as Preparation Example 16, except that the first capsule wall solution is prepared by Comparative Preparation Example 1.
[0148] Comparative Preparation Example 6
[0149] Comparative Preparation Example 6 is the same as Preparation Example 16, except that the first capsule wall solution is prepared by Comparative Preparation Example 2.
[0150] Comparative Preparation Example 7
[0151] Comparative Preparation Example 7 is the same as Preparation Example 16, except that the second capsule wall solution is prepared by Comparative Preparation Example 3.
[0152] Comparative Preparation Example 8
[0153] Comparative Preparation Example 8 is the same as Preparation Example 16, except that the second capsule wall solution is prepared by Comparative Preparation Example 4.
[0154] Preparation Examples 24-31 and Comparative Preparation Examples 9-17 are composite fibers and preparation methods thereof.
[0155] Preparation Example 24
[0156] Composite fiber, including the following raw materials: 10g polylactic acid, 5g polyglutamic acid, 20g ethyl acetate, 6g hemp stalk core ultrafine powder, 8g aromatic microcapsule, 1g sophorolipid;
[0157] The aromatic microcapsules were prepared by Preparation Example 16;
[0158] Composite fiber, prepared by the following method:
[0159] Polylactic acid and polyglutamic acid were dissolved in ethyl acetate at 50°C and a rotation speed of 1100 / min. After dissolving for 1 hour, hemp stalk core ultrafine powder, aromatic microcapsules and sophorolipids were added and ultrasonically dispersed for 10 minutes to form a spinning solution. The spinning solution was wet-spun to obtain composite fibers.
[0160] Preparation Example 25
[0161] Composite fiber, including the following raw materials: 12g polylactic acid, 5.5g polyglutamic acid, 22g ethyl acetate, 6.5g hemp stalk core ultrafine powder, 8.5g aromatic microcapsule, 1.5g sophorolipid;
[0162] The aromatic microcapsules were prepared by Preparation Example 17;
[0163] Composite fiber, prepared by the following method:
[0164] Polylactic acid and polyglutamic acid were dissolved in ethyl acetate at 52°C and a rotation speed of 1200 r / min for 0.9 h, and then ultrafine hemp stalk core powder, aromatic microcapsules and sophora biosurfactant were added. After ultrasonic dispersion for 13 min, a spinning solution was formed. The spinning solution was wet spun to obtain composite fibers.
[0165] Preparation Example 26
[0166] Composite fiber, including the following raw materials: 15g polylactic acid, 6g polyglutamic acid, 25g ethyl acetate, 7g hemp stalk core ultrafine powder, 9g aromatic microcapsule, 2g sophorolipid;
[0167] The aromatic microcapsules were prepared by Preparation Example 18;
[0168] Composite fiber, prepared by the following method:
[0169] Polylactic acid and polyglutamic acid were dissolved in ethyl acetate at 58°C and a rotation speed of 1400 r / min for 0.8 h, and then ultrafine hemp stalk core powder, aromatic microcapsules and sophora biosurfactant were added. After ultrasonic dispersion for 15 min, a spinning solution was formed. The spinning solution was wet spun to obtain composite fibers.
[0170] Preparation Example 27
[0171] Composite fiber, including the following raw materials: 18g polylactic acid, 6.5g polyglutamic acid, 28g ethyl acetate, 7.5g hemp stalk core ultrafine powder, 9.5g aromatic microcapsule, 2.5g sophorolipid;
[0172] The aromatic microcapsules were prepared by Preparation Example 19;
[0173] Composite fiber, prepared by the following method:
[0174] Polylactic acid and polyglutamic acid were dissolved in ethyl acetate at 58°C and a rotation speed of 1400 r / min for 0.6 h, and then ultrafine hemp stalk core powder, aromatic microcapsules and sophora biosurfactant were added. After ultrasonic dispersion for 18 min, a spinning solution was formed. The spinning solution was wet spun to obtain composite fibers.
