Resin composition, optical fiber, and method for producing optical fiber

By using a resin composition of urethane (meth)acrylamide, the problem of slow curing speed of the primary coated resin layer of the optical fiber is solved, and rapid curing and defect-free resin layer formation is achieved, thereby improving the productivity and resistance of the optical fiber. Microbending characteristics.

CN116348512BActive Publication Date: 2024-12-06SUMITOMO ELECTRIC INDUSTRIES LTD
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
CN202180061862.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-10-05
Filing Date
2021-08-02
Publication Date
2024-12-06
Estimated Expiration
2041-08-02

AI Technical Summary

Technical Problem

The primary coated resin composition of the existing optical fiber is slow to cure, resulting in possible defects and peeling between the glass fiber and the resin layer, increasing transmission loss and affecting productivity.

Method used

A resin having a (meth)acrylamide group at the end of the urethane bond is adopted using a photopolymerizable compound containing a urethane (meth)acrylamide and a photopolymerization initiator. The composition, by adjusting the composition and process conditions of the resin composition, such as coating and ultraviolet curing, improves the curing speed and Young's modulus balance of the primary resin layer.

Benefits of technology

The rapid curing, defect-free primary resin layer formation is achieved, which improves the productivity and microbending resistance of the optical fiber, and reduces transmission losses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116348512B_ABST
    Figure CN116348512B_ABST
Patent Text Reader

Abstract

A resin composition for primary coating of an optical fiber, comprising: a photopolymerizable compound including urethane (meth) acrylamide having a (meth) acrylamide group at at least one end of a urethane bond; and a photopolymerization initiator.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a resin composition for primary coating of an optical fiber, an optical fiber, and a method for producing the optical fiber.

[0002] This application claims the priority based on Japanese Application No. 2020-168494 and Japanese Application No. 2020-168496 filed on October 5, 2020, and cites all the contents described in the said Japanese Applications. Background Art

[0003] Generally, an optical fiber has a coating resin layer for protecting a glass fiber as a light transmission body. The coating resin layer is composed of two layers, for example, a primary resin layer in contact with the glass fiber and a secondary resin layer formed on the outer layer of the primary resin layer. It is known that the resin composition for the primary coating of the optical fiber uses a carbamate (meth)acrylate which is a reaction product of a polyol, a diisocyanate, and a hydroxyl-containing (meth)acrylate. For example, patent documents 1 to 5 describe a resin composition for the primary coating containing a carbamate (meth)acrylate as an oligomer.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2009-197163

[0007] Patent Document 2: Japanese Patent Application Publication No. 2012-111674

[0008] Patent Document 3: Japanese Patent Application Publication No. 2013-136783

[0009] Patent Document 4: Japanese Patent Application No. 2013-501125

[0010] Patent Document 5: Japanese Patent Application Publication No. 2014-114208 Summary of the invention

[0011] A resin composition for primary coating of an optical fiber according to one embodiment of the present disclosure contains a photopolymerizable compound including urethane (meth)acrylamide having a (meth)acrylamide group at at least one end of a urethane bond, and a photopolymerization initiator. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] [ Figure 1 ] Figure 1 This is a schematic cross-sectional view showing an example of the optical fiber according to the present embodiment. DETAILED DESCRIPTION

[0013] [Problems to be Solved by the Present Disclosure]

[0014] Compared with the resin composition for secondary coating, the curing speed of the resin composition for primary coating tends to be slower. In order to improve the productivity of optical fiber, it is required to increase the curing speed of the resin composition for primary coating. When the primary resin layer is not sufficiently cured, defects (voids) may be generated in the primary resin layer, or peeling may occur between the glass fiber and the primary resin layer, which may easily lead to an increase in transmission loss.

[0015] An object of the present disclosure is to provide a resin composition that has a fast curing speed and can form a resin layer suitable for primary coating of an optical fiber, and an optical fiber that is excellent in productivity.

[0016] [Effects of the present disclosure]

[0017] According to the present disclosure, a resin composition that has a fast curing speed and can form a resin layer suitable for primary coating of an optical fiber, and an optical fiber with excellent productivity can be provided.

[0018] [Description of Embodiments of the Present Disclosure]

[0019] First, the contents of the embodiments of the present disclosure are listed and described. One embodiment of the present disclosure relates to a primary coating resin composition for optical fiber, comprising a photopolymerizable compound containing urethane (meth) acrylamide having a (meth) acrylamide group at at least one end of a urethane bond, and a photopolymerization initiator.

[0020] Such a resin composition has a high curing speed and does not cause defects in the primary resin layer or separation between the glass fiber and the primary resin layer. Therefore, a resin layer suitable for primary coating of optical fiber can be formed, thereby improving the productivity of optical fiber.

[0021] From the viewpoint of increasing the curing speed of the primary resin layer, the urethane (meth)acrylamide may include a urethane oligomer having a (meth)acrylamide group at one end of a urethane bond, a urethane oligomer having (meth)acrylamide groups at both ends of a urethane bond, or a mixture thereof.

[0022] From the viewpoint of further increasing the curing speed of the primary resin layer, the urethane oligomer having a (meth)acrylamide group at one end of the urethane bond may include a urethane oligomer having a (meth)acrylamide group at one end of the urethane bond and a (meth)acryloyloxy group at the other end.

[0023] The carbamate (meth)acrylamide may include: a carbamate oligomer having (meth)acrylamide groups at both ends of a carbamate bond; and a carbamate oligomer having a (meth)acrylamide group at one end of a carbamate bond and a group based on at least one compound selected from a monohydric alcohol and a silane compound containing active hydrogen at the other end. Thus, it is easy to adjust the balance between the curing speed of the resin composition and the Young's modulus of the primary resin layer.

[0024] From the viewpoint of improving the photocurability of the resin composition, the content of the urethane (meth)acrylamide may be 10 parts by mass or more and 90 parts by mass or less based on 100 parts by mass of the total amount of the resin composition.

[0025] From the viewpoint of reducing the Young's modulus of the resin composition, the number average molecular weight of the urethane (meth)acrylamide may be 10,000 or more and 37,000 or less.

[0026] In order to adjust the Young's modulus of the primary resin layer, the photopolymerizable compound may further contain a (meth)acrylate.

[0027] In order to further increase the curing speed of the resin composition, the photopolymerizable compound may further contain an N-vinyl compound or a (meth)acrylamide compound.

[0028] An optical fiber according to one embodiment of the present disclosure includes: a glass fiber including a core and a cladding, a primary resin layer in contact with the glass fiber and covering the glass fiber, and a secondary resin layer covering the primary resin layer, wherein the primary resin layer includes a cured product of the above-mentioned resin composition. Such an optical fiber does not cause defects in the primary resin layer and does not peel off between the glass fiber and the primary resin layer, and thus has excellent productivity.

[0029] One embodiment of the present disclosure relates to a method for manufacturing an optical fiber, comprising: a coating step of coating the resin composition on the outer periphery of a glass fiber including a core and a cladding; and a curing step of curing the resin composition by irradiating ultraviolet light after the coating step. Thus, an optical fiber with excellent productivity can be manufactured.

[0030] [Details of the embodiments of the present disclosure]

[0031] Specific examples of the resin composition and optical fiber involved in the present embodiment are described with reference to the accompanying drawings as needed. It should be noted that the present disclosure is not limited to these examples, but is represented by the claims, and is intended to include all changes within the meaning and scope equivalent to the claims. In the following description, the same elements are marked with the same symbols in the description of the accompanying drawings, and repeated descriptions are omitted. (Meth)acrylamide in this specification refers to acrylamide or its corresponding methacrylamide. The same is true for other similar expressions such as (meth)acryloyloxy, (meth)acrylate, etc.

