A bone and joint biological lubricant and its preparation method and application

By introducing propane sultone and catechol-modified chitosan derivatives into bone and joint lubricants, the problems of insufficient lubricant adsorption and active oxygen scavenging functions are solved, and strong interfacial adhesion and excellent lubrication are achieved. Performance, significantly improves symptoms of osteoarthritis.

CN116350861BActive Publication Date: 2024-10-22YANTAI BORUN NEW MATERIAL TECH PARTNERSHIP (LLP)
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310511791.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-09
Publication Date
2024-10-22
Estimated Expiration
2043-05-09

AI Technical Summary

Technical Problem

Existing bone and joint lubricants are difficult to adsorb on the cartilage surface, have a single function, and cannot effectively remove active oxygen free radicals in the joint cavity, leading to the worsening of osteoarthritis.

Method used

Propane sultone and catechol-modified chitosan derivatives are used as bone and joint biolubricants. The interfacial adhesion and active oxygen free radical scavenging function of the lubricant are improved through grafting reaction. Combined with a good solvent, a lubricant with excellent properties is prepared. A new biological lubricant with excellent lubrication performance and active oxygen scavenging ability.

Benefits of technology

This biological lubricant can effectively adsorb on the cartilage surface, reduce the friction coefficient, significantly remove active oxygen free radicals in the joints, reduce inflammation, protect articular cartilage, and significantly improve the symptoms of osteoarthritis.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116350861B_ABST
    Figure CN116350861B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of biomedical technology, and provides a bone and joint biological lubricant, a preparation method and application thereof. The present invention uses natural macromolecular chitosan as the main chain, grafts propane sultone small molecules with good hydrophilicity and lubrication properties and catechol groups with adhesion and active oxygen free radical scavenging functions onto the chitosan side chain to obtain a chitosan derivative; the chitosan derivative is dissolved in a good solvent to obtain a novel bone and joint biological lubricant, which has good biocompatibility, strong interface adhesion, excellent water lubrication performance, and active oxygen free radical scavenging function, and has broad application prospects in the treatment of osteoarthritis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of biomedical technology, and in particular to a bone and joint biological lubricant, a preparation method and application thereof. Background Art

[0002] Biolubricants have the advantage of reducing friction between tissue interfaces and have been widely used in the medical field, such as treating dry eyes, preventing postoperative tissue adhesion, and relieving osteoarthritis. Osteoarthritis is a cartilage degenerative disease, and its typical feature is the increased friction and wear between the cartilage contact surfaces, resulting in the formation of chondrocyte fragments, which in turn leads to a significant increase in the concentration of reactive oxygen free radicals in the joint cavity. At present, the main method to improve the lubrication performance between osteoarthritis cartilage is to inject exogenous lubricants, such as hyaluronic acid, chitosan, etc., into the joint cavity. However, these lubricants are difficult to adsorb on the cartilage interface, and are easily squeezed out of the joint cavity when the cartilage contacts, requiring frequent injections to achieve the effect of lubricating the joint. At the same time, these lubricants often only have a lubricating function, and do not have a good scavenging function for the excessive reactive oxygen free radicals produced in the joint cavity caused by osteoarthritis. Under normal circumstances, excessive reactive oxygen free radicals will cause inflammation in the joint cavity and damage the articular cartilage. Cartilage damage further causes the formation of chondrocyte fragments, which in turn leads to an increase in the concentration of reactive oxygen free radicals in the joint cavity. This vicious cycle is the key to exacerbating the development of osteoarthritis.

[0003] Therefore, in view of the shortcomings of current lubricants for the treatment of osteoarthritis, such as difficulty in adsorbing on the cartilage surface and single function, it is urgent to invent a new type of biological lubricant with strong interfacial adhesion, excellent water lubrication performance and active oxygen free radical scavenging function. Summary of the invention

[0004] In view of this, the present invention provides a bone and joint biological lubricant and a preparation method and application thereof. The bone and joint biological lubricant provided by the present invention has strong interface adhesion, excellent water lubrication performance, and has the function of scavenging active oxygen free radicals.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] A bone and joint biological lubricant comprises propane sultone and catechol-modified chitosan derivatives and a good solvent; the structural formula of the propane sultone and catechol-modified chitosan derivatives is shown in Formula I:

[0007]

[0008] In formula I: X+Y+Z=0.9, X is 0.3-0.6, Y is 0.1-0.4, and Z is 0.2-0.5.

