A sulfur-containing carbon nitride material and its preparation method and application in photocatalytic hydrogen production

The preparation of sulfur-containing carbon nitride materials by calcining tripolymer thiocyanic acid and melamine under an inert atmosphere has solved the problems of complex and high cost in the existing technology, and achieved high-efficiency photocatalytic hydrogen production performance and good cycle stability .

CN116371441BActive Publication Date: 2024-11-05WUHAN INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310168130.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-22
Publication Date
2024-11-05
Estimated Expiration
2043-02-22

AI Technical Summary

Technical Problem

The existing sulfur-doped carbon nitride photocatalysts are complex and costly, and it is difficult to meet the simplicity and low energy consumption requirements in the field of photocatalytic hydrogen production.

Method used

The sulfur-containing carbon nitride material is prepared by indirect contact calcining under an inert atmosphere, simplifying the process flow and reducing energy consumption.

Benefits of technology

The prepared sulfur-containing carbon nitride material has a large specific surface area, high photocatalytic hydrogen production activity, good cycle stability and safety, and is suitable for photocatalytic hydrogen production applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116371441B_ABST
    Figure CN116371441B_ABST
Patent Text Reader

Abstract

The present invention relates to a sulfur-containing carbon nitride material and a preparation method thereof and application in photocatalytic hydrogen production. The sulfur-containing carbon nitride material is obtained by calcining thiocyanate in an inert atmosphere without direct contact with melamine. The sulfur-containing carbon nitride material provided by the present invention has a large specific surface area, strong light absorption capacity, high photocatalytic hydrogen production activity, and excellent cycle stability, and has good application prospects for photocatalytic hydrogen production. The preparation method thereof has good safety, simple synthetic raw materials, and few operation steps. The sulfur-containing carbon nitride material can be obtained by calcining two raw materials weighed in proportion in two porcelain boats placed in a tubular furnace and kept at a certain distance in one step, and the cost is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of catalysts of nitrogen compounds containing sulfur elements, and specifically relates to a sulfur-containing carbon nitride material and a preparation method thereof and application in photocatalytic hydrogen production. Background Art

[0002] It is particularly important to develop resources rationally. The water resources on the earth are abundant, and the solar energy is inexhaustible, so using solar energy to decompose water to produce hydrogen is one of the key ways to solve the energy problem.

[0003] Photocatalytic hydrogen production technology converts solar energy into hydrogen energy. It is a low-cost, environmentally friendly and pollution-free technology with mild reaction conditions and a wide range of applications. It has a very broad development prospect. Photocatalytic hydrogen production technology requires the catalytic action of photocatalysts. In recent decades, researchers have mainly focused on the research of semiconductor photocatalytic materials of oxides. Such materials are generally soluble in acid and alkali reagents and are therefore difficult to modify, which limits their application development.

[0004] In recent years, non-metallic semiconductor photocatalyst graphene carbon nitride (g-C3N4) materials have come into people's attention. 2 The hybridized C and N atoms form a certain conjugated system, which gives it excellent thermal stability, chemical stability and other properties. In addition, g-C3N4 can also absorb visible light, and the preparation process is simple and low-cost. It can catalyze the decomposition of water to produce hydrogen under visible light irradiation and triethanolamine as a hole scavenger. There is room for great development in the field of photocatalytic hydrogen production. However, g-C3N4 has disadvantages such as low specific surface area, wide bandgap of about 2.72eV, easy recombination of photogenerated electrons and holes, and low conductivity, which lead to limited catalytic activity, so it needs to be modified. At present, it can be modified by doping (metals, non-metals, precious metals, etc.),

