A method for preparing a heterogeneous catalyst for transesterification reaction

The preparation method of a near-neutral anion exchange resin using acetate as an active group solves the problems of insufficient catalyst activity and low selectivity in the transesterification method, and prepares an efficient, stable and easy-to-separate catalyst for alkyl oxalate. The synthesis achieves efficient transesterification reaction.

CN116351470BActive Publication Date: 2024-10-15SHENYANG INSTITUTE OF CHEMICAL TECHNOLOGY +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310198347.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-03
Publication Date
2024-10-15
Estimated Expiration
2043-03-03

AI Technical Summary

Technical Problem

Existing catalysts for preparing alkyl oxalates through transesterification have problems such as insufficient catalytic activity, low selectivity, and difficulty in separation. In particular, strongly basic anion exchange resins are prone to deactivation, and strongly acidic cation exchange resins have low catalytic efficiency.

Method used

A method for preparing a near-neutral anion exchange resin using acetate as the key active group, by placing the exchange resin containing chloride ions in alcohol to swell, mixing with acetate and a solvent, and washing with water and vacuum drying after the reaction. Heterogeneous catalysts for transesterification reactions.

Benefits of technology

It achieves the efficient and stable synthesis of catalytic dimethyl oxalate, methyl ethyl oxalate and dibutyl oxalate. The catalyst is not easy to deactivate and is easy to separate from the reaction system. The process is simple, green and environmentally friendly.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a method for preparing a heterogeneous catalyst for transesterification reaction, which comprises drying and dehydrating a conventional ion exchange resin obtained by polymerizing styrene and divinylbenzene containing chloride ions, swelling in an alcohol solution to obtain a resin matrix; the resin matrix is ​​mixed with a modifier containing acetate and an ethanol solution to react, and filtering, washing and drying to obtain a high-efficiency heterogeneous catalyst for oxalate transesterification reaction. The catalyst is a nearly neutral anion exchange resin with acetate as a key active group, and has the advantages of high efficiency, stability, not easy to deactivate, easy separation from the reaction system, etc. in catalyzing dimethyl oxalate and ethanol or butanol to synthesize methyl ethyl oxalate, diethyl oxalate and dibutyl oxalate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chemical industry catalysis, and in particular relates to a method for preparing a heterogeneous catalyst used for ester exchange reaction. Background Art

[0002] my country's ethylene glycol consumption is dominant in Asia, and it is also the world's largest ethylene glycol consumer market. With the rapid development of the coal chemical industry, the technology of producing ethylene glycol from synthesis gas via dimethyl oxalate (DMO) has developed rapidly. Due to the serious homogeneous competition of domestic coal-to-ethylene glycol technology, the overall operating rate of coal-to-ethylene glycol is less than 30%, resulting in a continuous slump in ethylene glycol prices, which has now fallen to 3,700 yuan / ton, greatly weakening the profitability of coal-to-ethylene glycol technology. Therefore, it is urgent to expand the downstream industry of ethylene glycol, develop DMO-based platform compounds, design synthesis processes for high value-added downstream products, develop a multi-end coal-to-ethylene glycol industry chain, and seek the development of downstream bulk or high value-added products of ethylene glycol.

[0003] Alkyl oxalate is an important organic chemical raw material, which is widely used in the preparation of various dyes, medicines, important solvents, extractants and various intermediates. It can undergo various condensation reactions with fatty acid esters, cyclohexyl acetophenone, amino alcohols and many heterocyclic compounds. Alkyl oxalate can be hydrolyzed to produce oxalic acid, which is widely used in defense, electronics, medicine, materials, agriculture, light industry and chemical industry; alkyl oxalate can be further hydrogenated to produce ethylene glycol, which is widely used in the production of synthetic fibers, unsaturated polyester resins, plastic films, and is also used as adhesives, solvents and plasticizers in fine chemicals; alkyl oxalate can be decomposed and ammoniated at normal pressure to produce high-quality slow-release and high-efficiency fertilizer oxamide, which is used in the agricultural field. In industry, the synthesis methods of alkyl oxalate are mainly two categories: traditional oxalylation method and carbon monoxide oxidative coupling method. Among them, the oxalylation method is a technology introduced and optimized from abroad in the 1950s. Its reaction requires a large amount of oxalic acid, is prone to side reactions, and has serious corrosion to equipment and is prone to environmental pollution. It is gradually difficult to meet the needs of modern industrial development. The carbon monoxide oxidative coupling method is a new technology discovered by Stein wand et al. in the mid-1960s. It uses a PdCl2-CuCl2 redox catalyst, which is very easy to be poisoned and deactivated, limiting the large-scale application of this process. The ester exchange method is a simple process for preparing alkyl oxalate, which can obtain the corresponding alkyl oxalate product in one step. It is a high value-added route for preparing alkyl oxalate.

