Synthesis and application of a heterocyclic heterogeneous catalyst
By introducing heterocyclic or heteroatom-substituted quaternary phosphonium ionic liquids and composite resin materials into the catalyst, the problems of separation and short life of the catalyst and product are solved, efficient and stable conversion of CO2 and epoxides is achieved, and production costs are reduced. And the synthesis efficiency of cyclic carbonate is improved.
Patent Information
- Application Number
- CN202310295425.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-03-24
AI Technical Summary
Existing catalysts have problems in the cycloaddition reaction between CO2 and epoxides, such as difficulty in separating the catalyst and the product, short catalyst life, and high cost of use. Moreover, the active components of the supported ionic liquid catalyst are difficult to determine, and the overall catalytic activity needs to be improved.
Design and develop composite materials to support heterocyclic or heteroatom-substituted quaternary phosphonium ionic liquid catalysts, enhance the nucleophilic-electrophilic effect of quaternary phosphonium ions through heterocyclic rings or heteroatoms, and synthesize composite resin materials to improve loading rate and catalytic activity. Achieve efficient and stable conversion of CO2 and epoxy compounds.
It achieves the effects of high catalyst activity, low cost, long service life, easy product separation and catalyst recovery, and improves the synthesis efficiency and product quality of cyclic carbonate.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure QLYQS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalytic cyclic compounds, and in particular to a method for catalyzing the synthesis of cyclic carbonates based on composite material-supported heterocyclic ionic liquids. Background Art
[0002] Carbon dioxide (CO2) is a greenhouse gas and an inexhaustible C1 resource. Its effective fixation and conversion has become one of the most challenging issues of this century, and the synthesis of cyclic carbonates using CO2 is a good fixation and conversion pathway. Cyclic carbonates are a multi-purpose and important chemical product with low toxicity, biodegradability, and high boiling point. They are widely used in power battery electrolytes and can also be used as organic synthesis intermediates to produce dimethyl carbonate, ethylene glycol and other products for use in polycarbonate, medicine, coatings and other fields.
[0003] At present, the catalyst used for the cycloaddition reaction of CO2 and epoxide mainly includes metal organic framework (MOF) (CN111454434A, CN105481821A), transition metal complex (CN107827857A, CN107827858A, CN111215148A) and composite catalyst (CN111393402A, CN107715918B) and other catalysts, although some catalysts have higher catalytic activity, it is necessary to use highly toxic organic solvents, which cause difficulties in the separation and purification of products and product quality. At the same time, the above-mentioned homogeneous catalysts are difficult to separate from the catalyst and the product, and the catalyst life is short, resulting in high cost of use, which restricts its further industrial application.
[0004] Ionic liquid (CN111362901A) has received extensive attention as a new medium. Among them, supported ionic liquid as a heterogeneous catalyst can effectively solve the separation problem of catalyst and product. Supported ionic liquid catalyst is divided into physical load and chemical load according to its loading mode. Physical load adopts physical adsorption mode, and catalyst stability is relatively poor and easy to lose, while chemical load is connected by chemical bonds formed between ionic liquid and carrier, while ensuring certain catalytic activity, it has higher stability. CN107537564B discloses a heterogeneous catalyst for catalyzing CO2 and epoxy compounds to prepare cyclic carbonate, the catalyst is formed by copolymerization of organic phosphine ligand containing olefin group and quaternary phosphonium salt containing olefin group and Lewis acid metal salt coordination, the catalyst obtained by the method can form a dual activation mode of multifunctional properties, but the active components of its copolymer are difficult to determine and the addition of metal salt increases the cost of the catalyst. CN104974128A discloses a method for preparing cyclic carbonate using a supported catalyst. The catalyst supports methoxyphenylphosphine, but the article does not further measure the loading amount and loading rate of its active components, and the overall catalytic activity needs to be improved.