[0032] (Resin composition)

[0033] The resin composition involved in this embodiment contains: a photopolymerizable compound including carbamate (meth) acrylamide, and a photopolymerization initiator. Carbamate (meth) acrylamide is a carbamate oligomer having a (meth) acrylamide group at at least one end of a carbamate bond. The photopolymerizability of the (meth) acrylamide group is better than that of the (meth) acryloyloxy group, so the curing speed of the carbamate (meth) acrylamide is faster than that of the carbamate (meth) acrylate without the (meth) acrylamide group, thereby improving the productivity of the optical fiber.

[0034] The carbamate (meth)acrylamide may be a carbamate oligomer having a (meth)acrylamide group at one end of the carbamate bond, or a carbamate oligomer having a (meth)acrylamide group at both ends of the carbamate bond. That is, the carbamate (meth)acrylamide involved in the present embodiment may include: a carbamate oligomer having a (meth)acrylamide group at one end of the carbamate bond, a carbamate oligomer having a (meth)acrylamide group at both ends of the carbamate bond, or a mixture thereof.

[0035] From the viewpoint of further improving the curing speed of the resin composition, the carbamate (meth) acrylamide involved in the present embodiment may include a carbamate oligomer having a (meth) acrylamide group at both ends of the carbamate bond. The carbamate oligomer having a (meth) acrylamide group at both ends of the carbamate bond may be a reaction product of a polyol, a diisocyanate, and an N-hydroxyalkyl (meth) acrylamide.

[0036] Examples of the polyol include polyether polyol, polyester polyol, polycaprolactone polyol, polycarbonate polyol, polybutadiene polyol, and bisphenol A-ethylene oxide addition diol. Examples of the polyether polyol include polytetramethylene ether glycol, polyethylene glycol, and polypropylene glycol. From the viewpoint of easy adjustment of the Young's modulus and elongation at break of the resin layer, polypropylene glycol, polytetramethylene ether glycol, or polycarbonate polyol is preferably used as the polyol.

[0037] From the viewpoint of obtaining a Young's modulus suitable for the primary resin layer, the number average molecular weight (Mn) of the polyol is preferably 2,000 to 20,000, more preferably 2,400 to 19,000, and further preferably 2,800 to 18,000.

[0038] Examples of the diisocyanate include 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, 1,5-naphthalene diisocyanate, norbornene diisocyanate, 1,5-pentamethylene diisocyanate, tetramethylxylylene diisocyanate, and trimethylhexamethylene diisocyanate.

[0039] Examples of the N-hydroxyalkyl (meth)acrylamide include N-methylol (meth)acrylamide, N-hydroxyethyl (meth)acrylamide, and N,N-dimethylol (meth)acrylamide. As the N-hydroxyalkyl (meth)acrylamide, N-hydroxyethyl acrylamide is preferably used.

[0040] From the viewpoint of adjusting the Young's modulus of the primary resin layer, the urethane (meth) acrylamide may further have a group based on at least one compound selected from a monohydric alcohol and a silane compound containing active hydrogen. Such urethane (meth) acrylamide may be a reaction product of a polyol, a diisocyanate, an N-hydroxyalkyl (meth) acrylamide, and at least one compound selected from a monohydric alcohol and a silane compound containing active hydrogen.

[0041] From the viewpoint of adjusting the balance between the curing speed of the resin composition and the Young's modulus of the primary resin layer, the urethane (meth)acrylamide may further contain a urethane oligomer having a (meth)acrylamide group at one end of the urethane bond and a group based on at least one compound selected from a monohydric alcohol and an active hydrogen-containing silane compound at the other end.

[0042] By introducing a monohydric alcohol-based group into urethane (meth)acrylamide, the ratio of the (meth)acrylamide group as a photopolymerizable group can be reduced, thereby reducing the Young's modulus of the primary resin layer.

[0043] By making the resin composition involved in this embodiment contain a carbamate oligomer having a (meth)acrylamide group at one end of the carbamate bond and a group based on a monohydric alcohol at the other end, the ratio of the photopolymerizable group is reduced, thereby easily reducing the Young's modulus of the primary resin layer. The carbamate oligomer having a (meth)acrylamide group and a group based on a monohydric alcohol is a reaction product of a polyol, a diisocyanate, an N-hydroxyalkyl (meth)acrylamide, and a monohydric alcohol.

[0044] Examples of the monohydric alcohol include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 2-methyl-2-propanol, 1-pentanol, 2-pentanol, 3-pentanol, 2-methyl-1-butanol, 3-methyl-1-butanol, 2-methyl-2-butanol, and 3-methyl-2-butanol.

[0045] By introducing a group based on a silane compound containing active hydrogen into urethane (meth)acrylamide, the ratio of the (meth)acrylamide group as a photopolymerizable group can be reduced, thereby reducing the Young's modulus of the primary resin layer and improving the adhesion to the glass fiber.

[0046] By making the resin composition involved in the present embodiment contain a carbamate oligomer having a (meth)acrylamide group at one end of the carbamate bond and a silane compound containing active hydrogen at the other end, the Young's modulus of the primary resin layer can be reduced, thereby improving the adhesion with the glass fiber. The carbamate oligomer having a (meth)acrylamide group and a group based on a silane compound containing active hydrogen is a reaction product of a polyol, a diisocyanate, an N-hydroxyalkyl (meth)acrylamide, and a silane compound containing active hydrogen.

[0047] Examples of the silane compound containing active hydrogen include N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, and 3-mercaptopropyltrimethoxysilane.

[0048] Examples of the synthesis method of urethane (meth)acrylamide include: a method in which a polyol is reacted with a diisocyanate and then reacted with N-hydroxyalkyl (meth)acrylamide (a monohydric alcohol or a silane compound containing active hydrogen as required); a method in which a diisocyanate is reacted with N-hydroxyalkyl (meth)acrylamide (a monohydric alcohol or a silane compound containing active hydrogen as required) and then reacted with a polyol; and a method in which a polyol, a diisocyanate, and N-hydroxyalkyl (meth)acrylamide (a monohydric alcohol or a compound containing active hydrogen as required) are reacted simultaneously.

[0049] When a bifunctional polyol is used, a method is preferably used in which a hydroxyl group (OH) of the polyol is reacted with an isocyanate group (NCO) of a diisocyanate, followed by a reaction with N-hydroxyalkyl (meth) acrylamide (a monohydric alcohol or a silane compound containing active hydrogen as required). When a trifunctional or higher polyol is used, a method is preferably used in which a diisocyanate is reacted with N-hydroxyalkyl (meth) acrylamide (a monohydric alcohol or a silane compound containing active hydrogen as required), followed by a reaction with a polyol.

[0050] The preparation of urethane (meth) acrylamide is described below by giving a specific example, for example, using bifunctional polypropylene polyol (polypropylene glycol) as a polyol, using 2,4-toluene diisocyanate as a diisocyanate, using N-hydroxyethyl acrylamide as an N-hydroxyalkyl (meth) acrylamide, using methanol as a monohydric alcohol, and using 3-mercaptopropyltrimethoxysilane as a silane compound containing active hydrogen.

[0051] First, polypropylene glycol is reacted with 2,4-toluene diisocyanate to synthesize an NCO-terminated prepolymer. Next, N-hydroxyethyl acrylamide, methanol, and 3-mercaptopropyltrimethoxysilane are reacted with the NCO-terminated prepolymer to synthesize urethane acrylamide. The urethane acrylamide can be represented by a mixture of the following (1) to (3).