[0009] Preferably, the method for preparing the propane sultone and catechol modified chitosan derivative comprises the following steps:

[0010] The chitosan solution and propane sultone are mixed to carry out a first grafting reaction to obtain propane sultone-modified chitosan;

[0011] 3,4-dihydroxyphenylpropionic acid, water, ethyl (3-(dimethylamino)propyl) carbodiimide hydrochloride and methoxy polyethylene glycol succinimide ester are mixed for activation reaction, and the obtained activation reaction solution and the propane sultone modified chitosan are mixed for a second grafting reaction to obtain propane sultone and catechol modified chitosan derivatives.

[0012] Preferably, the preparation method of the chitosan solution comprises: dispersing chitosan in water, then adding acetic acid solution to adjust the pH value to 4-6 to obtain the chitosan solution; the molecular weight of the chitosan is 100,000-1,000,000, and the viscosity is 10-200 mPa.s.

[0013] Preferably, the mass ratio of propane sultone to chitosan is 1:(1-5);

[0014] The first grafting reaction takes 4 to 24 hours and the reaction temperature is 50 to 100°C.

[0015] Preferably, the mass ratio of 3,4-dihydroxybenzenepropionic acid, ethyl (3-(dimethylamino)propyl) carbodiimide hydrochloride and methoxy polyethylene glycol succinimide ester is (1-10):(1-10):(1-20); the temperature of the activation reaction is 10-50°C, and the reaction time is 0.5-6h.

[0016] Preferably, the mass ratio of the propane sultone-modified chitosan to 3,4-dihydroxyphenylpropionic acid is 1:(1-10); the temperature of the second grafting reaction is 10-50° C., and the reaction time is 6-36 hours.

[0017] Preferably, after the first grafting reaction is completed, the method further comprises washing, dialyzing and freeze-drying the obtained solid product in sequence; and after the second grafting reaction is completed, the method further comprises dialyzing and freeze-drying the obtained product liquid in sequence.

[0018] Preferably, the good solvent includes one or more of deionized water, phosphate buffered saline and physiological saline.

[0019] Preferably, the concentration of propane sultone and catechol-modified chitosan derivative in the bone and joint biological lubricant is 0.1-20 mg / mL.

[0020] The present invention also provides a method for preparing the bone and joint biological lubricant described in the above scheme, comprising the following steps: dissolving the propane sultone and the catechol-modified chitosan derivative in the good solvent to obtain the bone and joint biological lubricant.

[0021] The present invention also provides the use of the bone and joint biological lubricant described in the above scheme or the bone and joint biological lubricant prepared by the preparation method described in the above scheme in the preparation of drugs for treating osteoarthritis.

[0022] The present invention provides a bone and joint biological lubricant, including propane sultone and catechol modified chitosan derivatives and a good solvent. The present invention selects natural polysaccharide chitosan as the central skeleton of the lubricant macromolecule, and grafts the propane sultone small molecule with good hydrophilicity and lubrication performance and the catechol group with adhesion and active oxygen free radical scavenging function onto the chitosan side chain. The obtained chitosan derivative has a strong affinity with articular cartilage, can be better adsorbed on the surface of articular cartilage to form a firm lubricating film, and effectively reduce the friction coefficient of the cartilage surface. At the same time, since the catechol group adhering to the surface of the cartilage has an excellent active oxygen free radical scavenging function, it can effectively remove the active oxygen free radicals in the joint cavity, significantly reduce the inflammation level in the joint, and thus play a protective role on the articular cartilage; in summary, the bone and joint biological lubricant provided by the present invention has good biocompatibility, strong interface adhesion, excellent water lubrication performance, and active oxygen free radical scavenging function, and has broad application prospects in the treatment of osteoarthritis. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 is the CS-PS-DA obtained in Example 5 1 H NMR spectroscopy;

[0024] Figure 2 The friction test results of NS, CS-PS lubricants and CS-PS-DA lubricants are shown;

[0025] Figure 3 is the scavenging efficiency of CS-PS lubricant and CS-PS-DA lubricant on hydroxyl radicals (·OH);