[0005] The present invention designs and develops a composite material loaded with heterocyclic or heteroatom-substituted quaternary phosphonium ionic liquid to catalyze the synthesis of cyclic carbonates from CO2, and utilizes heterocyclic or heteroatom-substituted quaternary phosphonium ionic liquid to enhance the nucleophilic-electrophilic effect. At the same time, the designed and synthesized composite resin material enhances the thermal and mechanical properties of the resin, has a high loading rate and good activity, and is used to catalyze the synthesis of cyclic carbonates from CO2 and epoxy compounds, thereby achieving efficient and stable conversion of carbonylation reactions. Summary of the invention
[0006] The object of the present invention is to provide a method for preparing cyclic carbonate by catalyzing the cycloaddition of epoxy compound and carbon dioxide using a composite material supported heterocyclic or heteroatom-substituted quaternary phosphonium ionic liquid catalyst.
[0007] The reaction formula of the present invention is:
[0008]
[0009] When R2 represents H, the structure of the epoxy compound used in the general formula is:
[0010]
[0011] Wherein m=1, 2, 3 or 4, n=0, 1, 2, 3 or 4.
[0012] When R2 is not H, the structure of the epoxy compound used is:
[0013]
[0014] A method for preparing cyclic carbonate using supported ionic liquids is characterized in that a composite material supported heterocyclic or heteroatom-substituted quaternary phosphonium ionic liquid is used as a catalyst, the amount of the catalyst is 0.1-2.0 mol% of the epoxy compound (calculated based on the content of the ionic liquid), and the corresponding cyclic carbonate is synthesized by catalyzing the cycloaddition of the epoxy compound and carbon dioxide under the conditions of a reaction pressure of 0.1-10.0 MPa, a reaction temperature of 50-150° C., and a reaction time of 0.5-10 hours. The synthesis method has the characteristics of high catalyst activity, low cost, long service life, easy product separation and catalyst recovery, etc.
[0015] The structure of the composite material loaded with ionic liquid involved in the present invention is as follows:
[0016]
[0017] Wherein, n=0-6, R1, R2 and R3 are groups substituted by one, two or three of the following functional groups at the same time: H, F, Cl, Br, I, P(CH3)2 or N(CH3)2;
[0018] The preferred cationic structure is as follows,
[0019]
[0020]
[0021] X is any of the following anions:
[0022]
[0023] Wherein R is any one of a C1-C6 alkyl group, a C4-C10 cycloalkyl group and a C4-C10 aryl group.
[0024] According to claim 1, the carrier is an organic polymer, such as any one of carbon material composite polystyrene, chitosan, and cellulose.
[0025] The supported quaternary phosphonium salt catalyst is prepared according to the following steps:
[0026] 1) Pretreatment of the carrier: Add 40g of anhydrous lithium chloride to a flask containing 250mL of dimethylacetamide, then stir at 70-100°C for 2h to dissolve it into a homogeneous solution, cool to room temperature, add 10g of cellulose, heat to 70-100°C and stir overnight, then cool to room temperature and stir until dissolved. Add two times the molar equivalent of a mixed solution of triethylamine and dimethylacetamide in an equal volume ratio to the above solution, cool to 8°C, drop a molar equivalent of p-toluenesulfonyl chloride and 30-60mL of dimethylacetamide mixed solution, and stir the reaction solution for 20-40h. Slowly pour the reaction mixture into a large amount of ice water, and the product precipitates. Stir, filter, wash with a large amount of ethanol, and vacuum dry at 30-60°C to obtain the product cellulose p-toluenesulfonate;
[0027] 2) Preparation of ionic liquid: In a 250mL four-necked flask, add 5-10g 4-chloro-1-butanol and 50-100mL acetonitrile, protect with nitrogen, slowly add two times the molar equivalent of tertiary phosphine compound when the temperature rises to 40-50°C, then continue to heat to 60-90°C and stir to react for 24-48h. After stopping the reaction, rotary evaporation is performed to obtain a homogeneous ionic liquid, which is then washed with ethyl acetate until there is no tertiary phosphine compound, and vacuum dried at 50-75°C for 12-24h to obtain a quaternary phosphonium ionic liquid;
[0028] 3) Preparation of loaded chlorinated ionic liquid: In a 250mL four-necked flask, add 10-20g of the modified cellulose carrier obtained in step 3), 50-100mL of acetonitrile and two times the molar equivalent of the ionic liquid obtained in step 2), and heat to 60-90°C under nitrogen protection and stir for 24-48h. After stopping the reaction, rotary evaporation is performed to obtain a homogeneous ionic liquid, which is then washed with ethyl acetate and vacuum dried at 50-75°C for 12-24h to obtain a quaternary phosphonium ionic liquid;
[0029] 4) Anion exchange of quaternary phosphonium-supported ionic liquid: 10 g of the supported catalyst obtained in step 3) and two times the molar equivalent of KX were added to a three-necked flask, and then 150 ml of methanol was added, nitrogen sealed, and the mixture in the flask was heated to 75°C with a constant temperature heating stirrer, and refluxed for 24 hours. After the reaction was completed, the mixture was allowed to stand and cool to room temperature, the supernatant was removed, the supported catalyst was taken out, and then washed with deionized water until the clear liquid did not contain inorganic salt KX, and vacuum dried at 50-75°C for 12-24 hours to obtain the corresponding anionic quaternary phosphonium-supported catalyst.