[0052] Am-(UIUP)nUIU-Am(1)

[0053] Am-(UIUP)nUIUM(2)

[0054] Am-(UIUP)nUIU-SC(3)

[0055] Here, Am represents a residue of N-hydroxyethyl acrylamide, M represents a residue of methanol, SC represents a residue of 3-mercaptopropyltrimethoxysilane, U represents a (thio)urethane bond, I represents a residue of 2,4-toluene diisocyanate, P represents a residue of polypropylene glycol, and n is an integer greater than or equal to 1.

[0056] The reaction product during synthesis of urethane acrylamide may contain the following (4) to (6) as by-products. (4) to (6) are called adducts and function as one type of monomer.

[0057] Am-UIUIU-Am(4)

[0058] Am-UIUIUM(5)

[0059] Am-UIUIU-SC(6)

[0060] The reaction product during synthesis of urethane acrylamide may contain the following (7) to (12) as by-products. Since (7) to (12) do not have a photopolymerizable group, it is desirable that they are not generated.

[0061] M-(UIUP)nUIUM(7)

[0062] Sc-(UIUP)nUIU-SC(8)

[0063] M-(UIUP)nUIU-SC(9)

[0064] MUIUM(10)

[0065] MUIU-SC(11)

[0066] SC-UIU-SC(12)

[0067] In the preparation of urethane (meth)acrylamide, the addition of methanol and 3-mercaptopropyltrimethoxysilane is optional. When methanol and 3-mercaptopropyltrimethoxysilane are not added, (1) is generated as a main component and (4) is generated as a by-product.

[0068] The molar ratio of NCO to OH (NCO / OH) when the polyol reacts with the diisocyanate is preferably 1.1 to 4.0, more preferably 1.2 to 3.5, and even more preferably 1.4 to 3.0. The molar ratio of the total of N-hydroxyalkyl (meth) acrylamide, monohydric alcohol, and active hydrogen-containing silane compound to NCO of the NCO-terminated prepolymer is preferably 1.00 to 1.15, more preferably 1.03 to 1.10. The molar ratio of the total of monohydric alcohol and active hydrogen-containing silane compound to NCO of the NCO-terminated prepolymer is preferably 0 to 0.5.

[0069] From the viewpoint of adjusting the balance between the curing speed of the resin composition and the Young's modulus of the resin layer, the urethane (meth) acrylamide may include: a urethane oligomer having a (meth) acrylamide group at both ends of the urethane bond; and a urethane oligomer having a (meth) acrylamide group at one end of the urethane bond and having a group based on at least one selected from a monohydric alcohol and an active hydrogen-containing silane compound at the other end.

[0070] From the viewpoint of improving the photocurability of the resin composition, the content of urethane (meth) acrylamide is preferably 10 parts by mass or more and 90 parts by mass or less, more preferably 20 parts by mass or more and 80 parts by mass or less, and further preferably 30 parts by mass or more and 75 parts by mass or less, based on 100 parts by mass of the total amount of the resin composition.

[0071] The carbamate oligomer having a (meth)acrylamide group at one end of the carbamate bond may also include a carbamate oligomer having a (meth)acrylamide group at one end of the carbamate bond and a (meth)acryloyloxy group at the other end. The carbamate oligomer having a (meth)acrylamide group and a (meth)acryloyloxy group as photopolymerizable groups has a faster curing speed than the carbamate oligomer having only a (meth)acryloyloxy group, and can improve the productivity of the optical fiber.

[0072] The urethane oligomer having a (meth)acrylamide group and a (meth)acryloyloxy group is a reaction product of a polyol, a diisocyanate, an N-hydroxyalkyl (meth)acrylamide, and a hydroxyl group-containing (meth)acrylate.

[0073] Examples of the hydroxyl-containing (meth)acrylate include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, caprolactone (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxyethyl phthalate, 2-hydroxy-O-phenylphenol propyl (meth)acrylate, 2-hydroxy-3-methacrylpropyl acrylate, trimethylolpropane di(meth)acrylate, and pentaerythritol tri(meth)acrylate. As the hydroxyl-containing (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, or 2-hydroxybutyl (meth)acrylate is preferably used.

[0074] Other methods for synthesizing urethane (meth)acrylamide when using a hydroxyl-containing (meth)acrylate as an essential component include, for example, a method in which a polyol is reacted with a diisocyanate and then reacted with N-hydroxyalkyl (meth)acrylamide and a hydroxyl-containing (meth)acrylate (a monohydric alcohol or a silane compound containing active hydrogen as required); a method in which a diisocyanate, N-hydroxyalkyl (meth)acrylamide and a hydroxyl-containing (meth)acrylate (a monohydric alcohol or a silane compound containing active hydrogen as required) are reacted and then reacted with a polyol; and a method in which a polyol, a diisocyanate, an N-hydroxyalkyl (meth)acrylamide and a hydroxyl-containing (meth)acrylate (a monohydric alcohol or a silane compound containing active hydrogen as required) are reacted simultaneously.

[0075] When a bifunctional polyol is used, a method is preferably used in which a hydroxyl group (OH) of the polyol is reacted with an isocyanate group (NCO) of a diisocyanate, and then the reaction is carried out with N-hydroxyalkyl (meth) acrylamide and a hydroxyl-containing (meth) acrylate (a monohydric alcohol or a silane compound containing active hydrogen as required). When a trifunctional or higher polyol is used, a method is preferably used in which a diisocyanate, N-hydroxyalkyl (meth) acrylamide and a hydroxyl-containing (meth) acrylate (a monohydric alcohol or a silane compound containing active hydrogen as required) are reacted, and then the reaction is carried out with a polyol.

[0076] The following is a specific example of the preparation of a urethane oligomer having a (meth)acrylamide group and a (meth)acryloyloxy group. For example, a bifunctional polypropylene polyol (polypropylene glycol) is used as a polyol, 2,4-toluene diisocyanate is used as a diisocyanate, N-hydroxyethyl acrylamide is used as an N-hydroxyalkyl (meth)acrylamide, 2-hydroxyethyl acrylate is used as a hydroxyl group-containing (meth)acrylate, methanol is used as a monohydric alcohol, and 3-mercaptopropyltrimethoxysilane is used as a silane compound containing active hydrogen.

[0077] First, polypropylene glycol is reacted with 2,4-toluene diisocyanate to synthesize an NCO-terminated prepolymer. Next, N-hydroxyethyl acrylamide, 2-hydroxyethyl acrylate, methanol, and 3-mercaptopropyltrimethoxysilane are reacted with the NCO-terminated prepolymer to synthesize a urethane oligomer. The urethane oligomer can be represented by a mixture of the following formulas (21) to (27).

[0078] Am-(UIUP)nUIU-Ac(21)

[0079] Am-(UIUP)nUIU-Am(22)

[0080] Ac-(UIUP)nUIU-Ac(23)

[0081] Am-(UIUP)nUIUM(24)

[0082] Am-(UIUP)nUIU-SC(25)

[0083] Ac-(UIUP)nUIUM(26)

[0084] Ac-(UIUP)nUIU-SC(27)

[0085] Here, Am represents a residue of N-hydroxyethyl acrylamide, Ac represents a residue of 2-hydroxyethyl acrylate, M represents a residue of methanol, SC represents a residue of 3-mercaptopropyltrimethoxysilane, U represents a (thio)urethane bond, I represents a residue of 2,4-toluene diisocyanate, P represents a residue of polypropylene glycol, and n is an integer greater than 1.