[0026] Figure 4 The CS-PS lubricant and CS-PS-DA lubricant react with oxygen anion free radicals (·O2 - ) removal efficiency;

[0027] Figure 5 The therapeutic effects of normal saline, CS-PS lubricant and CS-PS-DA lubricant on rats with osteoarthritis. DETAILED DESCRIPTION

[0028] The present invention provides a bone and joint biological lubricant, comprising propane sultone and catechol-modified chitosan derivatives and a good solvent; the structural formula of the propane sultone and catechol-modified chitosan derivatives is shown in Formula I:

[0029]

[0030] In formula I: X+Y+Z=0.9, X is 0.3-0.6, Y is 0.1-0.4, and Z is 0.2-0.5.

[0031] The deacetylation degree of the chitosan molecule used in the present invention is 90%, that is, X+Y+Z=0.9, wherein X represents the ratio of the chitosan units used for grafting with catechol groups to the total chitosan units, Y represents the ratio of the chitosan units used for grafting with propane sultone to the total chitosan units, and Z represents the ratio of the ungrafted chitosan units to the total chitosan units.

[0032] In the present invention, X is preferably 0.4 to 0.5, Y is preferably 0.2 to 0.3, and Z is preferably 0.3 to 0.4.

[0033] In the present invention, the preparation method of the propane sultone and catechol modified chitosan derivative comprises the following steps:

[0034] The chitosan solution and propane sultone are mixed to carry out a first grafting reaction to obtain propane sultone-modified chitosan;

[0035] 3,4-dihydroxyphenylpropionic acid, water, ethyl (3-(dimethylamino)propyl) carbodiimide hydrochloride and methoxy polyethylene glycol succinimide ester are mixed for activation reaction, and the obtained activation reaction solution and the propane sultone modified chitosan are mixed for a second grafting reaction to obtain propane sultone and catechol modified chitosan derivatives.

[0036] In the present invention, the reaction formula of the first grafting reaction and the second grafting reaction is shown in Formula II, which is described in detail below in conjunction with Formula II.

[0037]

[0038] In formula II: CS is chitosan, PS is propane sultone, and DA is 3,4-dihydroxyphenylpropionic acid.

[0039] The present invention mixes chitosan solution and propane sultone to carry out a first grafting reaction to obtain propane sultone modified chitosan (denoted as CS-PS). In the present invention, the preparation method of the chitosan solution preferably includes: dispersing chitosan in water, then adding acetic acid solution to adjust the pH value to 4-6 to obtain the chitosan solution. In the present invention, the molecular weight of the chitosan is preferably 100,000 to 1,000,000, more preferably 400,000 to 500,000, the viscosity of the chitosan is preferably 10 to 200 mPa.s, more preferably 50 to 150 mPa.s; the deacetylation degree of the chitosan is preferably 90%; the dosage ratio of the chitosan to water is preferably 1 g:100 mL, and the water is preferably deionized water; the concentration of the acetic acid solution is preferably 0.5 to 2 wt%, more preferably 1 to 1.5 wt%, and the pH value of the acetic acid solution is preferably 1 to 6, more preferably 2 to 5; in the present invention, after adding the acetic acid solution, the system is preferably stirred sufficiently to completely dissolve the chitosan.

[0040] In the present invention, the mass ratio of propane sultone to chitosan is 1:(1-5), more preferably 1:(2-4); the temperature of the first grafting reaction is preferably 50-100°C, more preferably 60-80°C, and the time of the first grafting reaction is preferably 4-24h, more preferably 6-20h.

[0041] After the first grafting reaction is completed, the present invention also preferably includes washing, dialyzing and freeze-drying the obtained solid product in sequence to obtain propane sultone modified chitosan. The present invention preferably filters the product liquid obtained from the first grafting reaction to obtain a solid product; the washing is preferably three times in acetone and methanol respectively; the dialysis solvent is preferably deionized water, the molecular weight cutoff of the dialysis bag is preferably 1000 to 10000 kDa, and the dialysis time is preferably 2 to 7 days; the freeze drying temperature is preferably -20 to -50°C, and the freeze drying time is preferably 12 to 36 hours.