[0004] In the process of preparing alkyl oxalate by transesterification, the catalyst is the key to determine whether the reaction is successful. Patent CN1583254 A discloses a molybdenum oxide catalyst for synthesizing phenyl oxalate by transesterification and its preparation method. The catalyst for synthesizing phenyl oxalate by transesterification is obtained by the steps of preparing molybdenum trioxide slurry, grinding the carrier, mixing with the slurry, impregnation, drying, etc. The preparation process of this catalyst has the advantages of low cost, no pollution to the environment, and no corrosion to the equipment. Patent CN 1986517 A discloses a method for synthesizing methyl phenyl oxalate and diphenyl oxalate catalyzed by a composite carrier-supported metal oxide. Titanium dioxide is used as a carrier and metal oxides are used as active components. The preparation of a composite carrier-supported metal oxide catalyst is realized and successfully used in the transesterification reaction to prepare phenyl oxalate. Patent CN 111672493 A discloses an alkaline mesoporous catalyst, a preparation method and application thereof, which realizes the preparation of a mesoporous magnesium oxide catalyst with a large specific surface area, a large pore size, a high alkali content and a medium-strong alkali center. The application of the catalyst in the synthesis of diethyl oxalate by the ester exchange method has the advantages of mild reaction conditions, high catalytic activity, high selectivity of the target product and long catalyst life. Patents CN109081779 A, ​​CN 112279762 A, CN 112279763 A, CN 112279762 A, CN 114292182 A, and CN112961057 A all disclose processes for preparing alkyl oxalate by transesterification. In the early alkyl oxalate synthesis stage, these processes all use the addition of catalysts to promote the transesterification reaction. However, the catalytic activity and selectivity of alkyl oxalate currently achieved are still far from the requirements of large-scale industrial production, and are accompanied by problems such as difficulty in separating the catalyst from the system. Therefore, it is still urgent to further develop a catalyst system with good catalytic activity, higher selectivity, convenient preparation, and easy separation.

[0005] Ion exchange resin is an insoluble polymer compound with functional groups (active groups that exchange ions), a network structure, and is insoluble. It is usually a spherical particle with a pore structure of gel type and macroporous type. It has two categories: acidic cation exchange resin and basic anion exchange resin. In organic synthesis, acids and bases are often used as catalysts for esterification, hydrolysis, transesterification, hydration and other reactions. Using ion exchange resins instead of inorganic acids and bases can also carry out the above reactions, and has more advantages. For example, the resin can be reused, the product is easy to separate, the reactor will not be corroded, the environment will not be polluted, and the reaction is easy to control. However, strong alkaline ion exchange resins are easily deactivated when catalyzing oxalate exchange reactions, and strong acidic resins are less efficient when catalyzing oxalate exchange reactions. Therefore, it is challenging to develop ion exchange resins with both high activity and high stability. Summary of the invention

[0006] According to one aspect of the present application, a method for preparing a heterogeneous catalyst for an ester exchange reaction is provided. In view of the fact that strongly basic anion exchange resins are easily deactivated and strongly acidic cation exchange resins have low catalytic efficiency during the synthesis of oxalate esters, the present application proposes a method for preparing a nearly neutral anion exchange resin with acetate as a key active group. The synthesized heterogeneous anion exchange resin has the advantages of high efficiency, stability, not easy to deactivate, and easy separation from the reaction system in catalyzing the synthesis of ethyl methyl oxalate, diethyl oxalate and dibutyl oxalate from dimethyl oxalate and ethanol or butanol.

[0007] This application adopts the following technical solutions:

[0008] A method for preparing a heterogeneous catalyst for transesterification reaction comprises the following steps:

[0009] S1. Place the exchange resin containing chloride ions in alcohol to swell and obtain a resin matrix;

[0010] S2. The resin matrix obtained in step S1 is mixed with a modifier containing acetate and a solvent, and reacted to obtain a heterogeneous catalyst for transesterification reaction.

[0011] Optionally, the exchange resin containing chloride ions is an exchange resin containing chloride ions that has been dried at 100-120° C. for 5-10 hours.

[0012] Optionally, the exchange resin containing chloride ions is obtained by the following preparation method:

[0013] Place a strongly basic anion exchange resin in hydrochloric acid and stir to react for 1 to 5 hours to obtain an exchange resin containing chloride ions;

[0014] The concentration of the hydrochloric acid is 0.1-0.6 mol / L;

[0015] The alkali content in the strong basic anion exchange resin is 10-30wt%.

[0016] The alkali content in the strongly basic anion exchange resin is selected from any value of 10wt%, 12wt%, 14wt%, 16wt%, 18wt%, 20wt%, 22wt%, 24wt%, 26wt%, 28wt%, 30wt%, or any range therebetween.

[0017] Optionally, the exchange resin containing chloride ions is obtained by the following preparation method: placing a strongly alkaline anion exchange resin in hydrochloric acid, stirring the reaction for 1 to 5 hours until it becomes weakly acidic, and obtaining an exchange resin containing chloride ions.

[0018] The active group in the strong alkaline anion exchange resin is hydroxide.

[0019] Optionally, the product after the stirring reaction is washed with water, washed with ethanol, filtered, and dried to obtain an exchange resin containing chloride ions.

[0020] Optionally, the content of chloride ions in the exchange resin containing chloride ions is 20-40 wt%.