[0175] Preparation Example 28
[0176] Composite fiber, including the following raw materials: 20g polylactic acid, 7g polyglutamic acid, 30g ethyl acetate, 8g hemp stalk core ultrafine powder, 10g aromatic microcapsule, 3g sophorolipid;
[0177] The aromatic microcapsules were prepared by Preparation Example 20;
[0178] Composite fiber, prepared by the following method:
[0179] Polylactic acid and polyglutamic acid are dissolved in ethyl acetate at 60°C and a rotation speed of 1500r / min. After dissolving for 0.5h, hemp stalk core ultrafine powder, aromatic microcapsules and sophora biosurfactant are added. After ultrasonic dispersion for 20min, a spinning solution is formed. The spinning solution is wet spun to obtain composite fibers.
[0180] Preparation Example 29
[0181] Preparation Example 29 is the same as Preparation Example 24, except that the aromatic microcapsules are prepared by Preparation Example 21.
[0182] Preparation Example 30
[0183] Preparation Example 30 is the same as Preparation Example 24, except that the aromatic microcapsules are prepared by Preparation Example 22.
[0184] Preparation Example 31
[0185] Preparation Example 31 is the same as Preparation Example 24, except that the aromatic microcapsules are prepared by Preparation Example 23.
[0186] Comparative Preparation Example 9
[0187] Comparative Preparation Example 9 is the same as Preparation Example 24, except that the aromatic microcapsules are prepared by Comparative Preparation Example 5.
[0188] Comparative Preparation Example 10
[0189] Comparative Preparation Example 10 is the same as Preparation Example 24, except that the aromatic microcapsules are prepared by Comparative Preparation Example 6.
[0190] Comparative Preparation Example 11
[0191] Comparative Preparation Example 11 is the same as Preparation Example 24, except that the aromatic microcapsules are prepared by Comparative Preparation Example 7.
[0192] Comparative Preparation Example 12
[0193] Comparative Preparation Example 12 is the same as Preparation Example 24, except that the aromatic microcapsules are prepared by Comparative Preparation Example 8.
[0194] Comparative Preparation Example 13
[0195] Comparative Preparation Example 13 is the same as Preparation Example 24, except that the aromatic microcapsules are the initial product obtained in step S2 of Preparation Example 16.
[0196] Comparative Preparation Example 14
[0197] Comparative Preparation Example 14 is the same as Preparation Example 24, except that the ultrafine hemp stalk core powder is not added.
[0198] Comparative Preparation Example 15
[0199] Comparative Preparation Example 15 is the same as Preparation Example 24, except that no sophorolipid is added.
[0200] Comparative Preparation Example 16
[0201] Comparative Preparation Example 16 is the same as Preparation Example 24, except that polylactic acid is replaced by polyglutamic acid.
[0202] Comparative Preparation Example 17
[0203] Comparative Preparation Example 17 is the same as Preparation Example 24, except that polyglutamic acid is replaced by polylactic acid.
[0204] Examples 1-8 provide multifunctional utility membrane fabrics.
[0205] Example 1
[0206] Multifunctional and practical membrane cloth, including the following raw materials: 150g chitosan fiber, 80g seaweed fiber, 300g composite fiber;
[0207] Wherein, the composite fiber is prepared by Preparation Example 24;
[0208] Functional and practical membrane cloth is made by the following method:
[0209] Chitosan fiber, seaweed fiber and composite fiber are combed, laid into a net and reinforced with hydroentanglement to produce a multifunctional and practical membrane cloth.
[0210] Example 2
[0211] Multifunctional and practical membrane cloth, including the following raw materials: 180g chitosan fiber, 90g seaweed fiber, 320g composite fiber;
[0212] Wherein, the composite fiber is prepared by Preparation Example 25;
[0213] Functional and practical membrane cloth is made by the following method:
[0214] Chitosan fiber, seaweed fiber and composite fiber are combed, laid into a net and reinforced with hydroentanglement to produce a multifunctional and practical membrane cloth.
[0215] Example 3
[0216] Multifunctional and practical membrane cloth, including the following raw materials: 200g chitosan fiber, 100g seaweed fiber, 350g composite fiber;
[0217] Wherein, the composite fiber is prepared by Preparation Example 26;
[0218] Functional and practical membrane cloth is made by the following method:
[0219] Chitosan fiber, seaweed fiber and composite fiber are combed, laid into a net and reinforced with hydroentanglement to produce a multifunctional and practical membrane cloth.