[0005] The g-C3N4 is modified by means of morphology control, semiconductor composite modification and loading of co-catalysts, and the above-mentioned shortcomings are improved by regulating the material composition or changing the properties such as specific surface area, thereby improving the photocatalytic activity. When g-C3N4 is sulfur-doped, by regulating the composition, electronic structure and thickness of g-C3N4, the specific surface area can be increased while causing certain defects, exposing more active sites, and improving the performance of photocatalytic hydrogen production. Patent CN111185216A discloses a scheme of mixing melamine and thiocyanate in a solvent, then performing a hydrothermal reaction to obtain a solid tubular composite, and then calcining with urea to obtain a hollow tubular sulfur-doped carbon nitride / graphite phase carbon nitride homojunction photocatalyst. Patent CN107930667A discloses a method for preparing sulfur-doped carbon nitride by dissolving melamine and thiocyanate in hot water respectively, mixing them evenly, and calcining them after a hydrothermal reaction. These disclosed preparation methods have complicated steps, require post-processing, and are relatively costly.

[0006] Therefore, it is necessary to develop some experimental methods with simpler operation, lower energy consumption cost and better effect, so as to apply them to the field of photocatalytic hydrogen production. The present invention uses only two raw materials, thiocyanate and melamine, which are weighed separately without direct contact and directly calcined in a tubular furnace to obtain a sulfur-containing carbon nitride material. The operation is simple, the energy consumption is low, and the prepared sulfur-containing carbon nitride material has good photocurrent responsiveness, a hydrogen production rate of 165.4 μmol / h, and good cyclic hydrogen production stability. Summary of the invention

[0007] The technical problem to be solved by the present invention is to provide a sulfur-containing carbon nitride material and a preparation method thereof and application in photocatalytic hydrogen production in view of the above-mentioned deficiencies in the prior art. The sulfur-containing carbon nitride material has a large specific surface area, is sensitive to visible light response, has high photocatalytic hydrogen production activity, and the preparation method is simple and easy to operate with good repeatability.

[0008] In order to solve the above technical problems, the technical solution provided by the present invention is:

[0009] Provided is a sulfur-containing carbon nitride material, which is obtained by calcining thiocyanuric acid in an inert atmosphere without direct contact with melamine.

[0010] According to the above scheme, the specific surface area of ​​the sulfur-containing carbon nitride material is 50 to 150 m 2 / g.

[0011] The present invention also provides a method for preparing the above sulfur-containing carbon nitride material, the specific steps of which are as follows:

[0012] 1) Weigh thiocyanuric acid and melamine in proportion and set aside;

[0013] 2) Spread thiocyanate evenly on the surface of porcelain boat No. 1, spread melamine evenly on the surface of porcelain boat No. 2, then put porcelain boat No. 1 in the middle of the constant temperature area of ​​the tubular furnace, put porcelain boat No. 2 in the tubular furnace near the air inlet, introduce inert gas into the tubular furnace through the air inlet, heat and calcine, cool to room temperature with the furnace, collect the sample in porcelain boat No. 1 and grind it to obtain sulfur-containing carbon nitride material.

[0014] According to the above scheme, the purity of thiocyanuric acid in step 1) is ≥ 95wt%, and the purity of melamine is ≥

[0015] 99wt%.

[0016] According to the above scheme, the mass ratio of thiocyanuric acid to melamine in step 1) is 0.5 to 2:1.

[0017] According to the above scheme, in step 2), the center distance between porcelain boat No. 1 and porcelain boat No. 2 is 10 to 20 cm.

[0018] According to the above scheme, the inert atmosphere in step 2) is nitrogen or argon, the gas purity is above 99.99 vol%, and the gas flow rate is 60-100 mL / min.

[0019] According to the above scheme, the calcination process conditions in step 2) are: heating to 500-600°C at a heating rate of 5-15°C / min at room temperature and keeping warm for 3-5h.

[0020] The present invention also includes the use of the above sulfur-containing carbon nitride material in photocatalytic hydrogen production.

[0021] The present invention calcines thiocyanuric acid and melamine in an inert atmosphere in a non-direct contact state to obtain a sulfur-containing carbon nitride material. The thiocyanuric acid is a precursor. During the calcination process, melamine generates ammonia gas that flows on the surface of the thiocyanuric acid, and has a certain stripping effect during the polymerization of thiocyanuric acid to produce sulfur-containing carbon nitride, thereby generating a sulfur-containing carbon nitride material with high crystallinity and certain defects. Test results show that the sulfur-containing carbon nitride material has excellent photocatalytic hydrogen production performance.