[0030] 5) Determination of the loading amount of quaternary phosphonium-loaded ionic liquid: Take the ionic liquid obtained in step 3) or 4) and perform XRF determination on the P element content. The loading amount is calculated to be in the range of 88%-100%.
[0031] Preferably, the cyclic carbonate described in the present invention is selected from at least one or a combination of two of ethylene carbonate, propylene carbonate, epoxy chloropropylene, epoxy cyclohexene carbonate, and phenylene carbonate.
[0032] Preferably, the molar ratio of the added amount of ionic liquid to the epoxy compound is 0.5-1.5%, for example, it can be 0.1%, 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0%, 5.5%, 6.0%, 6.5%, 7.0%, 7.5%, 8.0%, 8.5%, 9.0%, 9.5%, 10.0%, etc., preferably 0.5-1.5%.
[0033] Preferably, the operating pressure of the catalytic reaction is 1-5 MPa, for example, it can be 0.1 MPa, 0.5 MPa, 1.0 MPa, 1.5 MPa, 2.0 MPa, 2.5 MPa, 3.0 MPa, 3.5 MPa, 4.0 MPa, 4.5 MPa, 5.0 MPa, 5.5 MPa, 6.0 MPa, 6.5 MPa, 7.0 MPa, 7.5 MPa, 8.0 MPa, 8.5 MPa, 9.0 MPa, 9.5 MPa or 10.0 MPa, etc., preferably 1-5 MPa.
[0034] Preferably, the operating temperature of the catalytic reaction is 80-160°C, for example, it can be 60°C, 70°C, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 185°C, 190°C, 195°C, 200°C, 205°C, 210°C, 215°C or 220°C, etc., preferably 80-160°C. Preferably, the reaction time of the catalytic reaction is 2-5 h, for example, it can be 0.25 h, 0.5 h, 1.0 h, 1.5 h, 2.0 h, 2.5 h, 3.0 h, 3.5 h, 4.0 h, 4.5 h, 5.0 h, 5.5 h, 6.0 h, 8.0 h, 10.0 h, 12.0 h, 14.0 h, 16.0 h, 18.0 h, 20.0 h, 22.0 h or 24.0 h, etc., preferably 2-5 h.
[0035] After the reaction is completed, stirring is stopped, and the temperature in the reactor is cooled to room temperature before the reactor is disassembled. The upper liquid is sucked out to obtain the desired cyclic carbonate product. DETAILED DESCRIPTION
[0036] The present invention is described with the following embodiments, but the present invention is not limited to the following embodiments, and variations are included in the technical scope of the present invention without departing from the scope of the above-mentioned purpose.
[0037] Example 1
[0038]
[0039] Implementation method: In a 15 ml stainless steel autoclave, cellulose-supported triphenylphosphonium bromide (structural formula The reaction mixture was added with 0.3 g (0.5 mmol in terms of the content of ionic liquid, and the molar ratio to the epoxy compound is 0.5 mol%, the same below) and 7 ml propylene oxide (1a) (0.1 mol), and an appropriate amount of CO2 was charged at room temperature, and the vent valve of the reactor was closed; the reactor was placed in an automatic temperature-controlled heating furnace, and the pressure of the reactor was first adjusted to 1 MPa. In order to prevent the carbonylation reaction from being too intense in the initial stage, after the temperature reached the target temperature of 120°C, it was maintained for about 15 minutes, and the pressure of the reactor was adjusted to 2.5 MPa. The reaction was carried out at 120°C for 2 hours. After the reaction was completed, the reactor was cooled to room temperature, and unreacted CO2 was slowly released. After the catalyst was separated by filtration, a trace amount of the reaction solution was taken out and the conversion rate and selectivity were analyzed using Agilent 8890. The selectivity of the product propylene carbonate was 99.7%, and the conversion rate was 99.8%.