[0021] Optionally, the content of chloride ions in the exchange resin containing chloride ions is selected from any value of 20wt%, 22wt%, 24wt%, 26wt%, 28wt%, 30wt%, 32wt%, 34wt%, 36wt%, 38wt%, 40wt%, or any range therebetween.

[0022] Optionally, the molar ratio of the acetate to the chloride ions in the exchange resin containing chloride ions is 1-3:1.

[0023] Optionally, the molar ratio of the acetate to the chloride ions in the chloride ion-containing exchange resin is selected from any value of 1:1, 1.2:1, 1.4:1, 1.6:1, 1.8:1, 2:1, 2.2:1, 2.4:1, 2.6:1, 2.8:1, 3:1, or any range therebetween.

[0024] Optionally, the weight ratio of the ethanol to the exchange resin containing chloride ions is 2-4:1.

[0025] Optionally, the weight ratio of the acetate to the solvent is 1:10-30.

[0026] Optionally, the weight ratio of the acetate to the solvent is any value selected from 1:10, 1:12, 1:14, 1:16, 1:18, 1:20, 1:22, 1:24, 1:26, 1:28, 1:30, or any range therebetween.

[0027] Optionally, the weight ratio of the ethanol to the exchange resin containing chloride ions is selected from any value of 2:1, 2.2:1, 2.4:1, 2.6:1, 2.8:1, 3:1, 3.2:1, 3.4:1, 3.6:1, 3.8:1, 4:1, or any range therebetween.

[0028] Optionally, in step S2, the reaction conditions are: stirring at 20-30° C. for 10-15 hours.

[0029] Optionally, the acetate is selected from at least one of potassium acetate, sodium acetate, magnesium acetate, calcium acetate, zinc acetate, copper acetate, and manganese acetate.

[0030] Optionally, the exchange resin containing chloride ions is selected from at least one of a strongly basic anion resin containing chloride ions, a weakly basic anion resin containing chloride ions, and a transformation of an anion resin containing chloride ions.

[0031] Optionally, the solvent is selected from at least one of methanol, ethanol and water.

[0032] Optionally, step S2 further comprises washing the product with water and alcohol after the reaction, and then vacuum drying it at 70-90° C. for 5-12 hours to obtain a heterogeneous catalyst for transesterification reaction.

[0033] Optionally, step S2 further comprises washing the product with water 2 to 3 times, washing it with alcohol 2 to 3 times after the reaction, filtering it, and then vacuum drying it at 70 to 90° C. for 5 to 12 hours to obtain a heterogeneous catalyst for transesterification reaction.

[0034] According to another aspect of the present application, there is provided a use of a heterogeneous catalyst for transesterification reaction prepared according to the above-mentioned preparation method in the directional synthesis of alkyl oxalate by transesterification reaction.

[0035] Optionally, the transesterification reaction includes using a heterogeneous catalyst for transesterification reaction to catalyze the transesterification reaction of at least one of the alcohol compounds and ester compounds with oxalic acid ester to synthesize alkyl oxalate.

[0036] Optionally, the alcohol compound is selected from at least one of ethanol and butanol.

[0037] Optionally, the ester compound is selected from at least one of dimethyl oxalate, diethyl oxalate and dibutyl oxalate.

[0038] Optionally, the alkyl oxalate is selected from at least one of diethyl oxalate, ethyl methyl oxalate, dibutyl oxalate and methyl butyl oxalate.

[0039] Optionally, the weight ratio of the heterogeneous catalyst for the transesterification reaction to the oxalate is 0.001-0.1:1.

[0040] Optionally, the weight ratio of the heterogeneous catalyst used in the transesterification reaction to the oxalate is 0.04-0.06:1.

[0041] Optionally, the conditions for the transesterification reaction are: reaction temperature 60-140° C., reaction pressure 10-50 KPa.

[0042] Optionally, the reaction temperature in the transesterification reaction conditions is selected from any value of 60°C, 80°C, 100°C, 120°C, 140°C, or any range therebetween.

[0043] The beneficial effects of this application include:

[0044] The method for preparing a heterogeneous catalyst for ester exchange reaction provided in the present application does not require calcination during the preparation process, has a simple process, has good comprehensive catalyst performance, is green and environmentally friendly, and is easy to separate the reaction system. It is a new catalyst for the directional synthesis of alkyl oxalate by ester exchange method. Implementation

[0045] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0046] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.

[0047] The solvents methanol and ethanol are both commercially available analytical grade solvents with a purity of ≥99.5%.