[0022] The beneficial effects of the present invention are as follows: 1. The sulfur-containing carbon nitride material provided by the present invention has a large specific surface area, strong light absorption capacity, high photocatalytic hydrogen production activity, and excellent cycle stability, and has good application prospects for photocatalytic hydrogen production. 2. The present invention uses only two raw materials, thiocyanate and melamine, and indirectly uses melamine to generate ammonia for stripping, and does not directly use a large amount of ammonia gas for direct contact, which reduces the danger and has good safety. The synthetic raw materials are simple and the operation steps are few. The two raw materials weighed in proportion are placed in two porcelain boats placed in a tubular furnace and kept at a certain distance, and the sulfur-containing carbon nitride material can be obtained by calcining in one step, which is low in cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 A comparison chart of the photocatalytic hydrogen production effects of the sulfur-containing carbon nitride materials prepared in Comparative Example 1 and Examples 1-5 of the present invention;

[0024] Figure 2 The photocurrent test graph of the sulfur-containing carbon nitride material prepared in Comparative Example 1 and Examples 1-3;

[0025] Figure 3 The photocurrent test graphs of the sulfur-containing carbon nitride materials prepared in Comparative Example 1 and Examples 1, 4, and 5;

[0026] Figure 4 This is a comparison diagram of hydrogen production of the sulfur-containing carbon nitride material prepared in Example 4 under different wavelengths;

[0027] Figure 5 This is a test chart of the stability of the sulfur-containing carbon nitride material prepared in Example 4 for continuous 20 hours of photocatalytic hydrogen production cycle;

[0028] Figure 6 XRD spectra of sulfur-containing carbon nitride materials prepared in Comparative Example 1 and Examples 1-3;

[0029] Figure 7 XRD spectra of sulfur-containing carbon nitride materials prepared in Comparative Example 1 and Examples 1, 4, and 5;

[0030] Figure 8 The nitrogen isothermal adsorption-desorption curves of the sulfur-containing carbon nitride materials prepared in Comparative Example 1 and Examples 1-3;

[0031] Fig. 9 The nitrogen isothermal adsorption-desorption curves of the sulfur-containing carbon nitride materials prepared in Comparative Example 1 and Examples 1, 4, and 5;

[0032] Fig.10 The pore size distribution diagram of the sulfur-containing carbon nitride materials prepared in Comparative Example 1 and Examples 1-3;

[0033] Fig.11 The pore size distribution diagram of the sulfur-containing carbon nitride materials prepared in Comparative Example 1 and Examples 1, 4, and 5;

[0034] Fig.12 The impedance diagrams of the sulfur-containing carbon nitride materials prepared in Comparative Example 1 and Examples 1-3;

[0035] Fig.13 Impedance diagrams of the sulfur-containing carbon nitride materials prepared in Comparative Example 1 and Examples 1, 4, and 5. DETAILED DESCRIPTION

[0036] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below with reference to the accompanying drawings.

[0037] Comparative Example 1

[0038] A sulfur-containing carbon nitride material, the specific preparation method is as follows:

[0039] 1) Weigh 2 g of thiocyanuric acid (purity 95 wt%) and set aside;

[0040] 2) Spread the thiocyanate solid on a porcelain boat, place it in the middle of the constant temperature zone of a tubular furnace, introduce nitrogen (99.99 vol%) into the tubular furnace, set the nitrogen flow rate to 80 mL / min, then heat the boat to 550°C at a heating rate of 10°C / min at room temperature for calcination for 3 h. After naturally cooling to room temperature, grind into powder to obtain sulfur-containing carbon nitride material (denoted as SCN).