[0220] Example 4
[0221] A multifunctional practical membrane cloth, comprising the following raw materials: 230 g chitosan fiber, 110 g seaweed fiber, and 380 g composite fiber; wherein the composite fiber is prepared by Preparation Example 27;
[0222] Functional and practical membrane cloth is made by the following method:
[0223] Chitosan fiber, seaweed fiber and composite fiber are combed, laid into a net and reinforced with hydroentanglement to produce a multifunctional and practical membrane cloth.
[0224] Example 5
[0225] A multifunctional practical membrane cloth, comprising the following raw materials: 260g chitosan fiber, 120g seaweed fiber, and 400g composite fiber; wherein the composite fiber is prepared by Preparation Example 28;
[0226] Functional and practical membrane cloth is made by the following method:
[0227] Chitosan fiber, seaweed fiber and composite fiber are combed, laid into a net and reinforced with hydroentanglement to produce a multifunctional and practical membrane cloth.
[0228] Example 6
[0229] Example 6 is the same as Example 1, except that the composite fiber is prepared by Preparation Example 29.
[0230] Example 7
[0231] Example 7 is the same as Example 1, except that the composite fiber is prepared by Preparation Example 30.
[0232] Example 8
[0233] Example 8 is the same as Example 1, except that the composite fiber is prepared by Preparation Example 31.
[0234] In order to verify the properties of the multifunctional practical membrane cloth provided by the present application, the applicant set up comparative examples 1-9, wherein: comparative example 1
[0235] Comparative Example 1 is the same as Example 1, except that the composite fiber is prepared by Comparative Preparation Example 9.
[0236] Comparative Example 2
[0237] Comparative Example 2 is the same as Example 1, except that the composite fiber is prepared by Comparative Preparation Example 10.
[0238] Comparative Example 3
[0239] Comparative Example 3 is the same as Example 1, except that the composite fiber is prepared by Comparative Preparation Example 11.
[0240] Comparative Example 4
[0241] Comparative Example 4 is the same as Example 1, except that the composite fiber is prepared by Comparative Preparation Example 12.
[0242] Comparative Example 5
[0243] Comparative Example 5 is the same as Example 1, except that the composite fiber is prepared by Comparative Preparation Example 13.
[0244] Comparative Example 6
[0245] Comparative Example 6 is the same as Example 1, except that the composite fiber is prepared by Comparative Preparation Example 14.
[0246] Comparative Example 7
[0247] Comparative Example 7 is the same as Example 1, except that the composite fiber is prepared by Comparative Preparation Example 15.
[0248] Comparative Example 8
[0249] Comparative Example 8 is the same as Example 1, except that the composite fiber is prepared by Comparative Preparation Example 16.
[0250] Comparative Example 9
[0251] Comparative Example 9 is the same as Example 1, except that the composite fiber is prepared by Comparative Preparation Example 17.
[0252] The properties of the multifunctional practical membrane fabrics prepared in Examples 1-8 and Comparative Examples 1-9 of the present application were tested respectively, and the following result parameters were obtained, as shown in Table 1.
[0253] (1) Water absorption performance of the multifunctional practical membrane cloth: The multifunctional practical membrane cloths obtained in Examples 1-8 and Comparative Examples 1-9 were used as facial mask cloths, and the water absorption performance of the multifunctional practical membrane cloths was tested with reference to QB / T 2872-2017 "Facial Mask".
[0254] (2) Aroma sustained-release performance of the multifunctional practical membrane cloth: After the multifunctional practical membrane cloths obtained in Examples 1-8 and Comparative Examples 1-9 were used as facial mask cloths and dried, the aroma sustained-release performance of the multifunctional practical membrane cloths was tested. The presence of aroma was detected at intervals of 5 days, 10 days, 15 days, 20 days, 25 days, and 30 days, respectively. Among them, Y indicates the presence of aroma, and N indicates the absence of aroma.