[0042] After obtaining the propane sultone-modified chitosan, the present invention mixes 3,4-dihydroxyphenylpropionic acid, water, ethyl (3-(dimethylamino)propyl) carbodiimide hydrochloride (EDC·HCl) and methoxy polyethylene glycol succinimide ester (NHS) to carry out an activation reaction, and mixes the obtained activation reaction liquid with the propane sultone-modified chitosan to carry out a second grafting reaction to obtain a propane sultone and catechol-modified chitosan derivative (referred to as CS-PS-DA). In the present invention, the mass ratio of the 3,4-dihydroxybenzenepropionic acid, ethyl (3-(dimethylamino)propyl) carbodiimide hydrochloride and methoxy polyethylene glycol succinimide ester is preferably (1-10):(1-10):(1-20), more preferably (1-7):(1-7):(2-16), more preferably 1:1.5:2; the amount ratio of the 3,4-dihydroxybenzenepropionic acid and water is preferably 0.1 g:20 mL; the temperature of the activation reaction is preferably 10-50°C, more preferably 20-30°C. In a specific embodiment of the present invention, the activation reaction is preferably carried out directly at room temperature without additional heating or cooling. The activation reaction time is preferably 0.5-6 h, more preferably 1-5 h; the activation reaction is preferably carried out under nitrogen protection.

[0043] In the present invention, the mass ratio of the propane sultone modified chitosan and 3,4-dihydroxyphenylpropionic acid is 1:(1-10), more preferably 1:(1-8), and further preferably 1:(1-5); the temperature of the second grafting reaction is preferably 10-50°C, more preferably 20-30°C. In a specific embodiment of the present invention, the second grafting reaction is preferably carried out directly at room temperature without additional heating or cooling. The time of the second grafting reaction is preferably 6-36h, more preferably 12-24h; the second grafting reaction is preferably carried out under nitrogen protection.

[0044] After the second grafting reaction is completed, the present invention preferably also includes dialyzing and freeze-drying the resulting product solution in sequence; the dialysis solvent is preferably deionized water, the molecular weight cutoff of the dialysis bag is preferably 2000-5000 kDa, the dialysis time is preferably 2-5 days, more preferably 3 days; the freeze-drying temperature is preferably -20 to -50°C, and the freeze-drying time is preferably 12 to 36 hours.

[0045] In the present invention, the good solvent preferably includes one or more of deionized water, phosphate buffered saline (PBS) and normal saline (NS); the pH value of the phosphate buffer solution is preferably 6.8-7.5; the concentration of propane sultone and catechol-modified chitosan derivatives in the bone and joint biological lubricant is preferably 0.1-20 mg / mL, more preferably 5-15 mg / mL, and further preferably 10 mg / mL.

[0046] The present invention also provides a method for preparing the bone and joint biological lubricant of the above scheme, comprising the following steps: dissolving the propane sultone and the catechol-modified chitosan derivative in the good solvent to obtain the bone and joint biological lubricant. The present invention has no special requirements for the specific conditions of the dissolution, and stirring at room temperature until completely dissolved is sufficient.

[0047] The present invention also provides the use of the bone and joint biological lubricant described in the above scheme or the bone and joint biological lubricant prepared by the preparation method described in the above scheme in the preparation of a drug for treating osteoarthritis. The bone and joint biological lubricant provided by the present invention has good biocompatibility, strong interface adhesion, excellent water lubrication performance, and active oxygen free radical scavenging function, and has broad application prospects in the treatment of osteoarthritis.

[0048] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0049] Example 1

[0050] Weigh 1.0g chitosan (molecular weight of 500,000, viscosity of 100mPa.s, degree of deacetylation of 90%) and disperse it in 100mL deionized water, then add 100mL 1% acetic acid solution and stir thoroughly for 1h to dissolve the chitosan. Add 0.5g propane sultone to the chitosan solution and react at 80℃ for 12h. After the reaction, the product is washed three times in acetone and methanol solution respectively. The washed product is dissolved in 100mL deionized water and then dialyzed in deionized water for 3 days to remove impurities. After dialysis, freeze-dry to obtain chitosan modified with propane sultone (CS-PS).