[0040] Example 2
[0041] The same as in Example 1, the catalyst used is cellulose-supported tri(2-furyl)phosphonium chloride (in the structural formula, X=Cl) 0.12 g (about 0.5 mmol), and other conditions remained unchanged to obtain the product (2a) with a selectivity of 99.3% and a conversion rate of 99.5%.
[0042] Example 3
[0043] The same as Example 1, except that the catalyst used was 0.1 g (about 0.5 mmol) of cellulose-supported triphenylphosphonium chloride (where X=Cl, R=Ph) and other conditions remained unchanged, yielding (2a) with a selectivity of 99.7% and a conversion rate of 99.3%.
[0044] Example 4
[0045] The same as Example 1, except that the catalyst used was resin-supported triphenylphosphonium chloride, the additive was sodium phenolate, the temperature was 80° C., and other conditions remained unchanged, to obtain (2a) with a selectivity of 99.7% and a conversion rate of 99.4%.
[0046] Example 5
[0047] The same method as in Example 1 was used, except that the temperature was 80°C and other conditions remained unchanged, and (2a) was obtained with a selectivity of 99.7% and a conversion rate of 89.4%.
[0048] Example 6
[0049] The same method as in Example 1 was used, except that the temperature was 160° C. and other conditions remained unchanged, and (2a) was obtained with a selectivity of 99.7% and a conversion rate of 99.8%.
[0050] Example 7
[0051] The same as Example 1, the reaction time was 3.5 hours, and other factors remained unchanged, to obtain (2a) with a selectivity of 99.7% and a conversion rate of 95.5%.
[0052] Example 8
[0053] The same as Example 1, except that the reaction time was 5 hours and other factors remained unchanged, yielded (2a) with a selectivity of 99.7% and a conversion rate of 99.6%.
[0054] Example 9
[0055] The same as Example 1, except that the amount of catalyst was 0.6 g (molar ratio to the epoxide was 1.0 mol%), the reaction temperature was 140° C., the reaction time was 4.0 hours, and other conditions remained unchanged, yielding (2a) with a selectivity of 99.7% and a conversion rate of 99.7%.
[0056] Example 10
[0057] The same as Example 1, except that the amount of catalyst used was 1.2 g (1.5 mol % molar ratio to the epoxide compound), the reaction temperature was 120° C., the reaction time was 2.0 hours, and other conditions remained unchanged, yielding (2a) with a selectivity of 99.7% and a conversion rate of 99.9%.
[0058] Embodiment 11
[0059] The same as in Example 1, except that the reaction pressure was 1.0 MPa and other conditions remained unchanged, yielding (2a) with a selectivity of 99.7% and a conversion of 97.5%.
[0060] Example 12
[0061] The same as in Example 1, except that the reaction pressure was 5.0 MPa and other conditions remained unchanged, yielding (2a) with a selectivity of 99.6% and a conversion rate of 99.3%.
[0062] Example 13
[0063] As in Example 1, after the catalyst was used 8 times, (2a) was obtained with a selectivity of 99.4% and a conversion rate of 97.1%.
[0064] Embodiment 14
[0065]
[0066] The same method as in Example 1 was used, except that the epoxy compound used was ethylene oxide (1b), and other factors remained unchanged, to obtain (2b) with a selectivity of 99.2% and a conversion rate of 98.9%.
[0067] Embodiment 15
[0068] The same as Example 1, except that the epoxy compound used was ethylene oxide (1b), the amount of catalyst used was 0.6 g (the molar ratio to the epoxy compound was 1.0 mol%), and other conditions remained unchanged, to obtain (2b) with a selectivity of 99.5% and a conversion rate of 99.4%.
[0069] Example 16
[0070]
[0071] The same as Example 1, except that the epoxy compound used was epichlorohydrin (1c), and other conditions remained unchanged, to obtain (2c) with a selectivity of 93.7% and a conversion rate of 99.7%.