[0255] Table 1:
[0256]
[0257] It can be seen from the data shown in Table 1 above that the comprehensive quality of the multifunctional practical membrane cloth prepared in Examples 1-8 of the present application is far superior to that of the multifunctional practical membrane cloth prepared in Comparative Examples 1-9. The multifunctional practical membrane cloth prepared in Examples 1-8 has significant water absorption performance and aroma sustained release performance. When used as a facial mask cloth, it can play a good role in hydrating and moisturizing. After being used as a facial mask cloth and dried, the aroma release time can be effectively maintained for one month, and it can be made into aromatherapy, which fully demonstrates that the multifunctional practical membrane cloth of the present application has excellent comprehensive performance, multiple practical functions, and broad application prospects.
[0258] It can be seen from Example 1 and Comparative Examples 1 and 2 that the composite fiber in Example 1 is prepared from Preparation Example 24, the aromatic microcapsules in Preparation Example 24 are prepared from Preparation Example 16, and the first capsule wall solution in Preparation Example 16 is prepared from Preparation Example 6. Modified chitosan is used in Preparation Example 6 and mixed with tea tree oil to form porous modified chitosan. Compared with Comparative Examples 1 and 2, the multifunctional practical membrane cloth prepared in Example 1 has better water absorption performance and better sustained-release performance of aroma.
[0259] It can be seen from Example 1 and Comparative Examples 3 and 4 that the composite fiber in Example 1 is prepared by Preparation Example 24, the aromatic microcapsules in Preparation Example 24 are prepared by Preparation Example 16, the second capsule wall solution in Preparation Example 16 is prepared by Preparation Example 11, and the second capsule wall solution in Preparation Example 11 includes porous starch and carboxymethyl-β-cyclodextrin. Compared with Comparative Examples 3 and 4, the fragrance of the multifunctional practical membrane cloth prepared in Example 1 can be slowly released, and the fragrance can last for one month.
[0260] It can be seen from Example 1 and Comparative Example 5 that the composite fiber in Example 1 is prepared by Preparation Example 24, and the fragrance microcapsules of Preparation Example 24 are prepared by Preparation Example 16, and the fragrance microcapsules have a double-layer structure; compared with the fragrance microcapsules in Comparative Example 5, which are the initial product obtained by step S2 in Preparation Example 16, the initial product has a single-layer structure. The multifunctional practical membrane cloth prepared in Example 1 not only has good fragrance sustained-release function, but also has more significant water absorption performance.
[0261] It can be seen from Example 1 compared with Comparative Examples 6 and 7 that the composite fiber in Example 1 is prepared by Preparation Example 24, and hemp stalk core ultrafine powder and sophora biosurfactant are added to the composite fiber. Compared with Comparative Examples 6 and 7, the comprehensive performance of the multifunctional practical membrane cloth prepared in Example 1 is more excellent.
[0262] It can be seen from Example 1 that compared with Comparative Examples 8 and 9, the composite fiber in Example 1 is prepared by Preparation Example 24, and polylactic acid and polyglutamic acid are added to the composite fiber. The synergistic effect of the two effectively improves the water absorption performance of the membrane cloth, thereby enabling the aromatic microcapsules of the composite fiber to slowly release aroma molecules. Compared with the membrane cloths of Comparative Examples 8 and 9, the multifunctional and practical membrane cloth of Example 1 has broad application prospects.
[0263] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make non-creative modifications to the present embodiment as needed, but such modifications are protected by patent law as long as they are within the scope of the claims of the present application.