[0051] 0.1 g of 3,4-dihydroxyphenylpropionic acid, 0.15 g of ethyl (3-(dimethylamino)propyl) carbodiimide hydrochloride, and 0.2 g of N-hydroxysuccinimide were dissolved in 20 mL of deionized water and reacted at room temperature for 2 h under nitrogen protection. Subsequently, 0.1 g of propane sultone-modified chitosan was added to the reaction solution, and the reaction continued at room temperature for 12 h under nitrogen protection. After the reaction, the resulting solution was dialyzed in deionized water for 3 days to remove impurities, and finally freeze-dried to obtain a propane sultone and catechol-modified chitosan derivative (CS-PS-DA). CS-PS-DA was dissolved in NS to prepare a solution with a concentration of 10 mg / mL to obtain a CS-PS-DA lubricant.

[0052] Example 2

[0053] Weigh 1.0g chitosan (molecular weight of 500,000, viscosity of 100mPa.s, degree of deacetylation of 90%) and disperse it in 100mL deionized water, then add 100mL 1% acetic acid solution and stir thoroughly for 1h to dissolve the chitosan. Add 1.0g propane sultone to the chitosan solution and react at 80℃ for 12h. After the reaction, the product is washed three times in acetone and methanol solution respectively. The washed product is dissolved in 100mL deionized water and then dialyzed in deionized water for 3 days to remove impurities. After dialysis, freeze-dry to obtain chitosan modified with propane sultone (CS-PS).

[0054] 0.1 g of 3,4-dihydroxyphenylpropionic acid, 0.15 g of ethyl (3-(dimethylamino)propyl) carbodiimide hydrochloride, and 0.2 g of N-hydroxysuccinimide were dissolved in 20 mL of deionized water and reacted at room temperature for 2 h under nitrogen protection. Subsequently, 0.1 g of propane sultone-modified chitosan was added to the reaction solution and continued to react at room temperature for 12 h under nitrogen protection. After the reaction, the resulting solution was dialyzed in deionized water for 3 days to remove impurities, and finally freeze-dried to obtain a propane sultone and catechol-modified chitosan derivative (CS-PS-DA). CS-PS-DA was dissolved in NS to prepare a solution with a concentration of 10 mg / mL to obtain a CS-PS-DA lubricant.

[0055] Example 3

[0056] Weigh 1.0g chitosan (molecular weight of 500,000, viscosity of 100mPa.s, degree of deacetylation of 90%) and disperse it in 100mL deionized water, then add 100mL 1% acetic acid solution and stir thoroughly for 1h to dissolve the chitosan. Add 1.0g propane sultone to the chitosan solution and react at 80℃ for 12h. After the reaction, the product is washed three times in acetone and methanol solution respectively. The washed product is dissolved in 100mL deionized water and then dialyzed in deionized water for 3 days to remove impurities. After dialysis, freeze-dry to obtain chitosan modified with propane sultone (CS-PS).

[0057] 0.2 g of 3,4-dihydroxyphenylpropionic acid, 0.3 g of ethyl (3-(dimethylamino)propyl) carbodiimide hydrochloride, and 0.4 g of N-hydroxysuccinimide were dissolved in 20 mL of deionized water and reacted at room temperature for 2 h under nitrogen protection. Subsequently, 0.1 g of propane sultone-modified chitosan was added to the reaction solution and continued to react at room temperature for 12 h under nitrogen protection. After the reaction, the resulting solution was dialyzed in deionized water for 3 days to remove impurities, and finally freeze-dried to obtain a propane sultone and catechol-modified chitosan derivative (CS-PS-DA). CS-PS-DA was dissolved in NS to prepare a solution with a concentration of 10 mg / mL to obtain a CS-PS-DA lubricant.

[0058] Example 4

[0059] Weigh 1.0g chitosan (molecular weight of 500,000, viscosity of 100mPa.s, degree of deacetylation of 90%) and disperse it in 100mL deionized water, then add 100mL 1% acetic acid solution and stir thoroughly for 1h to dissolve the chitosan. Add 1.0g propane sultone to the chitosan solution and react at 80℃ for 12h. After the reaction, the product is washed three times in acetone and methanol solution respectively. The washed product is dissolved in 100mL deionized water and then dialyzed in deionized water for 3 days to remove impurities. After dialysis, freeze-dry to obtain chitosan modified with propane sultone (CS-PS).