[0048] Chloride ion exchange resins are commercially available or can be prepared as follows:

[0049] Weigh a commercially available strong alkaline anion exchange resin (a common commercial resin obtained by polymerization of vinylbenzene and styrene followed by quaternization reaction, with an active group of hydroxide and an alkali density of 0.25 mmol / g) and place it in a drying oven for drying, wherein the required drying temperature ranges from 100 to 120°C and the required drying time ranges from 5 to 10 h to obtain a dry resin; weigh the dry resin and place it in a certain concentration of HCl solution, and stir it thoroughly at room temperature until it becomes weakly acidic, wherein the stirring time ranges from 1 to 5 h and the solubility range of the hydrochloric acid solution used is from 0.05 to 0.2 mol / L; then wash with water, wash with ethanol, filter, dry, etc. to obtain a hydrochloric acid-chlorinated exchange resin containing chloride ions. Example

[0050] Weigh 40.28 g of exchange resin with chloride anion (a mature commercial preparation method is to polymerize divinylbenzene and styrene and then chlorinate and then quaternize to obtain it; there are many brands on the market, but the structure is basically the same, which has little effect on the oxalate exchange reaction), dry it at 115 ° C for 10 h, and finally obtain 22.99 g of dehydrated resin matrix, the chloride ion content in the dehydrated resin matrix is ​​20wt%; weigh 10 g of the dried resin and swell it in 31 g of ethanol solution for 2 h to obtain the swollen resin matrix A1; weigh 11.61 g of potassium acetate and 155 g of ethanol solution, add them to a beaker respectively, stir until completely dissolved, and prepare a potassium acetate modifier solution B of a certain concentration; A1 and B solution are completely mixed and stirred continuously at room temperature for 10 h; then filter the modified resin particles, rinse with 200 g of deionized water, dissolve the washed resin particles in 150 g of ethanol, and stir at room temperature for 30 After filtration for 3 min, the mixture was washed with ethanol and 11.66 g of wet resin was obtained. The mixture was placed in a vacuum drying oven at a drying pressure of 0.08 MPa and a drying temperature of 70 °C for 12 h. The mixture was placed at room temperature to obtain 9.05 g of modified resin catalyst, which was named Catalyst No. 1. Example

[0051] Weigh 40.28 g of exchange resin with chloride anion (a mature commercial preparation method is to polymerize divinylbenzene and styrene and then chlorinate and then quaternize to obtain it; there are many brands on the market, but the structure is basically the same, which has little effect on the oxalate exchange reaction), dry it at 115 ° C for 10 h, and finally obtain 22.99 g of dehydrated resin matrix, the chloride ion content in the dehydrated resin matrix is ​​20wt%; weigh 10 g of the dried resin and swell it in 31 g of ethanol solution for 2 h to obtain the swollen resin matrix A1; weigh 17.82 g of calcium acetate and 500 g of ethanol solution, add them to a beaker respectively, stir until completely dissolved, and prepare a calcium acetate modifier solution B of a certain concentration; A1 and B solution are completely mixed and stirred continuously at room temperature for 10 h; then filter the modified resin particles, rinse with 200 g of deionized water, dissolve the washed resin particles in 150 g of ethanol, and stir at room temperature for 30 After filtration for 3 min, the mixture was washed with ethanol and 8.76 g of wet resin was obtained. The mixture was placed in a vacuum drying oven at a drying pressure of 0.08 MPa and a drying temperature of 70 °C for 12 h. The mixture was placed at room temperature to obtain 6.75 g of modified resin catalyst, which was named Catalyst No. 2. Example

[0052] Weigh 40.28 g of exchange resin with chloride anion (a mature commercial preparation method is to polymerize divinylbenzene and styrene and then chlorinate and then quaternize to obtain it; there are many brands on the market, but the structure is basically the same, which has little effect on the oxalate exchange reaction), dry it at 115 ° C for 10 h, and finally obtain 22.99 g of dehydrated resin matrix, the chloride ion content in the dehydrated resin matrix is ​​20wt%; weigh 10 g of the dried resin and swell it in 31 g of ethanol solution for 2 h to obtain the swollen resin matrix A1; weigh 9.24 g of sodium acetate and 130 g of ethanol solution, add them to a beaker respectively, stir until completely dissolved, and prepare a sodium acetate modifier solution B of a certain concentration; A1 and B solution are completely mixed and stirred continuously at room temperature for 10 h; then filter the modified resin particles, rinse with 200 g of deionized water, dissolve the washed resin particles in 150 g of ethanol, and stir at room temperature for 30 min later, filter and repeat the above ethanol washing operation for 3 times. After filtration, 11.10 g of wet resin was obtained, which was placed in a vacuum drying oven at a drying pressure of 0.08 MPa and a drying temperature of 70 °C for 12 h. After being placed at room temperature, 8.61 g of modified resin catalyst was obtained, which was named Catalyst No. 3. Example

[0053] Weigh 40.28 g of exchange resin with chloride anion (a mature commercial preparation method is to polymerize divinylbenzene and styrene and then chlorinate and then quaternize to obtain it; there are many brands on the market, but the structure is basically the same, which has little effect on the oxalate exchange reaction), dry it at 115 ° C for 10 h, and finally obtain 22.99 g of dehydrated resin matrix, the chloride ion content in the dehydrated resin matrix is ​​20wt%; weigh 10 g of the dried resin and swell it in 31 g of ethanol solution for 2 h to obtain the swollen resin matrix A1; weigh 24.16 g of magnesium acetate and 339 g of ethanol solution, add them to a beaker respectively, stir until completely dissolved, and prepare a magnesium acetate modifier solution B of a certain concentration; A1 and B solution are completely mixed and stirred continuously at room temperature for 10 h; then filter the modified resin particles, rinse with 200 g of deionized water, dissolve the washed resin particles in 150 g of ethanol, and stir at room temperature for 30 After filtration for 3 min, the mixture was washed with ethanol and the above-mentioned washing process was repeated for 3 times. After filtration, 11.37 g of wet resin was obtained. The mixture was placed in a vacuum drying oven at a drying pressure of 0.08 MPa and a drying temperature of 70 °C for 12 h. After being placed at room temperature, 8.53 g of modified resin catalyst was obtained, which was named Catalyst No. 4. Example