[0041] Example 1

[0042] A sulfur-containing carbon nitride material, the specific preparation method is as follows:

[0043] 1) Weigh 2 g of thiocyanuric acid (purity 95 wt%) and 3 g of melamine (purity 99 wt%) and set aside;

[0044] 2) Spread thiocyanate on porcelain boat No. 1, and place it in the middle of the constant temperature area of ​​the tubular furnace; spread melamine on porcelain boat No. 2, and place it in the tubular furnace near the air inlet. The center distance between porcelain boat No. 1 and porcelain boat No. 2 is 15 cm. Nitrogen (99.99 vol%) is introduced into the tubular furnace, and the nitrogen flow rate is set to 80 mL / min. Then, the temperature is increased to 550°C at a heating rate of 10°C / min at room temperature for calcination. The calcination time is 3 h. After naturally cooling to room temperature, the mixture is ground into powder to obtain sulfur-containing carbon nitride material (denoted as A).

[0045] Example 2

[0046] A sulfur-containing carbon nitride material, the preparation method of which is similar to that of Example 1, except that in step 2) the nitrogen gas flow rate is set to 100 mL / min, and the obtained product is recorded as B.

[0047] Example 3

[0048] A sulfur-containing carbon nitride material, the preparation method of which is similar to that of Example 1, except that in step 2), the nitrogen gas flow rate is set to 60 mL / min, and the obtained product is recorded as C.

[0049] Example 4

[0050] A sulfur-containing carbon nitride material, the preparation method of which is similar to that of Example 1, except that in step 2), the center distance between porcelain boat No. 1 and porcelain boat No. 2 is 10 cm, and the obtained product is recorded as D.

[0051] Example 5

[0052] A sulfur-containing carbon nitride material, the preparation method of which is similar to that of Example 1, except that in step 2), the center distance between porcelain boat No. 1 and porcelain boat No. 2 is 20 cm, and the obtained product is recorded as E.

[0053] Photocatalytic hydrogen production performance test: 20 mg of the sulfur-containing carbon nitride material prepared in Comparative Example 1 and Examples 1-5 were respectively added to 6 portions of 100 mL of deionized water solution containing 10 wt% triethanolamine, and 0.33 mL of H2PtCl4 solution was added to each solution (based on the mass fraction of 20 mg of photocatalyst loaded Pt being 3 wt%, H2PtCl4 plays the role of a co-catalyst in the photocatalytic system). After the mixed solution was ultrasonically dispersed for 30 minutes, it was illuminated in a photoreactor (Labsolar-6A, the light source was a 300 W xenon lamp with a 420 nm cutoff filter) for 4 hours for testing. The visible light photocatalytic hydrogen production effect comparison of the sulfur-containing carbon nitride materials prepared in Comparative Example 1 and Examples 1-5 is shown in the figure below. Figure 1 As shown, it can be seen that the H2 production rates of the sulfur-containing carbon nitride materials prepared in Comparative Example 1 and Examples 1-5 are: SCN 62.9μmol / h, A 144.9μmol / h, B 127.1μmol / h, C108.1μmol / h, D 165.4μmol / h, E 119.9μmol / h, among which the photocatalytic hydrogen production rates of A to E are higher than SCN, and the photocatalytic hydrogen production rate of D is the highest. Photocurrent test: The sulfur-containing carbon nitride materials prepared in Comparative Example 1 and Examples 1-5 were respectively prepared into 1.0g / L aqueous dispersions, and 8μL of each aqueous dispersion was dripped onto the surface of a glassy carbon electrode (3mm in diameter). A Chenhua electrochemical workstation was used to place the photocurrent test in a 0.5mol / L Na2SO4 solution under illumination conditions of >420nm. The photocurrent can reflect the photocatalytic performance of the material. The higher the photocurrent, the more it can promote the separation of photogenerated carriers, and the better the photocatalytic effect of the material. The photocurrent test graphs of the sulfur-containing carbon nitride materials prepared in Comparative Example 1 and Examples 1-3 are as follows: Figure 2 As shown, the photocurrent test graphs of the sulfur-containing carbon nitride materials prepared in Comparative Example 1 and Examples 1, 4, and 5 are as follows Figure 3 As shown, the test results show that SCN has the smallest photocurrent. By comparing Examples 1-3, it can be seen that when the porcelain boat distance is kept at 15 cm and the gas flow rate is adjusted, the photocurrent of A prepared in Example 1 is the largest. By comparing Examples 1, 4, and 5, it can be seen that when the gas flow rate is kept at 80 mL / min and the porcelain boat distance is adjusted, the photocurrent of D prepared in Example 4 is the largest.