[0072] Embodiment 17
[0073]
[0074] The same method as in Example 1 was used, except that the epoxy compound used was styrene oxide (1d), and other conditions remained unchanged, to obtain (2d) with a selectivity of 98.0% and a conversion rate of 99.3%.
[0075] Embodiment 18
[0076]
[0077] The same as Example 1, except that the epoxy compound used was phenoxyethylene oxide (1e), and other conditions remained unchanged, to obtain (2e) with a selectivity of 97.8% and a conversion rate of 99.1%.
[0078] Embodiment 19
[0079]
[0080] The same as Example 1, except that the epoxy compound used was cyclohexene oxide (lf), the reaction temperature was 140°C, the pressure was 5 MPa, the time was 8 hours, and other conditions remained unchanged, to obtain (2f) with a selectivity of 99.0% and a conversion rate of 99.6%.
[0081] Embodiment 20
[0082]
[0083] Same as Example 1, except that the epoxy compound used was allyl ethylene oxide (1 g), the amount of catalyst used was 2.0 mol% of the epoxy compound, and other conditions remained unchanged, yielding (2 g) with a selectivity of 99.0% and a conversion rate of 99.5%.
Claims
1. A novel method for catalyzing CO by heterocyclic ionic liquid supported on composite materials 2 A method for synthesizing cyclic carbonates, It is characterized in that The catalytic reaction uses organic or inorganic composite materials loaded with heterocyclic or heteroatom-substituted quaternary phosphonium ionic liquids as catalysts, or adds trace additives to CO 2 As raw materials for synthesizing cyclic carbonates; The trace additives are metal inorganic and organic compounds; The structural formula of the used loaded heterocyclic or heteroatom substituted quaternary phosphonium ionic liquid is as follows: ; Wherein, n=0-6, R1, R2 and R3 are groups substituted by one, two or three of the following functional groups at the same time: ; The cation structure is as follows: , , , ; X is any of the following anions: , Wherein R is any one of a C1-C6 alkyl group, a C4-C10 cycloalkyl group and a C4-C10 aryl group.
2. The method according to claim 1, It is characterized in that The carrier is an organic or inorganic composite material.
3. The method according to claim 1, It is characterized in that The organic composite material is any one of cellulose, polyethylene glycol, lignin, chitosan, and carbon material composite polystyrene.
4. The method according to claim 1, It is characterized in that The inorganic compound is any one of MCM-41, SAB-15 and ZSM-5.
5. The method according to claim 1, It is characterized in that The amount of the trace additive added is 10-10000ppm.
6. The method according to claim 1, It is characterized in that The trace additive anion is any one of the following: 。 7. The method according to claim 1, It is characterized in that The general formula of the catalytic reaction is: , Wherein R is one of a substituted or unsubstituted C1-C20 straight chain or branched alkyl group, a substituted or unsubstituted C3-C20 cycloalkyl group, a substituted or unsubstituted C3-C20 heterocycloalkyl group, or a substituted or unsubstituted C6-C20 aryl group.
8. The method according to claim 1, It is characterized in that The molar ratio of the added amount of the catalyst ionic liquid to the epoxy compound is 0.1-10.0%.
9. The method according to claim 8, It is characterized in that The molar ratio of the added amount of the catalyst ionic liquid to the epoxy compound is 0.5-1.5%.
10. The method according to claim 7, It is characterized in that The epoxy compound is selected from at least one of ethylene oxide, propylene oxide, epichlorohydrin, cyclohexene oxide and styrene oxide.
11. The method according to claim 1, It is characterized in that The operating pressure of the catalytic reaction is 0.1-10 MPa.
12. The method according to claim 11, It is characterized in that The operating pressure of the catalytic reaction is 1-5 MPa.
13. The method according to claim 1, It is characterized in that The operating temperature of the catalytic reaction is 60-220°C.
14. The method according to claim 13, It is characterized in that The operating temperature of the catalytic reaction is 80-160°C.
15. The method according to claim 1, It is characterized in that The operation time of the catalytic reaction is 0.25-24h.
16. The method according to claim 15, It is characterized in that The operation time of the catalytic reaction is 2-5h.