[0054] Weigh 40.28 g of exchange resin with chloride anion (a mature commercial preparation method is to polymerize divinylbenzene and styrene and then chlorinate and then quaternize to obtain it; there are many brands on the market, but the structure is basically the same, which has little effect on the oxalate exchange reaction), dry it at 115 ° C for 10 h, and finally obtain 22.99 g of dehydrated resin matrix, the chloride ion content in the dehydrated resin matrix is ​​20wt%; weigh 10 g of the dried resin and swell it in 31 g of ethanol solution for 2 h to obtain the swollen resin matrix A1; weigh 20.67 g of zinc acetate and 290 g of ethanol solution, add them to a beaker respectively, stir until completely dissolved, and prepare a zinc acetate modifier solution B of a certain concentration; A1 and B solution are completely mixed and stirred continuously at room temperature for 10 h; then filter the modified resin particles, rinse with 200 g of deionized water, dissolve the washed resin particles in 150 g of ethanol, and stir at room temperature for 30 After filtration for 3 min, the mixture was washed with ethanol and 10.69 g of wet resin was obtained. The mixture was placed in a vacuum drying oven at a drying pressure of 0.08 MPa and a drying temperature of 70 °C for 12 h. The mixture was placed at room temperature to obtain 8.29 g of modified resin catalyst, which was named Catalyst No. 5. Example

[0055] Weigh 40.28 g of exchange resin with chloride anion (a mature commercial preparation method is to polymerize divinylbenzene and styrene and then chlorinate and then quaternize to obtain it; there are many brands on the market, but the structure is basically the same, which has little effect on the oxalate exchange reaction), dry it at 115 ° C for 10 h, and finally obtain 22.99 g of dehydrated resin matrix, the chloride ion content in the dehydrated resin matrix is ​​20wt%; weigh 10 g of the dried resin and swell it in 31 g of ethanol solution for 2 h to obtain the swollen resin matrix A1; weigh 22.5 g of copper acetate and 315 g of ethanol solution, add them to a beaker respectively, stir until completely dissolved, and prepare a copper acetate modifier solution B of a certain concentration; A1 and B solution are completely mixed and stirred continuously at room temperature for 10 h; then filter the modified resin particles, rinse with 200 g of deionized water, dissolve the washed resin particles in 150 g of ethanol, and stir at room temperature for 30 After filtration for 3 min, the mixture was washed with ethanol and the above-mentioned washing process was repeated for 3 times. After filtration, 10.86 g of wet resin was obtained. The mixture was placed in a vacuum drying oven at a drying pressure of 0.08 MPa and a drying temperature of 70 °C for 12 h. After being placed at room temperature, 8.43 g of modified resin catalyst was obtained, which was named Catalyst No. 6. Example

[0056] Weigh 40.28 g of exchange resin with chloride anion (a mature commercial preparation method is to polymerize divinylbenzene and styrene and then chlorinate and then quaternize to obtain it; there are many brands on the market, but the structure is basically the same, which has little effect on the oxalate exchange reaction), dry it at 115 ° C for 10 h, and finally obtain 22.99 g of dehydrated resin matrix, the chloride ion content in the dehydrated resin matrix is ​​20wt%; weigh 10 g of the dried resin and swell it in 31 g of ethanol solution for 2 h to obtain the swollen resin matrix A1; weigh 19.5 g of manganese acetate and 273 g of ethanol solution, add them to a beaker respectively, stir until completely dissolved, and prepare a manganese acetate modifier solution B of a certain concentration; A1 and B solution are completely mixed and stirred continuously at room temperature for 10 h; then filter the modified resin particles, rinse with 200 g of deionized water, dissolve the washed resin particles in 150 g of ethanol, and stir at room temperature for 30 After filtration for 3 min, the mixture was washed with ethanol and 10.35 g of wet resin was obtained. The mixture was placed in a vacuum drying oven at a drying pressure of 0.08 MPa and a drying temperature of 70 °C for 12 h. The mixture was placed at room temperature to obtain 8.02 g of modified resin catalyst, which was named Catalyst No. 7. Example

[0057] Weigh 40 g of a strongly alkaline anion exchange resin (a common commercial resin obtained by polymerization of vinylbenzene and styrene followed by quaternization reaction, with the active group being hydroxide and the alkaline content being 10 wt%) and place it in 600 mL of 0.4 mol / L HCl solution. Stir it thoroughly at room temperature for 5 h until it becomes weakly acidic. After filtering, wash it twice with ethanol, and obtain a resin precursor containing chloride ions after suction filtration, which is placed in a desiccator for later use.