[0060] 0.3 g of 3,4-dihydroxyphenylpropionic acid, 0.45 g of ethyl (3-(dimethylamino)propyl) carbodiimide hydrochloride, and 0.6 g of N-hydroxysuccinimide were weighed and dissolved in 20 mL of deionized water, and reacted at room temperature for 2 h under nitrogen protection. Subsequently, 0.1 g of propane sultone-modified chitosan was added to the reaction solution and continued to react at room temperature for 12 h under nitrogen protection. After the reaction, the resulting solution was dialyzed in deionized water for 3 days to remove impurities, and finally freeze-dried to obtain a propane sultone and catechol-modified chitosan derivative (CS-PS-DA). CS-PS-DA was dissolved in NS to prepare a solution with a concentration of 10 mg / mL to obtain a CS-PS-DA lubricant.

[0061] Example 5

[0062] Weigh 1.0g chitosan (molecular weight of 500,000, viscosity of 100mPa.s, degree of deacetylation of 90%) and disperse it in 100mL deionized water, then add 100mL 1% acetic acid solution and stir thoroughly for 1h to dissolve the chitosan. Add 1.0g propane sultone to the chitosan solution and react at 80℃ for 12h. After the reaction, the product is washed three times in acetone and methanol solution respectively. The washed product is dissolved in 100mL deionized water and then dialyzed in deionized water for 3 days to remove impurities. After dialysis, freeze-dry to obtain chitosan modified with propane sultone (CS-PS).

[0063] 0.5 g of 3,4-dihydroxyphenylpropionic acid, 0.75 g of ethyl (3-(dimethylamino)propyl) carbodiimide hydrochloride, and 1.0 g of N-hydroxysuccinimide were dissolved in 20 mL of deionized water and reacted at room temperature for 2 h under nitrogen protection. Subsequently, 0.1 g of propane sultone-modified chitosan was added to the reaction solution and continued to react at room temperature for 12 h under nitrogen protection. After the reaction, the resulting solution was dialyzed in deionized water for 3 days to remove impurities, and finally freeze-dried to obtain a propane sultone and catechol-modified chitosan derivative (CS-PS-DA). CS-PS-DA was dissolved in NS to prepare a solution with a concentration of 10 mg / mL to obtain a CS-PS-DA lubricant.

[0064] Figure 1 is the CS-PS-DA obtained in Example 5 1 H NMR spectrum. Figure 2 It can be confirmed that the obtained product has the target structure.

[0065] Example 6 Evaluation of the tribological properties of lubricants

[0066] The CS-PS-DA lubricant (10 mg / mL), normal saline (NS) and propane sultone-modified chitosan lubricant (CS-PS lubricant) (10 mg / mL) prepared in Example 5 were used as test samples for tribological testing. The preparation method of the propane sultone-modified chitosan solution is as follows: the propane sultone-modified chitosan prepared in Example 5 is dissolved in normal saline to prepare a 10 mg / mL solution. The CS-PS lubricants used in the subsequent examples are the same as those here, and will not be described in detail later.

[0067] The tribological test was conducted using TRB (CSM, Anton Paar). The test conditions were as follows: load: 1 N and 2 N, temperature 25 °C, frequency 1 Hz, amplitude 5 mm, test time 0.5 h, the friction test counterpart and substrate were both fresh bovine cartilage, the counterpart size was 7 mm × 5 mm, and the substrate size was 15 mm × 8 mm.

[0068] Friction test results are as follows Figure 2 As shown. Figure 2 It can be seen from the results that CS-PS-DA lubricant exhibits better lubrication performance than NS and CS-PS, with the friction coefficient as low as 0.025 under a load of 1N and as low as 0.024 under a load of 2N.