[0086] The reaction product when synthesizing a urethane oligomer may contain the following (28) to (34) as by-products. (28) to (34) are called adducts, and they function as one type of monomer.

[0087] Am-UIU-Ac(28)

[0088] Am-UIU-Am(29)

[0089] Ac-UIU-Ac(30)

[0090] Am-UIUM(31)

[0091] Am-UIU-SC(32)

[0092] Ac-UIUM(33)

[0093] Ac-UIU-SC(34)

[0094] The reaction product when synthesizing the urethane oligomer may contain the following (35) to (40) as by-products. Since (35) to (40) do not have a photopolymerizable group, it is desirable that they are not generated.

[0095] M-(UIUP)nUIUM(35)

[0096] SC-(UIUP)nUIU-SC(36)

[0097] M-(UIUP)nUIU-SC(37)

[0098] MUIUM(38)

[0099] MUIU-SC(39)

[0100] SC-UIU-SC(40)

[0101] When preparing the urethane oligomer, the addition of methanol and 3-mercaptopropyltrimethoxysilane is optional. When methanol and 3-mercaptopropyltrimethoxysilane are not added, a mixture of (21) to (23) and (28) to (30) is produced.

[0102] The molar ratio of NCO to OH (NCO / OH) when the polyol reacts with the diisocyanate is preferably 1.1 to 4.0, more preferably 1.2 to 3.5, and further preferably 1.4 to 3.0. The molar ratio of N-hydroxyalkyl (meth) acrylamide to NCO of the NCO-terminated prepolymer is preferably 0.1 to 0.95, more preferably 0.2 to 0.8. The molar ratio of hydroxyl-containing (meth) acrylate to NCO of the NCO-terminated prepolymer is preferably 0.1 to 0.95, more preferably 0.2 to 0.9. The molar ratio of the total of N-hydroxyalkyl (meth) acrylamide, hydroxyl-containing (meth) acrylate, monohydric alcohol and active hydrogen-containing silane compound to NCO of the NCO-terminated prepolymer is preferably 1.00 to 1.15, more preferably 1.03 to 1.10. The molar ratio of the total of monohydric alcohol and active hydrogen-containing silane compound to NCO of the NCO-terminated prepolymer is preferably 0 to 0.5.

[0103] From the viewpoint of improving the photocurability of the resin composition, the content of the urethane (meth)acrylamide comprising a urethane oligomer having a (meth)acrylamide group and a (meth)acryloyloxy group is preferably 30 parts by mass or more and 90 parts by mass or less, more preferably 40 parts by mass or more and 80 parts by mass or less, and further preferably 45 parts by mass or more and 75 parts by mass or less, based on 100 parts by mass of the total amount of the resin composition.

[0104] From the viewpoint of obtaining a Young's modulus suitable for the primary resin layer, the number average molecular weight (Mn) of the urethane (meth)acrylamide is preferably 6,000 to 40,000, more preferably 8,000 to 38,000, and even more preferably 10,000 to 37,000.

[0105] The photopolymerizable compound involved in this embodiment may further include carbamate (meth) acrylate. Carbamate (meth) acrylate is a carbamate oligomer having a (meth) acryloyloxy group but not a (meth) acrylamide group. Carbamate (meth) acrylate is obtained by reacting a polyol, a diisocyanate, and a hydroxyl-containing (meth) acrylate by a conventional method.

[0106] The polyol and diisocyanate used for the synthesis of the urethane (meth)acrylate are not particularly limited, and they can be selected from the compounds exemplified in the synthesis of the urethane (meth)acrylamide described above and used.

[0107] Examples of the hydroxyl-containing (meth)acrylate include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, caprolactone (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxyethyl phthalate, 2-hydroxy-O-phenylphenol propyl (meth)acrylate, 2-hydroxy-3-methacrylpropyl acrylate, trimethylolpropane di(meth)acrylate, and pentaerythritol tri(meth)acrylate.

[0108] From the viewpoint of obtaining a Young's modulus suitable for the primary resin layer, the Mn of the urethane (meth)acrylate may be 5,000 to 30,000, 6,000 to 20,000, or 8,000 to 15,000.

[0109] The total content of the urethane (meth)acrylamide and the urethane (meth)acrylate may be 40 parts by mass or more and 90 parts by mass or less based on the total amount of the resin composition.

[0110] As a catalyst for synthesizing carbamate (meth) acrylamide and carbamate (meth) acrylate, an organic tin compound or an amine compound can be used. Examples of the organic tin compound include dibutyltin dilaurate, dibutyltin diacetate, dibutyltin maleate, dibutyltin bis(2-ethylhexyl thioglycolate), dibutyltin bis(isooctyl thioglycolate), and dibutyltin oxide. From the viewpoint of availability or catalyst performance, dibutyltin dilaurate or dibutyltin diacetate is preferably used as the catalyst.

[0111] The photopolymerizable compound involved in this embodiment may further include a photopolymerizable compound (hereinafter referred to as a "monomer") that does not have a carbamate bond. Examples of the monomer include: (meth)acrylates, N-vinyl compounds, and (meth)acrylamide compounds. The monomer may be a monofunctional monomer having one photopolymerizable ethylenically unsaturated group, or a polyfunctional monomer having two or more ethylenically unsaturated groups.

[0112] Examples of the monofunctional (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, isopentyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, phenoxyethyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, benzyl (meth)acrylate, and (meth)acrylate. dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentyl (meth)acrylate, nonylphenol polyethylene glycol (meth)acrylate, nonylphenoxy polyethylene glycol (meth)acrylate, isobornyl (meth)acrylate, 3-phenoxybenzyl (meth)acrylate, methylphenoxyethyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, m-phenoxybenzyl (meth)acrylate, 2-(2-ethoxyethoxy)ethyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl acrylate, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, and ω-carboxy-polycaprolactone (meth)acrylate.

[0113] Examples of the polyfunctional (meth)acrylate include ethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, cyclohexanedimethanol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, 1,4-butylene glycol di(meth)acrylate. Acid ester, diethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, 1,14-tetradecanediol di(meth)acrylate, 1,16-hexadecanediol di(meth)acrylate, 1,20-eicosandiol di(meth)acrylate, isopentyl glycol di(meth)acrylate, 3-ethyl-1,8-octanediol di(meth)acrylate, tricyclodecanol di(meth)acrylate, 9,9-bis[4-(2-hydroxyethoxy)phenyl] ] bifunctional monomers such as fluorene di(meth)acrylate, bisphenol A epoxy di(meth)acrylate, bisphenol F epoxy di(meth)acrylate, bisphenol A EO adduct di(meth)acrylate, bisphenol F EO adduct di(meth)acrylate, bisphenol A PO adduct di(meth)acrylate, bisphenol F PO adduct di(meth)acrylate; trimethylolpropane tri(meth)acrylate, trimethyloloctane tri(meth)acrylate, trimethylolpropane polyethoxy tri(meth)acrylate, trimethylolpropane polypropoxy tri(meth)acrylate, trimethylol Monomers having three or more functions, such as propane polyethoxy polypropoxy tri(meth)acrylate, tri[(meth)acryloyloxyethyl] isocyanurate, pentaerythritol tri(meth)acrylate, pentaerythritol polyethoxy tetra(meth)acrylate, pentaerythritol polypropoxy tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and caprolactone-modified tri[(meth)acryloyloxyethyl] isocyanurate.