Claims
1. Multifunctional practical membrane cloth, characterized in that: The multifunctional practical membrane cloth comprises the following raw materials in parts by weight: 15-26 parts of chitosan fiber, 8-12 parts of seaweed fiber, and 30-40 parts of composite fiber; The composite fiber comprises the following raw materials in parts by weight: 10-20 parts of polylactic acid, 5-7 parts of polyglutamic acid, 20-30 parts of ethyl acetate, 6-8 parts of superfine hemp stalk core powder, 8-10 parts of aromatic microcapsules, and 1-3 parts of sophorolipids; The aromatic microcapsules are prepared by the following method: S1. Add essence and PEG-60 hydrogenated castor oil into water, stir for 10-60 min at a temperature of 40-60° C. and a rotation speed of 600-800 r / min to mix evenly, and obtain a capsule core emulsion; S2, treating the capsule core emulsion obtained in step S1 with the first capsule wall solution by ultrasonic treatment at 50-70° C. for 30-40 min, and uniformly mixing them to form a microcapsule solution; and then spray drying to obtain a primary product; S3, subjecting the primary product obtained in step S2 to adsorption treatment with the second capsule wall solution at room temperature for 10-30 minutes; and then freeze-drying to obtain aromatic microcapsules; The first capsule wall solution is prepared by the following method: Firstly, the modified chitosan is dissolved in a succinic acid solution with a concentration of 5-20wt% to obtain a modified chitosan solution; then, the modified chitosan solution is fully mixed with tea tree oil, and homogenized and emulsified at a speed of 20000-25000 rpm for 30-60 seconds to obtain a first capsule wall solution; The modified chitosan is prepared by the following method: S11, dissolving chitosan in a citric acid solution with a concentration of 3-5wt%, fully dissolving to obtain a chitosan citric acid aqueous solution; dissolving octadecyl alcohol in ethanol at 50-60°C, mixing evenly, obtaining an octadecyl alcohol ethanol solution; S12, first uniformly mix the chitosan citric acid aqueous solution obtained in step S11 and the octadecyl alcohol ethanol solution to form a mixed solution; then add concentrated sulfuric acid with a concentration of 98wt% to the obtained mixed solution, mix evenly, and stir at 100-120°C and a speed of 600-800r / min to react for 8-10h; then adjust the pH to 8-11, let stand for 10-30min, filter, wash, and dry to obtain modified chitosan.
2. The multifunctional practical membrane cloth according to claim 1, characterized in that: The composite fiber is prepared by the following method: Polylactic acid and polyglutamic acid are dissolved in ethyl acetate at 50-60°C and a rotation speed of 1100-1500r / min for 0.5-1h, and then hemp stalk core ultrafine powder, aromatic microcapsules and sophorolipids are added and ultrasonically dispersed for 10-20min to form a spinning solution; the spinning solution is wet-spun to obtain composite fibers.
3. The multifunctional practical membrane cloth according to claim 1, characterized in that: The mass ratio of the essence, PEG-60 hydrogenated castor oil and water is 8-12:1-2:20; the mass ratio of the capsule core emulsion to the first capsule wall solution is 1:1.2-1.6; and the mass ratio of the primary product to the second capsule wall solution is 1:1.1-1.
5.
4. The multifunctional practical membrane cloth according to claim 1, characterized in that: The mass ratio of the modified chitosan, the succinic acid solution and the tea tree oil is 20:40-60:5-7.
5. The multifunctional practical membrane cloth according to claim 1, characterized in that: The modified chitosan comprises the following raw materials in parts by weight: 11-15 parts of chitosan, 30-50 parts of citric acid solution, 5-9 parts of octadecyl alcohol, 10-30 parts of ethanol, and 6-12 parts of concentrated sulfuric acid.
6. The multifunctional practical membrane cloth according to claim 1, characterized in that: The second capsule wall solution is prepared by the following method: According to weight, 1-3 parts of porous starch and 10-14 parts of carboxymethyl-β-cyclodextrin are added to 20-30 parts of water, and stirred at 50-60° C. and 600-800 r / min for 10-30 min to obtain a second capsule wall solution.
7. The multifunctional practical membrane cloth according to claim 1, characterized in that: The multifunctional practical membrane cloth is prepared by the following method: Chitosan fiber, seaweed fiber and composite fiber are combed, laid into a net and reinforced with hydroentanglement to produce a multifunctional and practical membrane cloth.
Citation Information
Patent Citations
Telangiectasis-removal facial mask containing chamomile extract
CN107049851A
Gamma-polyglutamic acid / polylactic acid biocompatible nanofiber membrane and preparing method
CN107460639A
Antibacterial and antiviral functional fiber and preparation method thereof
CN111235678A