[0069] Example 7 Hydroxyl Radical Scavenging (·OH) Ability Test

[0070] The hydroxyl radical scavenging kit was purchased from Shanghai Youxuan Biotechnology Co., Ltd. 200 μL of CS-PS lubricant (10 mg / mL) and CS-PS-DA lubricant (10 mg / mL) in Example 5 were reacted with the solution in the kit at 37°C for 1 hour, and the absorbance of the mixed solution at 536 nm was measured by ultraviolet spectrophotometer to calculate the scavenging efficiency of CS-PS and CS-PS-DA lubricants on ·OH. The determination principle of ·OH scavenging is that hydrogen peroxide (H2O2) reacts with Fe 2+ The Fenton reaction produces OH, which converts o-phenanthroline-Fe 2+ Fe in aqueous solution 2+ Oxidized to Fe 3+ , resulting in a decrease in the absorbance of the solution at 536nm. The degree to which the sample inhibits the decrease in the absorbance at 536nm reflects its ability to remove .

[0071] Figure 3 is the scavenging efficiency of CS-PS lubricant and CS-PS-DA lubricant on hydroxyl radicals (·OH). Figure 3 The results in [ 24 ] showed that the hydroxyl radical scavenging efficiency of CS-PS lubricant was only 14.5%, while that of CS-PS-DA lubricant reached 40%, which was mainly attributed to the presence of catechol structural units in the CS-PS-DA lubricant molecules.

[0072] Example 8 Oxygen Anion Free Radicals (·O2 - ) Clearance Test

[0073] The oxygen anion scavenging ability kit was purchased from Shanghai Youxuan Biotechnology Co., Ltd. 200 μL CS-PS lubricant (10 mg / mL) and CS-PS-DA lubricant (10 mg / mL) in Example 5 were reacted with the solution in the kit at 37°C for 30 min, and the absorbance of the mixed solution at 530 nm was measured to evaluate the effects of CS-PS lubricant and CS-PS-DA lubricant on·O2 - The removal efficiency of O2 - The principle of the clearance determination is that xanthine and xanthine oxidase reaction system produce O2 -, reacts with hydroxylamine hydrochloride to generate NO2 - NO2 - It reacts with p-aminobenzenesulfonic acid and α-naphthylamine to generate a red azo compound with a characteristic absorption peak at 530nm. The sample is resistant to ·O2 - The scavenging ability was negatively correlated with the absorbance at 530 nm.

[0074] Figure 4 The CS-PS lubricant and CS-PS-DA lubricant react with oxygen anion free radicals (·O2 - ) removal efficiency. Figure 4 The results in the literature showed that CS-PS·O2 - The removal efficiency is only 2.5%, while the ·O2 - The removal efficiency reached 66%, which is mainly attributed to the presence of catechol structural units in the CS-PS-DA lubricant molecule.

[0075] Example 9: Verification of osteoarthritis treatment in mice

[0076] First, rats were anesthetized with sodium pentobarbital (30 mg / kg), the right knee hair was shaved, and then disinfected with alcohol. The rat epidermis and fascia were cut to expose the right knee joint and open the joint cavity. Subsequently, the anterior cruciate ligament and medial collateral ligament were cut and the rat internal meniscus was removed, and finally the joint cavity and epidermis were sutured. In addition, the sham operation group only performed the operation of opening and suturing the joint cavity, without cutting the ligament and retaining the meniscus. Two weeks after the operation, the rats were randomly divided into 4 groups (n=6 in each group): sham operation group (Sham), model group (OA), CS-PS treatment group and CS-PS-DA treatment group. Every 2 weeks, 100 μL NS was injected into the joint cavity of rats in the sham operation group and the model group; 100 μL CS-PS lubricant (10 mg / mL) and CS-PS-DA lubricant (10 mg / mL) in Example 5 were injected into the lubricant treatment group. The treatment process lasted for eight weeks.

[0077] Figure 5 The therapeutic effects of normal saline, CS-PS lubricant and CS-PS-DA lubricant on rats with osteoarthritis. Figure 5 The results in the study showed that the degree of cartilage wear in the CS-PS-DA lubricant-treated group was significantly less than that in the NS and CS-PS treatment groups, and the cartilage thickness was even close to that of the sham group (Sham), which may be related to the good lubrication and adsorption properties of the CS-PS-DA lubricant on the cartilage surface. At the same time, the cartilage in the NS and CS-PS treatment groups had typical osteoarthritis characteristics, such as vertical cracks, surface discontinuity, erosion, and deformation. However, the cartilage in the CS-PS-DA lubricant-treated group showed no obvious deformation, and the lesions and erosion on the cartilage surface were also smaller.