[0114] By making the photopolymerizable compound contain (meth)acrylate, the Young's modulus of the resin layer can be adjusted. The content of (meth)acrylate can be 1 to 60 parts by mass, 5 to 50 parts by mass, or 10 to 40 parts by mass based on 100 parts by mass of the total amount of the resin composition.

[0115] Examples of the N-vinyl compound include N-vinylpyrrolidone, N-vinylcaprolactam, N-vinylmethyloxazolidinone, N-vinylimidazole, and N-vinyl-N-methylacetamide.

[0116] By including an N-vinyl compound in the photopolymerizable compound, the curing speed of the resin composition can be further increased. The content of the N-vinyl compound can be 1 to 30 parts by mass, 2 to 20 parts by mass, or 5 to 15 parts by mass, based on 100 parts by mass of the total amount of the resin composition.

[0117] Examples of the (meth)acrylamide compound include dimethyl (meth)acrylamide, diethyl (meth)acrylamide, (meth)acryloyl morpholine, hydroxymethyl (meth)acrylamide, hydroxyethyl (meth)acrylamide, isopropyl (meth)acrylamide, dimethylaminopropyl (meth)acrylamide, dimethylaminopropyl acrylamide / methyl chloride salt, diacetone acrylamide, (meth)acryloyl piperidine, (meth)acryloyl pyrrolidine, (meth)acrylamide, N-hexyl (meth)acrylamide, N-methyl (meth)acrylamide, N-butyl (meth)acrylamide, N-methylol (meth)acrylamide, and N-methylolpropane (meth)acrylamide.

[0118] By making the photopolymerizable compound contain a (meth)acrylamide compound, the curing speed of the resin composition can be further increased. The content of the (meth)acrylamide compound can be 1 to 30 parts by mass, 2 to 20 parts by mass, or 5 to 15 parts by mass, based on 100 parts by mass of the total amount of the resin composition.

[0119] The photopolymerization initiator can be appropriately selected from known radical photopolymerization initiators and used. Examples of the photopolymerization initiator include 1-hydroxycyclohexyl phenyl ketone (Omnirad 184, manufactured by IGM Resins), 2,2-dimethoxy-2-phenylacetophenone (Omnirad 651, manufactured by IGM Resins), 2,4,6-trimethylbenzoyldiphenylphosphine oxide (Omnirad TPO, manufactured by IGM Resins), (2,4,6-trimethylbenzoyl)-phenylphosphonic acid ethyl ester (Omnirad TPO-L, manufactured by IGM Resins), 2-benzyl-2-dimethylamino-4'-morpholinobutylphenone (Omnirad 369, manufactured by IGM Resins), 2-dimethylamino-2-(4-methyl-benzyl)-1-(4-morpholin-4-yl-phenyl)-butan-1-one (Omnirad 379, manufactured by IGM Resins). Resins Co., Ltd.), bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (Omnirad 819, manufactured by IGM Resins Co., Ltd.), and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one (Omnirad 907, manufactured by IGM Resins Co., Ltd.).

[0120] The photopolymerization initiator may be used in combination of two or more. From the viewpoint of excellent rapid curability of the resin composition, the photopolymerization initiator preferably contains 2,4,6-trimethylbenzoyldiphenylphosphine oxide.

[0121] The content of the photopolymerization initiator is preferably 0.2 to 5 parts by mass, more preferably 0.3 to 4 parts by mass, and even more preferably 0.4 to 3 parts by mass, based on the total amount of the resin composition.

[0122] The resin composition according to the present embodiment may further contain a photoacid generator, a silane coupling agent, a leveling agent, a defoaming agent, an antioxidant, an ultraviolet absorber, and the like.

[0123] As the photoacid generator, a + B - As the photoacid generator, for example, sulfonium salts such as CPI-100P, 110P (manufactured by San-Apro Co., Ltd.), Omnicat 270, 290 (manufactured by IGM Resins Co., Ltd.); iodonium salts such as Omnicat 250 (manufactured by IGM Resins Co., Ltd.), WPI-113, 116, 124, 169, 170 (manufactured by FUJIFILM Wako Pure Chemical Corporation) can be listed.

[0124] Examples of the silane coupling agent include tetramethyl silicate, tetraethyl silicate, mercaptopropyl trimethoxysilane, vinyl trichlorosilane, vinyl triethoxysilane, vinyl tri(β-methoxy-ethoxy)silane, β-(3,4-epoxycyclohexyl)-ethyl trimethoxysilane, dimethoxydimethylsilane, diethoxydimethylsilane, 3-acryloxypropyl trimethoxysilane, γ-glycidoxypropyl trimethoxysilane, γ-glycidoxypropyl methyl diethoxysilane, γ-methacryloxypropyl trimethoxysilane, N-(β-aminoethyl)silane,

[0047] The invention also includes the following:

[0048] N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethyldimethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, γ-chloropropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, bis-[3-(triethoxysilyl)propyl]tetrasulfide, bis-[3-(triethoxysilyl)propyl]disulfide, γ-trimethoxysilylpropyldimethylthiocarbamoyltetrasulfide and γ-trimethoxysilylpropylbenzothiazolyltetrasulfide.

[0125] From the viewpoint of coating properties, the viscosity of the resin composition of the present embodiment at 25° C. is preferably 0.5 Pa·s to 10 Pa·s, more preferably 0.8 Pa·s to 9 Pa·s, and further preferably 1 Pa·s to 8 Pa·s. The viscosity of the resin composition at 25° C. can be measured using a B-type viscometer ("Digital Viscometer DV-II" manufactured by Brookfield) under the conditions of spindle No. 18 and a rotation speed of 10 rpm.

[0126] (optical fiber)

[0127] Figure 1 The optical fiber 10 includes a glass fiber 13 including a core 11 and a cladding 12 , and a coating resin layer 16 provided on the periphery of the glass fiber 13 and including a primary resin layer 14 and a secondary resin layer 15 .

[0128] The cladding 12 surrounds the core 11. The core 11 and the cladding 12 mainly include glass such as quartz glass. For example, the core 11 can use quartz glass doped with germanium or pure quartz glass, and the cladding 12 can use pure quartz glass or quartz glass doped with fluorine.

[0129] exist Figure 1For example, the outer diameter (D2) of the glass fiber 13 is about 100 μm to 125 μm, and the diameter (D1) of the core 11 constituting the glass fiber 13 is about 7 μm to 15 μm. The thickness of the coating resin layer 16 is generally about 22 μm to 70 μm. The thickness of each layer of the primary resin layer 14 and the secondary resin layer 15 can be about 5 μm to 50 μm.

[0130] When the outer diameter of the glass fiber 13 is about 125 μm and the thickness of the coating resin layer 16 is 60 μm to 70 μm, the thickness of each of the primary resin layer 14 and the secondary resin layer 15 can be about 10 μm to 50 μm, for example, the thickness of the primary resin layer 14 can be 35 μm, and the thickness of the secondary resin layer 15 can be 25 μm. The outer diameter of the optical fiber 10 can be about 245 μm to 265 μm.

[0131] When the outer diameter of the glass fiber 13 is about 125 μm and the thickness of the coating resin layer 16 is 24 μm to 48 μm, the thickness of each of the primary resin layer 14 and the secondary resin layer 15 can be about 8 μm to 38 μm, for example, the thickness of the primary resin layer 14 can be 25 μm, and the thickness of the secondary resin layer 15 can be 10 μm. The outer diameter of the optical fiber 10 can be about 173 μm to 221 μm.