[0058] Weigh 12 g of the above resin precursor and swell it in 33 g of ethanol solution for 2 h to obtain the swollen resin matrix A2; weigh 13.27 g of potassium acetate and 319 g of ethanol solution, add them into a beaker respectively, stir until completely dissolved, and prepare a potassium acetate modifier solution B of a certain concentration; A2 and B solution are completely mixed and stirred continuously at room temperature for 10 h; then filter the modified resin particles, rinse with 200 g of deionized water, dissolve the washed resin particles in 150 g of ethanol, stir at room temperature for 30 min, filter and repeat the above ethanol washing operation 3 times, after filtration, put it into a vacuum drying oven with a drying pressure of 0.08 MPa and a drying temperature of 80 ℃, dry it for 12 h, and place it at room temperature to obtain 10.21 g of modified resin catalyst, named Catalyst No. 8. Example

[0059] Weigh 40 g of a strongly basic anion exchange resin (a common commercial resin obtained by polymerization of vinylbenzene and styrene followed by quaternization reaction, with the active group being hydroxide and the base content being 10 wt%) and place it in 600 mL of 0.4 mol / L HCl solution, and stir it thoroughly at room temperature for 5 h until it becomes weakly acidic; filter and wash it twice with ethanol, and obtain a resin precursor containing chloride ions after suction filtration, which is placed in a desiccator for later use;

[0060] Weigh 12 g of the above resin precursor and swell it in 33 g of ethanol solution for 2 h to obtain the swollen resin matrix A2; weigh 21.39 g of calcium acetate and 514 g of ethanol solution, add them into a beaker respectively, stir until completely dissolved, and prepare a calcium acetate modifier solution B of a certain concentration; A2 and B solution are completely mixed and stirred continuously at room temperature for 10 h; then filter the modified resin particles, rinse with 200 g of deionized water, dissolve the washed resin particles in 150 g of ethanol, stir at room temperature for 30 min, filter and repeat the above ethanol washing operation 3 times, after filtration, put it into a vacuum drying oven with a drying pressure of 0.08 MPa and a drying temperature of 80 ℃, dry it for 12 h, and leave it at room temperature to obtain 7.47 g of modified resin catalyst, named Catalyst No. 9. Example

[0061] Weigh 40 g of a strongly basic anion exchange resin (a common commercial resin obtained by polymerization of vinylbenzene and styrene followed by quaternization reaction, with the active group being hydroxide and the base content being 10 wt%) and place it in 600 mL of 0.4 mol / L HCl solution, and stir it thoroughly at room temperature for 5 h until it becomes weakly acidic; filter and wash it twice with ethanol, and obtain a resin precursor containing chloride ions after suction filtration, which is placed in a desiccator for later use;

[0062] Weigh 12 g of the above resin precursor and swell it in 33 g of ethanol solution for 2 h to obtain the swollen resin matrix A2; weigh 11.09 g of sodium acetate and 267 g of ethanol solution, add them into a beaker respectively, stir until completely dissolved, and prepare a sodium acetate modifier solution B of a certain concentration; A2 and B solution are completely mixed and stirred continuously at room temperature for 10 h; then filter the modified resin particles, rinse with 200 g of deionized water, dissolve the washed resin particles in 150 g of ethanol, stir at room temperature for 30 min, filter and repeat the above ethanol washing operation 3 times, after filtration, put it into a vacuum drying oven with a drying pressure of 0.08 MPa and a drying temperature of 80 ℃, dry it for 12 h, and leave it at room temperature to obtain 9.67 g of modified resin catalyst, named catalyst No. 10. Example

[0063] Weigh 40 g of a strongly basic anion exchange resin (a common commercial resin obtained by polymerization of vinylbenzene and styrene followed by quaternization reaction, with the active group being hydroxide and the base content being 10 wt%) and place it in 600 mL of 0.4 mol / L HCl solution, and stir it thoroughly at room temperature for 5 h until it becomes weakly acidic; filter and wash it twice with ethanol, and obtain a resin precursor containing chloride ions after suction filtration, which is placed in a desiccator for later use;

[0064] Weigh 12 g of the above resin precursor and swell it in 33 g of ethanol solution for 2 h to obtain the swollen resin matrix A2; weigh 28.97 g of magnesium acetate and 696 g of ethanol solution, add them into a beaker respectively, stir until completely dissolved, and prepare a magnesium acetate modifier solution B of a certain concentration; A2 and B solution are completely mixed and stirred continuously at room temperature for 10 h; then filter the modified resin particles, rinse with 200 g of deionized water, dissolve the washed resin particles in 150 g of ethanol, stir at room temperature for 30 min, filter and repeat the above ethanol washing operation 3 times, after filtration, put it into a vacuum drying oven with a drying pressure of 0.08 MPa and a drying temperature of 80 ℃, dry it for 12 h, and place it at room temperature to obtain 9.92 g of modified resin catalyst, named catalyst No. 11. Example

[0065] Weigh 40 g of a strongly basic anion exchange resin (a common commercial resin obtained by polymerization of vinylbenzene and styrene followed by quaternization reaction, with the active group being hydroxide and the base content being 10 wt%) and place it in 600 mL of 0.4 mol / L HCl solution, and stir it thoroughly at room temperature for 5 h until it becomes weakly acidic; filter and wash it twice with ethanol, and obtain a resin precursor containing chloride ions after suction filtration, which is placed in a desiccator for later use;