[0054] Figure 4 This is a comparison chart of hydrogen production under different wavelengths of the sulfur-containing carbon nitride material prepared in Example 4, wherein several portions of photocatalyst solutions were prepared, and the preparation method of each portion of the photocatalyst solution was as follows: 20 mg of the sulfur-containing carbon nitride material D prepared in Example 4 was added to 100 mL of a deionized water solution containing 10 wt% triethanolamine, and 0.33 mL of H2PtCl4 solution (based on the mass fraction of 20 mg of photocatalyst loaded Pt being 3 wt%) was added, and the mixed solution was ultrasonically dispersed for 30 minutes to obtain the result. The prepared photocatalyst solution was placed in a photoreactor (Labsolar-6A, the light source was a 300W xenon lamp) and illuminated for 4 hours to conduct a hydrogen production test, and the wavelengths of the light were 365 nm, 420 nm, 450 nm, 500 nm, 550 nm, and cutoff 420 nm (i.e., >420 nm), respectively. Figure 4 It can be seen that there is a certain hydrogen production effect under the illumination of each wavelength.

[0055] Test the cyclic stability of catalytic hydrogen production by sulfur-containing carbon nitride material: 20 mg of sulfur-containing carbon nitride material D prepared in Example 4 was added to 100 mL of deionized water solution containing 10 wt% triethanolamine, and 0.33 mL of H2PtCl4 (based on the mass fraction of 3 wt% of Pt loaded on 20 mg of photocatalyst) was added. After the mixed solution was ultrasonically dispersed for 30 minutes, a cyclic hydrogen production stability test was carried out in a photoreactor (Labsolar-6A, the light source was a 300 W xenon lamp with a 420 nm cutoff filter). The test was stopped every 4 hours, and 5 cycles were tested for a total of 20 hours. The cyclic stability test of the sulfur-containing carbon nitride material prepared in Example 4 for continuous 20 hours of photocatalytic hydrogen production is shown in the figure. Figure 5 As shown in the figure, it is found that the sulfur-containing carbon nitride material has good cycle stability.

[0056] Figure 6 The XRD spectra of the sulfur-containing carbon nitride materials prepared in Comparative Example 1 and Examples 1-3 are shown in FIG. Figure 7 The XRD spectra of the sulfur-containing carbon nitride materials prepared in Comparative Example 1 and Examples 1, 4, and 5 are shown in FIG. Figure 6 , Figure 7It can be seen that there are two main peaks in the XRD spectrum of the sample. The peak of the (100) plane corresponding to about 13° represents the intralayer structural stacking of the material unit ring. Another peak at about 27.1° corresponds to the interlayer stacking of the conjugated aromatic unit, which is attributed to the (002) plane. Comparing the positions and intensities of the corresponding peaks, the corresponding (002) plane peak intensity of SCN is the lowest, and the peak intensity of the materials prepared in Examples 1-5 is improved, indicating that the sulfur-containing carbon nitride material synthesized by introducing melamine as a source of ammonia has a more ordered structure and a higher degree of crystallinity. The (002) crystal planes of the materials prepared in Examples 1-5 have all moved to a certain extent, resulting in a smaller interlayer spacing and fewer migration paths for carriers, thereby improving the separation efficiency of carriers.