[0132] When the outer diameter of the glass fiber 13 is about 100 μm and the thickness of the coating resin layer 16 is 22 μm to 37 μm, the thickness of each of the primary resin layer 14 and the secondary resin layer 15 can be about 5 μm to 32 μm, for example, the thickness of the primary resin layer 14 can be 25 μm, and the thickness of the secondary resin layer 15 can be 10 μm. The outer diameter of the optical fiber 10 can be about 144 μm to 174 μm.

[0133] By applying the resin composition according to the present embodiment to the primary resin layer, an optical fiber with excellent productivity can be produced.

[0134] The method for producing an optical fiber according to the present embodiment includes: a coating step of coating the resin composition on the outer circumference of a glass fiber including a core and a cladding; and a curing step of curing the resin composition by irradiating ultraviolet rays after the coating step.

[0135] From the viewpoint of improving the microbending resistance of the optical fiber, the Young's modulus of the primary resin layer is preferably 0.8 MPa or less, more preferably 0.5 MPa or less at 23°C ± 2°C. When the Young's modulus of the primary resin layer exceeds 0.8 MPa, external force is easily transmitted to the glass fiber, and the increase in transmission loss due to microbending may become greater.

[0136] The Young's modulus of the primary resin layer can be measured by the Pullout Modulus (POM) method at 23°C. Use two chuck devices to fix two locations of the optical fiber, remove the coating resin layer (primary resin layer and secondary resin layer) between the two chuck devices, then fix one chuck device and slowly move the other chuck device in the opposite direction to the fixed chuck device. Let the length of the portion of the optical fiber sandwiched between the moving chuck devices be L, the movement amount of the chuck be Z, the outer diameter of the primary resin layer be Dp, the outer diameter of the glass fiber be Df, the Poisson's ratio of the primary resin layer be n, and the load when the chuck device is moved be W. In this case, the Young's modulus of the primary resin layer can be calculated by the following formula.

[0137] Young's modulus (MPa) = ((1+n)W / πLZ) × ln(Dp / Df)

[0138] The secondary resin layer 15 can be formed, for example, by curing a resin composition containing a photopolymerizable compound including a carbamate (meth)acrylate, a photopolymerization initiator, and the like. The resin composition forming the secondary resin layer has a composition different from that of the resin composition for the primary coating. The resin composition for the secondary coating can be prepared using conventionally known techniques. The resin composition for the secondary coating can contain carbamate (meth)acrylamide, can contain carbamate (meth)acrylate, or can contain carbamate (meth)acrylamide and carbamate (meth)acrylate.

[0139] From the viewpoint of improving the microbending resistance of the optical fiber, the Young's modulus of the secondary resin layer is preferably 800 MPa or more, more preferably 1000 MPa or more, and further preferably 1200 MPa or more at 23°C±2°C. The upper limit of the Young's modulus of the secondary resin layer is not particularly limited, but from the viewpoint of imparting appropriate toughness to the secondary resin layer, it may be 3000 MPa or less, 2500 MPa or less, or 2000 MPa or less at 23°C±2°C.

[0140] The Young's modulus of the secondary resin layer can be measured by the following method. First, the optical fiber is immersed in a mixed solvent of acetone and ethanol, and only the coating resin layer is pulled out in a cylindrical shape. At this time, the primary resin layer and the secondary resin layer become one, but since the Young's modulus of the primary resin layer is more than 1 / 1000 and less than 1 / 10000 of the Young's modulus of the secondary resin layer, the Young's modulus of the primary resin layer can be ignored. Next, the solvent is removed from the coating resin layer by vacuum drying, and then a tensile test is performed at 23°C (tensile speed is 1 mm / min), and the Young's modulus can be calculated by the secant formula of 2.5% strain.

[0141] From the viewpoint of improving the heat resistance of the secondary resin layer, the Tg of the secondary resin layer is preferably 70°C or higher, more preferably 75°C or higher. From the viewpoint of suppressing an increase in the transmission loss of the optical fiber at low temperatures, it is preferably 105°C or lower, more preferably 95°C or lower.

[0142] In the method for producing an optical fiber according to the present embodiment, by using the resin composition according to the present embodiment as the resin composition for primary coating, an optical fiber with excellent productivity can be produced.

[0143] Example

[0144] Hereinafter, the present disclosure will be described in more detail by showing the evaluation test results using the examples and comparative examples related to the present disclosure. It should be noted that the present disclosure is not limited to these examples.

[0145] [Synthesis of carbamate acrylamide]

[0146] (A-1)

[0147] Polypropylene glycol (trade name "SANNIX PP-3000" manufactured by Sanyo Chemical Industries, Ltd.) with an Mn of 3000 was reacted with 2,4-toluene diisocyanate (TDI) at 60°C for 1 hour in a manner that the molar ratio of NCO to OH (NCO / OH) was 1.5 to prepare an NCO-terminated prepolymer. As a catalyst, 200 ppm of dibutyltin dilaurate was added relative to the final total amount added. Next, N-hydroxyethyl acrylamide (HEAA) was added in a manner that the molar ratio of OH of HEAA to NCO of the NCO-terminated prepolymer was 1.05, and the mixture was reacted at 60°C for 1 hour to obtain a urethane acrylamide (A-1) with an Mn of 11400.

[0148] (A-2)

[0149] PP-3000 and TDI were reacted at 60°C for 1 hour so that NCO / OH was 1.5 to prepare an NCO-terminated prepolymer. 200 ppm of dibutyltin dilaurate was added to the final total amount. Then, methanol was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.4, and HEAA was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.65, and the mixture was reacted at 60°C for 1 hour to obtain a urethane acrylamide (A-2) having an Mn of 11,300.

[0150] (A-3)

[0151] PP-3000 and TDI were reacted at 60°C for 1 hour so that NCO / OH was 1.5 to prepare an NCO-terminated prepolymer. 200 ppm of dibutyltin dilaurate was added relative to the final total amount. Next, 3-mercaptopropyltrimethoxysilane (MPTS) was added so that the molar ratio of SH to NCO of the NCO-terminated prepolymer was 0.1, and HEAA was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.95, and the mixture was reacted at 60°C for 1 hour to obtain a urethane acrylamide (A-3) having an Mn of 11400.

[0152] (A-4)

[0153] Polypropylene glycol (trade name "PP-4000" manufactured by Sanyo Chemical Industries, Ltd.) having an Mn of 4000 was reacted with TDI at 60°C for 1 hour so that NCO / OH was 1.5 to prepare an NCO-terminated prepolymer. 200 ppm of dibutyltin dilaurate was added relative to the final total amount added. Then, MPTS was added so that the molar ratio of SH to NCO of the NCO-terminated prepolymer was 0.05, methanol was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.2, and HEAA was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.8, and the reaction was carried out at 60°C for 1 hour to obtain a urethane acrylamide (A-4) having an Mn of 15900.

[0154] (A-5)

[0155] A polycarbonate diol having an Mn of 3000 (trade name "ETERNACOLL PH-300" manufactured by Ube Industries, Ltd.) was reacted with TDI at 60°C for 1 hour so that NCO / OH was 1.5, thereby preparing an NCO-terminated prepolymer. 200 ppm of dibutyltin dilaurate was added to the final total amount. Then, methanol was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.4, and HEAA was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.65, and the reaction was carried out at 60°C for 1 hour, thereby obtaining a urethane acrylamide (A-5) having an Mn of 11600.