[0066] Weigh 12 g of the above resin precursor and swell it in 33 g of ethanol solution for 2 h to obtain the swollen resin matrix A2; weigh 24.81 g of zinc acetate and 596 g of ethanol solution, add them into beakers respectively, stir until completely dissolved, and prepare a zinc acetate modifier solution B of a certain concentration; A2 and B solution are completely mixed and stirred continuously at room temperature for 10 h; then filter the modified resin particles, rinse with 200 g of deionized water, dissolve the washed resin particles in 150 g of ethanol, stir at room temperature for 30 min, filter and repeat the above ethanol washing operation 3 times, after filtration, put it into a vacuum drying oven with a drying pressure of 0.08 MPa and a drying temperature of 80 ℃, dry it for 12 h, and leave it at room temperature to obtain 9.89 g of modified resin catalyst, named catalyst No. 12. Example

[0067] Weigh 40g of strong alkaline anion exchange resin (common commercial resin obtained by polymerization of vinylbenzene and styrene followed by quaternization reaction, with the active group being hydroxide and the base content being 10wt%) and place it in 600mL of 0.4 mol / L HCl solution, and stir it thoroughly at room temperature for 5 hours until it becomes weakly acidic; filter and wash it twice with ethanol, and obtain a resin precursor containing chloride ions after suction filtration, which is placed in a desiccator for later use;

[0068] Weigh 12 g of the above resin precursor in 33 g of ethanol solution and swell it for 2 h to obtain the swollen resin matrix A2; weigh 26.97 g of copper acetate and 648 g of ethanol solution, add them into beakers respectively, stir until completely dissolved, and prepare a copper acetate modifier solution B of a certain concentration; mix the A and B solutions completely, and stir them thoroughly at room temperature for 24 h; then wash with ethanol 6-8 times, each time for 5 min, after filtration, put it into a vacuum drying oven, the drying pressure is 0.08 MPa, the drying temperature is 80°C, dry it for 12 h, and leave it at room temperature to obtain 10.07 g of modified resin catalyst, named Catalyst No. 13. Example

[0069] Weigh 40 g of a strongly basic anion exchange resin (a common commercial resin obtained by polymerization of vinylbenzene and styrene followed by quaternization reaction, with the active group being hydroxide and the base content being 10 wt%) and place it in 600 mL of 0.4 mol / L HCl solution, and stir it thoroughly at room temperature for 5 h until it becomes weakly acidic; filter and wash it twice with ethanol, and obtain a resin precursor containing chloride ions after suction filtration, which is placed in a desiccator for later use;

[0070] Weigh 12 g of the above resin precursor and swell it in 33 g of ethanol solution for 2 h to obtain the swollen resin matrix A2; weigh 23.41 g of manganese acetate and 562 g of ethanol solution, add them into a beaker respectively, stir until completely dissolved, and prepare a manganese acetate modifier solution B of a certain concentration; mix the A and B solutions completely and stir continuously at room temperature for 10 h; then filter the modified resin particles, rinse with 200 g of deionized water, dissolve the washed resin particles in 150 g of ethanol, stir at room temperature for 30 min, filter and repeat the above ethanol washing operation 3 times, after filtration, put it into a vacuum drying oven with a drying pressure of 0.08 MPa and a drying temperature of 80 °C, dry it for 12 h, and place it at room temperature to obtain 9.46 g of modified resin catalyst, named catalyst No. 14.

[0071] The catalysts prepared in Examples 1 to 14 as described above were used for the reaction performance evaluation method of the directional synthesis of alkyl oxalate by transesterification reaction: 100 g of dimethyl oxalate (DMO) and 235 g of ethanol were filled into a 1 L reaction distillation tower, fully stirred, heated to 80° C., 5 g of catalyst was added, the reflux ratio was set to 3:1, the reaction was carried out at a reaction temperature of 80° C. for 5 h, the reaction pressure was 45 KPa, and the catalyst performance was examined. The results are shown in Table 1.

[0072] Table 1 Reaction performance of the catalysts obtained in Examples 1 to 14 for catalytic directional synthesis of alkyl oxalates

[0073] Experiment number t / min <![CDATA[ X DMO (%)]]> <![CDATA[ S MEO (%)]]> <![CDATA[ S DEO (%)]]> <![CDATA[ Y MEO (%)]]> <![CDATA[ Y DEO (%)]]> Catalyst No. 1 180 94.92 5.40 94.60 5.13 89.79 Catalyst No. 2 300 84.88 16.11 83.89 13.67 71.21 Catalyst No. 3 180 94.85 6.40 93.60 6.07 88.78 Catalyst No. 4 180 93.97 5.27 94.73 4.95 89.02 Catalyst No. 5 180 91.35 8.85 91.15 8.08 83.27 Catalyst No. 6 180 92.85 7.38 92.62 6.85 86.00 Catalyst No. 7 300 88.46 10.71 89.29 9.47 78.99 Catalyst No. 8 180 98.88 1.35 98.65 1.33 97.55 Catalyst No. 9 300 87.17 11.73 88.27 10.23 76.94 Catalyst No. 10 180 94.72 6.44 93.56 6.10 88.62 Catalyst No. 11 180 97.12 2.08 97.92 2.02 95.10 Catalyst No. 12 180 96.85 3.34 96.66 3.23 93.62 Catalyst No. 13 180 98.58 2.63 97.37 2.59 95.99 Catalyst No. 14 300 92.57 8.57 91.43 7.93 84.64