[0078] The results of the above embodiments show that the present invention selects natural polysaccharide chitosan as the central skeleton of the lubricant macromolecule through the innovative design of the molecular structure, and simultaneously introduces lubricating and adhesive functional segments into the skeleton molecular structure, which not only enhances the affinity between the lubricant and the articular cartilage, but also effectively forms a lubricating layer and reduces the friction on the cartilage surface. At the same time, since the catechol group adhering to the surface of the cartilage also has excellent active oxygen free radical scavenging function, the inflammation level in the joint can be significantly reduced. The CS-PS-DA lubricant provided by the present invention is a new type of biological lubricant, which has broad application prospects in the treatment of osteoarthritis.

[0079] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A bone and joint biological lubricant, characterized in that: It includes propane sultone and catechol modified chitosan derivatives and a good solvent; the structural formula of the propane sultone and catechol modified chitosan derivatives is shown in Formula I: Formula I; In formula I: X+Y+Z=0.9, X is 0.3-0.6, Y is 0.1-0.4, and Z is 0.2-0.5; The preparation method of the propane sultone and catechol modified chitosan derivative comprises the following steps: The chitosan solution and propane sultone are mixed to carry out a first grafting reaction to obtain propane sultone-modified chitosan; 3,4-dihydroxyphenylpropionic acid, water, ethyl (3-(dimethylamino)propyl) carbodiimide hydrochloride and N-hydroxysuccinimide are mixed for activation reaction, and the obtained activation reaction liquid and the propane sultone modified chitosan are mixed for a second grafting reaction to obtain propane sultone and catechol modified chitosan derivatives; the activation reaction temperature is 10-50°C, and the reaction time is 0.5-6h.

2. The bone and joint biological lubricant according to claim 1, characterized in that: The preparation method of the chitosan solution comprises: dispersing chitosan in water, then adding acetic acid solution to adjust the pH value to 4-6, so as to obtain the chitosan solution; the molecular weight of the chitosan is 100,000-1,000,000, and the viscosity is 10-200 mPa.s.

3. The bone and joint biological lubricant according to claim 1, characterized in that: The mass ratio of propane sultone to chitosan is 1:(1-5); The first grafting reaction takes place for 4 to 24 hours at a temperature of 50 to 100°C.

4. The bone and joint biological lubricant according to claim 1, characterized in that: The mass ratio of the 3,4-dihydroxyphenylpropionic acid, ethyl (3-(dimethylamino)propyl) carbodiimide hydrochloride and N-hydroxysuccinimide is (1-10):(1-10):(1-20); the mass ratio of the propane sultone-modified chitosan and 3,4-dihydroxyphenylpropionic acid is 1:(1-10); the temperature of the second grafting reaction is 10-50° C., and the reaction time is 6-36 hours.

5. The bone and joint biological lubricant according to claim 1, characterized in that: After the first grafting reaction is completed, the obtained solid product is sequentially washed, dialyzed and freeze-dried; after the second grafting reaction is completed, the obtained product liquid is sequentially dialyzed and freeze-dried.

6. The bone and joint biological lubricant according to claim 1, characterized in that: The good solvent includes one or more of deionized water, phosphate buffered saline and physiological saline.

7. The bone and joint biological lubricant according to claim 1 or 6, characterized in that: The concentration of propane sultone and catechol-modified chitosan derivative in the bone and joint biological lubricant is 0.1-20 mg / mL.

8. The method for preparing the bone and joint biological lubricant according to any one of claims 1 to 7, characterized in that: The following steps are involved: The propane sultone and the catechol-modified chitosan derivative are dissolved in the good solvent to obtain the bone and joint biological lubricant.

9. Use of the bone and joint biological lubricant according to any one of claims 1 to 7 or the bone and joint biological lubricant prepared by the preparation method according to claim 8 in the preparation of a drug for treating osteoarthritis.

Citation Information

Patent Citations

  • Chitosan biomacromolecule and preparation method and application thereof

    CN108976317A

  • Modified chitosan, preparation method of modified chitosan, biological lubricant and application of biological lubricant

    CN114854026A

  • Process for bone tissue decellularization

    US20170021059A1

  • Biological polysaccharide hydrogel, preparation method therefor and application thereof

    WO2023020256A1