[0156] (A-6)

[0157] Polytetramethylene glycol (trade name "PTG-L" manufactured by Hodogaya Chemical Industry Co., Ltd.) having an Mn of 3000 was reacted with TDI at 60°C for 1 hour so that NCO / OH was 1.5, thereby preparing an NCO-terminated prepolymer. 200 ppm of dibutyltin dilaurate was added relative to the final total amount added. Then, methanol was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.4, and HEAA was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.65, and the mixture was reacted at 60°C for 1 hour, thereby obtaining a urethane acrylamide (A-6) having an Mn of 11500.

[0158] (A-7)

[0159] A polypropylene glycol having an Mn of 12,000 (trade name "PREMINOL S4013F" manufactured by AGC Corporation) and TDI were reacted at 60°C for 1 hour so that NCO / OH was 2.0 to prepare an NCO-terminated prepolymer. 200 ppm of dibutyltin dilaurate was added relative to the final total amount added. Then, MPTS was added so that the molar ratio of SH to NCO of the NCO-terminated prepolymer was 0.05, methanol was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.2, and HEAA was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.8, and the reaction was carried out at 60°C for 1 hour to obtain a urethane acrylamide (A-7) having an Mn of 23,400.

[0160] (A-8)

[0161] Polypropylene glycol (trade name "PREMINOL S4318F" manufactured by AGC Corporation) having an Mn of 18,000 was reacted with TDI at 60°C for 1 hour so that NCO / OH was 2.0, thereby preparing an NCO-terminated prepolymer. 200 ppm of dibutyltin dilaurate was added to the final total amount. Next, HEAA was added so that the molar ratio of OH to NCO in the NCO-terminated prepolymer was 1.05, and the mixture was reacted at 60°C for 1 hour, thereby obtaining a urethane acrylamide (A-8) having an Mn of 36,500.

[0162] (B-1)

[0163] Polypropylene glycol (trade name "SANNIX PP-3000" manufactured by Sanyo Chemical Industries, Ltd.) with an Mn of 3000 was reacted with 2,4-toluene diisocyanate (TDI) at 60°C for 1 hour in a manner that the molar ratio of NCO to OH (NCO / OH) was 1.5, thereby preparing an NCO-terminated prepolymer. As a catalyst, 200 ppm of dibutyltin dilaurate was added relative to the final total amount added. Next, N-hydroxyethyl acrylamide (HEAA) was added in a manner that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.9, and 2-hydroxyethyl acrylate (HEA) was added in a manner that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.15, and the reaction was carried out at 60°C for 1 hour, thereby obtaining a urethane acrylamide (B-1) with an Mn of 11400.

[0164] (B-2)

[0165] PP-3000 and TDI were reacted at 60°C for 1 hour so that NCO / OH was 1.5 to prepare an NCO-terminated prepolymer. As a catalyst, 200 ppm of dibutyltin dilaurate was added relative to the final total amount. Next, HEAA was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.3, and HEA was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.75, and the reaction was carried out at 60°C for 1 hour to obtain a urethane acrylamide (B-2) with an Mn of 11400.

[0166] (B-3)

[0167] PP-3000 and TDI were reacted at 60°C for 1 hour so that NCO / OH was 1.5 to prepare an NCO-terminated prepolymer. As a catalyst, 200 ppm of dibutyltin dilaurate was added relative to the final total amount. Next, HEAA was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.5, HEA was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.15, and methanol was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.4, and the reaction was carried out at 60°C for 1 hour to obtain a urethane acrylamide (B-3) with an Mn of 11300.

[0168] (B-4)

[0169] Polypropylene glycol (trade name "SANNIX PP-4000" manufactured by Sanyo Chemical Industries, Ltd.) having an Mn of 4000 was reacted with TDI at 60°C for 1 hour so that NCO / OH was 1.5, thereby preparing an NCO-terminated prepolymer. As a catalyst, 200 ppm of dibutyltin dilaurate was added relative to the final total amount. Next, HEAA was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.6, HEA was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.2, methanol was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.2, and 3-mercaptopropyltrimethoxysilane (MPTS) was added so that the molar ratio of SH to NCO of the NCO-terminated prepolymer was 0.05, and the reaction was carried out at 60°C for 1 hour to obtain a urethane acrylamide (B-4) having an Mn of 15900.

[0170] (B-5)

[0171] A polycarbonate diol having an Mn of 3000 (trade name "ETERCOLL PH-300" manufactured by Ube Industries, Ltd.) was reacted with TDI at 60°C for 1 hour so that NCO / OH was 1.5, thereby preparing an NCO-terminated prepolymer. As a catalyst, 200 ppm of dibutyltin dilaurate was added relative to the final total amount. Next, HEAA was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.5, HEA was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.15, and methanol was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.4, and the reaction was carried out at 60°C for 1 hour, thereby obtaining a urethane acrylamide (B-5) having an Mn of 11500.

[0172] (B-6)

[0173] Polytetramethylene glycol (trade name "PTG-L" manufactured by Hodogaya Chemical Industry Co., Ltd.) having an Mn of 3000 was reacted with TDI at 60°C for 1 hour so that NCO / OH was 1.5, thereby preparing an NCO-terminated prepolymer. As a catalyst, 200 ppm of dibutyltin dilaurate was added relative to the final total amount added. Next, HEAA was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.5, HEA was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.15, and methanol was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.4, and the reaction was carried out at 60°C for 1 hour, thereby obtaining a urethane acrylamide (B-6) having an Mn of 11500.

[0174] (B-7)

[0175] Polypropylene glycol (trade name "PREMINOL S4013F" manufactured by AGC Corporation) having an Mn of 12,000 was reacted with TDI at 60°C for 1 hour so that NCO / OH was 2.0, thereby preparing an NCO-terminated prepolymer. As a catalyst, 200 ppm of dibutyltin dilaurate was added relative to the final total amount. Next, HEAA was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.6, HEA was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.2, methanol was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.2, and 3-mercaptopropyltrimethoxysilane was added so that the molar ratio of SH to NCO of the NCO-terminated prepolymer was 0.05, and the reaction was carried out at 60°C for 1 hour to obtain a urethane acrylamide (B-7) having an Mn of 23,300.

[0176] (B-8)

[0177] A polypropylene glycol having an Mn of 18,000 (trade name "PREMINOL S4318F" manufactured by AGC Corporation) and TDI were reacted at 60°C for 1 hour so that NCO / OH was 2.0 to prepare an NCO-terminated prepolymer. As a catalyst, 200 ppm of dibutyltin dilaurate was added relative to the final total amount. Next, HEAA was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.6, HEA was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.2, and 3-mercaptopropyltrimethoxysilane was added so that the molar ratio of SH to NCO of the NCO-terminated prepolymer was 0.25, and the reaction was carried out at 60°C for 1 hour to obtain a urethane acrylamide (B-8) having an Mn of 36,600.

[0178] [Synthesis of urethane acrylate]

[0179] (Y-1)

[0180] PP-3000 and TDI were reacted at 60°C for 1 hour so that NCO / OH was 1.5 to prepare an NCO-terminated prepolymer. 200 ppm of dibutyltin dilaurate was added to the final total amount. Next, HEA was added so that the molar ratio of OH to NCO in the NCO-terminated prepolymer was 1.05, and the mixture was reacted at 60°C for 1 hour to obtain a urethane acrylate (Y-1) having an Mn of 11,300.