[0074] The catalyst prepared in Example 8 was selected for the reaction performance evaluation method of the directional synthesis of alkyl oxalate by ester exchange reaction: 100 g of dimethyl oxalate and 377 g of butanol were filled in a 1 L reaction distillation tower, fully stirred, heated to 120 ° C, added 5 g of catalyst, the reflux ratio was set to 5:1, and the reaction was carried out at a reaction temperature of 120 ° C for 5 h and a reaction pressure of 20 KPa. The catalyst performance was examined, and the results are shown in Table 2.

[0075] Table 2 Reaction performance of the catalyst obtained in Example 8 for catalytic synthesis of alkyl oxalate at different catalytic times

[0076] t / min <![CDATA[ X DMO (%)]]> <![CDATA[ S MBO (%)]]> <![CDATA[ S DBO (%)]]> <![CDATA[ Y MBO (%)]]> <![CDATA[ Y DBO (%)]]> 5 25.94 39.51 60.49 10.25 15.69 30 64.91 36.41 63.59 23.63 41.28 60 77.37 33.85 66.15 26.19 51.18 120 86.11 28.98 71.02 24.96 61.15 180 89.12 25.24 74.76 22.49 66.63 300 91.10 14.03 85.97 12.78 78.32

[0077] In the above table, X represents conversion rate, S represents selectivity, and Y represents yield; DMO is dimethyl oxalate, MBO is methyl butyl oxalate, and DBO is dibutyl oxalate.

[0078] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. An application of a heterogeneous catalyst for transesterification reaction in the directional synthesis of alkyl oxalate by transesterification reaction, characterized in that: The preparation method of the heterogeneous catalyst for transesterification reaction comprises the following steps: S1, placing the exchange resin containing chloride ions in ethanol to swell and obtain a resin matrix; S2, mixing the resin matrix obtained in step S1 with a modifier containing acetate and a solvent, and reacting them to obtain a heterogeneous catalyst for transesterification reaction; The solvent is selected from at least one of methanol, ethanol and water; The heterogeneous catalyst used for transesterification reaction is a nearly neutral anion exchange resin with acetate as a key active group.

2. The use according to claim 1, characterized in that: The exchange resin containing chloride ions is obtained by the following preparation method: Place a strongly basic anion exchange resin in hydrochloric acid and stir to react for 1 to 5 hours to obtain an exchange resin containing chloride ions; The concentration of the hydrochloric acid is 0.1-0.6 mol / L; The alkali content in the strong basic anion exchange resin is 10-30wt%.

3. The use according to claim 1, characterized in that: The content of chloride ions in the exchange resin containing chloride ions is 20-40wt%.

4. The use according to claim 1, characterized in that: The molar ratio of the acetate to the chloride ions in the chloride ion exchange resin is 1 to 3:1; The weight ratio of the acetate to the solvent is 1:10-30.

5. The use according to claim 1, characterized in that: In the step S1, the weight ratio of the ethanol to the exchange resin containing chloride ions is 2-4:

1.

6. The use according to claim 1, characterized in that: In the step S2, the reaction conditions for the mixed reaction of the resin matrix and the modifier are: stirring at 20-30° C. for 10-15 hours.

7. The use according to claim 1, characterized in that: The acetate is selected from at least one of potassium acetate, sodium acetate, magnesium acetate, calcium acetate, zinc acetate, copper acetate and manganese acetate.

8. The use according to claim 1, characterized in that: The exchange resin containing chloride ions is selected from at least one of a strongly basic anion resin containing chloride ions and a weakly basic anion resin containing chloride ions.

9. The use according to claim 1, characterized in that: The transesterification reaction comprises using a heterogeneous catalyst for transesterification reaction to catalyze the transesterification reaction of at least one of alcohol compounds and ester compounds with oxalic acid ester to synthesize alkyl oxalate.

10. The use according to claim 9, characterized in that: The alcohol compound is selected from at least one of ethanol and butanol.

11. The use according to claim 9, characterized in that: The ester compound is selected from at least one of dimethyl oxalate, diethyl oxalate and dibutyl oxalate.

12. The use according to claim 9, characterized in that: The alkyl oxalate is selected from at least one of diethyl oxalate, ethyl methyl oxalate, dibutyl oxalate and methyl butyl oxalate.

13. The use according to claim 9, characterized in that: The weight ratio of the heterogeneous catalyst used in the transesterification reaction to the oxalate is 0.001-0.1:

1.

14. The use according to claim 1, characterized in that: The conditions of the transesterification reaction are: reaction temperature 60-140° C., reaction pressure 10-50 KPa.