[0057] Figure 8 The nitrogen isothermal adsorption-desorption curves of the sulfur-containing carbon nitride materials prepared in Comparative Example 1 and Examples 1-3 are shown in FIG. Fig. 9 The nitrogen isothermal adsorption-desorption curves of the sulfur-containing carbon nitride materials prepared in Comparative Example 1 and Examples 1, 4, and 5 are shown in FIG. Fig.10 is a pore size distribution diagram of the sulfur-containing carbon nitride materials prepared in Comparative Example 1 and Examples 1-3, Fig.11 The pore size distribution diagram of the sulfur-containing carbon nitride material prepared in Comparative Example 1 and Examples 1, 4, and 5. Figure 8 , Fig. 9 It can be seen that the typical N2 adsorption-desorption isotherms show that this type of sulfur-containing carbon nitride material samples have a mesoporous structure, among which sample D has the largest specific surface area, reaching 135.75 m 2 / g, the large specific surface area can expose more active sites, thereby improving the photocatalytic hydrogen production activity. Fig.10 , Fig.11 The pore size distribution diagram shows that the sulfur-containing carbon nitride material sample contains mesopores.

[0058] Fig.12 The impedance diagrams of the sulfur-containing carbon nitride materials prepared in Comparative Example 1 and Examples 1-3 are shown in FIG. Fig.13 The impedance diagrams of the sulfur-containing carbon nitride materials prepared in Comparative Example 1 and Examples 1, 4, and 5 are shown in FIG. Fig.12 , Fig.13 It can be seen that compared with the comparative example SCN, the sulfur-containing carbon nitride materials prepared in Examples 1-5 have a smaller semicircle, and the semicircle of sample D is the smallest, which indicates that SCN has the highest carrier migration resistance, and the carrier migration resistance of D is relatively the smallest, with high migration efficiency and stronger electron transmission ability.

Claims

1. A sulfur-containing carbon nitride material, characterized in that: It is obtained by calcining thiocyanuric acid in an inert atmosphere without direct contact with melamine; The specific steps of its preparation method are as follows: 1) Weigh thiocyanuric acid and melamine in proportion, wherein the mass ratio of thiocyanuric acid to melamine is 0.5-2:1, and set aside; 2) Spread thiocyanate evenly on the surface of porcelain boat No. 1, spread melamine evenly on the surface of porcelain boat No. 2, then put porcelain boat No. 1 in the middle of the constant temperature area of ​​the tubular furnace, put porcelain boat No. 2 in the tubular furnace near the air inlet, the center distance between porcelain boat No. 1 and porcelain boat No. 2 is 10-20 cm, introduce inert gas into the tubular furnace through the air inlet, heat and calcine, the calcination process conditions are: heat up to 500-600°C at a heating rate of 5-15°C / min at room temperature, keep warm for 3-5h, cool to room temperature with the furnace, collect the sample in porcelain boat No. 1 and grind to obtain sulfur-containing carbon nitride material.

2. The sulfur-containing carbon nitride material according to claim 1, characterized in that: The specific surface area of ​​the sulfur-containing carbon nitride material is 50-150m 2 / g.

3. A method for preparing the sulfur-containing carbon nitride material according to claim 1 or 2, characterized in that: The specific steps are as follows: 1) Weigh thiocyanuric acid and melamine in proportion and set aside; 2) Spread thiocyanate evenly on the surface of porcelain boat No. 1, spread melamine evenly on the surface of porcelain boat No. 2, then put porcelain boat No. 1 in the middle of the constant temperature area of ​​the tubular furnace, put porcelain boat No. 2 in the tubular furnace near the air inlet, introduce inert gas into the tubular furnace through the air inlet, heat and calcine, cool to room temperature with the furnace, collect the sample in porcelain boat No. 1 and grind it to obtain sulfur-containing carbon nitride material.

4. The method for preparing the sulfur-containing carbon nitride material according to claim 3, characterized in that: Step 1) The purity of thiocyanuric acid is ≥ 95wt%, and the purity of melamine is ≥ 99wt%.

5. The method for preparing the sulfur-containing carbon nitride material according to claim 3, characterized in that: Step 2) The inert gas is nitrogen or argon, the gas purity is above 99.99 vol%, and the gas flow rate is 60-100 mL / min.

6. Use of the sulfur-containing carbon nitride material according to claim 1 or 2 in photocatalytic hydrogen production.