[0181] (Y-2)

[0182] PP-3000 and TDI were reacted at 60°C for 1 hour so that NCO / OH was 1.5 to prepare an NCO-terminated prepolymer. 200 ppm of dibutyltin dilaurate was added to the final total amount. Then, methanol was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.4, and HEA was added so that the molar ratio of OH to NCO of the NCO-terminated prepolymer was 0.65, and the mixture was reacted at 60°C for 1 hour to obtain a urethane acrylate (Y-2) having an Mn of 11200.

[0183] (Z-1)

[0184] Urethane acrylate (Z-1) having an Mn of 2200 was obtained in the same manner as in the synthesis of (Y-1), except that a polypropylene glycol having an Mn of 600 (trade name "PP-600" manufactured by Sanyo Chemical Industries, Ltd.) was reacted with TDI so that NCO / OH was 2.0 to prepare an NCO-terminated prepolymer.

[0185] The Mn of polyol is the value listed in the catalog of each product. The Mn of urethane acrylamide and urethane acrylate were measured using the ACQUITY APC RI system manufactured by Waters under the following conditions: sample concentration: 0.2 mass % THF solution, injection volume: 20 μL, sample temperature: 15°C, mobile phase: THF, XT column for organic solvent: particle size 2.5 μm, pore size Column inner diameter 4.6 × column length 150mm + particle size 2.5μm, pore size Column inner diameter 4.6 × column length 150mm + particle size 1.7μm, pore size Column inner diameter: 4.6×column length: 150 mm, column temperature: 40° C., flow rate: 0.8 mL / min.

[0186] As photopolymerizable compounds, nonylphenol polyethylene glycol acrylate (trade name "ARONIX M-113" manufactured by Toagosei Co., Ltd.), 2-(2-ethoxyethoxy)ethyl acrylate (EOEOEA), trimethylolpropane triacrylate (TMPTA), N-vinyl caprolactam (NVCL), acryloyl morpholine (ACMO), bisphenol A epoxy di(meth)acrylate (trade name "Viscoat#540" manufactured by Osaka Organic Chemical Industry Co., Ltd.), and tripropylene glycol diacrylate (TPGDA) were prepared. As photopolymerization initiators, 2,4,6-trimethylbenzoyldiphenylphosphine oxide (Omnirad TPO) and 1-hydroxycyclohexyl phenyl ketone (Omnirad 184) were prepared. As a silane coupling agent, 3-acryloxypropyltrimethoxysilane (APTMS) was prepared.

[0187] [Resin composition for primary coating]

[0188] The photopolymerizable compound, the photopolymerization initiator, and the silane coupling agent were mixed in the amounts (parts by mass) shown in Table 1, Table 2, or Table 3 to prepare the primary coating resin composition of each Example and Comparative Example.

[0189] [Resin composition for secondary coating]

[0190] 25 parts by mass of urethane acrylate (Z-1), 36 parts by mass of TPGTA, 37 parts by mass of Viscoat #540, 1 part by mass of Omnirad TPO, and 1 part by mass of Omnirad 184 were mixed to obtain a resin composition for secondary coating.

[0191] [Fabrication of optical fiber]

[0192] The resin composition for primary coating and the resin composition for secondary coating were applied to the outer peripheral surface of a glass fiber 13 having a diameter of 125 μm, respectively. Then, each resin composition was cured by irradiating ultraviolet rays to form a coating resin layer 16 having a primary resin layer 14 and a secondary resin layer 15, thereby manufacturing an optical fiber 10. The thickness of the primary resin layer 14 was set to 35 μm, and the thickness of the secondary resin layer 15 was set to 25 μm. The line speed was changed to 2500 m / min, 3000 m / min, and 3500 m / min, and optical fibers were manufactured respectively.

[0193] (Young's modulus of primary resin layer)

[0194] The Young's modulus of the primary resin layer was measured by a Pullout Modulus (POM) method at 23°C.

[0195] (Gel fraction)

[0196] The optical fiber was immersed in methyl ethyl ketone at 60°C for 12 hours to extract the uncured components in the coating resin layer. After the optical fiber was taken out, the methyl ethyl ketone was removed by a vacuum dryer, and the gel fraction was calculated according to the following formula.

[0197] Gel fraction [%] = (mass of optical fiber after extraction - mass of glass fiber) / (mass of optical fiber before extraction - mass of glass fiber) × 100

[0198] Although the uncured components in the primary resin layer and the secondary resin layer were extracted, the curability of the primary resin layer could be compared because the secondary resin layer used the same resin composition. The case where the gel fraction exceeded 80% was evaluated as "A", the case where the gel fraction was 70% to 80% was evaluated as "B", and the case where the gel fraction was less than 70% was evaluated as "C".

[0199] (low temperature characteristics)

[0200] A layer of optical fiber was wound on a glass bobbin with a tension of 50g, and the transmission characteristics of the signal light at a wavelength of 1550nm were measured at respective temperature conditions of 23°C and -40°C to obtain the transmission losses at 23°C and -40°C. The case where the transmission loss difference of the transmission loss at 23°C minus the transmission loss at -40°C was less than 0dB was evaluated as "A", the case where it was more than 0dB and less than 0.01dB / km was evaluated as "B", and the case where it exceeded 0.01dB / km was evaluated as "C".

[0201] [Table 1]

[0202]

[0203] [Table 2]

[0204]

[0205] [Table 3]

[0206]

[0207] Explanation of symbols

[0208] 10. Fiber Optics

[0209] 11 Core

[0210] 12 Cladding

[0211] 13 Fiberglass

[0212] 14 Primary resin layer

[0213] 15 Secondary resin layer

[0214] 16 Coating resin layer

Claims

1. A resin composition for primary coating of an optical fiber, comprising: A photopolymerizable compound comprising urethane (meth) acrylamide and a photopolymerization initiator, The carbamate (meth)acrylamide has a (meth)acrylamide group at at least one end of the carbamate bond, The urethane (meth)acrylamide includes: a urethane oligomer having (meth)acrylamide groups at both ends of a urethane bond; and a urethane oligomer having a (meth)acrylamide group at one end of a urethane bond and a group based on a silane compound containing active hydrogen at the other end.

2. The resin composition according to claim 1, in, The content of the urethane (meth)acrylamide is 10 parts by mass or more and 90 parts by mass or less based on 100 parts by mass of the total amount of the resin composition.

3. The resin composition according to claim 1 or claim 2, in, The number average molecular weight of the urethane (meth)acrylamide is 10,000 to 37,000.

4. The resin composition according to claim 1 or claim 2, in, The photopolymerizable compound further includes a (meth)acrylate.

5. The resin composition according to claim 1 or claim 2, in, The photopolymerizable compound further includes an N-vinyl compound.

6. The resin composition according to claim 1 or claim 2, in, The photopolymerizable compound further includes a (meth)acrylamide compound.

7. An optical fiber having: Glass fiber with core and cladding, a primary resin layer in contact with the glass fiber and covering the glass fiber, and a secondary resin layer covering the primary resin layer, The primary resin layer comprises a cured product of the resin composition according to any one of claims 1 to 6 .

8. A method for manufacturing an optical fiber, include: A coating step of coating the resin composition according to any one of claims 1 to 6 on the outer periphery of a glass fiber having a core and a cladding; as well as After the coating step, a curing step is performed to cure the resin composition by irradiating ultraviolet rays.

Citation Information

Patent Citations

  • Liquid curable resin composition

    JP2009197163A

  • Radiation-curable resin composition

    JP2012111674A

  • D1368 cr radiation-curable primary coating for optical fiber

    JP2013136783A

  • Radiation-curable coating material for D1452GB optical fiber

    JP2013501125A

  • D1378 ca radiation-curable primary coating for optical fiber

    JP2014114208A