A method for preparing iron-carbon particles and an enhanced artificial wetland phosphorus removal method based on the same

By using hydrated iron oxide-supported biochar particles in constructed wetlands, the problems of low adsorption capacity and secondary pollution of conventional substrates are solved, achieving efficient phosphorus removal and long-term operation effects, and reducing operating costs.

CN116393112BActive Publication Date: 2024-10-01SHANDONG UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310233398.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-10
Publication Date
2024-10-01
Estimated Expiration
2043-03-10

AI Technical Summary

Technical Problem

Among the existing constructed wetland phosphorus removal methods, the adsorption capacity of conventional substrates is low and can easily reach saturation, resulting in the need for frequent replacement of fillers, which affects the long-term operation of the wetland. The biological method is unstable, and the chemical method can easily cause secondary pollution.

Method used

Hydrated iron oxide-supported biochar particles are prepared as functional particles and fixed in the gaps between wetland fillers through the cyclic pulse method. The high specific surface area of ​​biochar and the strong binding properties of hydrated iron oxide are used to improve the adsorption capacity of phosphorus and avoid Packing replacement and secondary contamination.

Benefits of technology

It significantly improves the phosphorus removal efficiency of constructed wetlands, extends the service life of fillers, reduces operating costs, and maintains the permeability and environmental friendliness of wetland fillers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116393112B_ABST
    Figure CN116393112B_ABST
Patent Text Reader

Abstract

The present invention relates to an iron-carbon particle and a method for enhancing phosphorus removal in artificial wetlands based on the iron-carbon particle, and belongs to the field of ecological water treatment technology. Prepare hydrated iron oxide-loaded biochar particles as functional particles for phosphorus removal by adsorption, and use a cyclic pulse method to fix the functional particles in the gaps between wetland fillers, so as to enhance the phosphorus removal effect of artificial wetlands without destroying the matrix. The iron-carbon particles obtained by compounding biochar and hydrated iron oxide are fixed in the wetland matrix, have low hydraulic resistance, have no negative impact on the permeability coefficient of the wetland filler, and have a good effect of enhancing the phosphorus removal efficiency of the subsurface artificial wetland. The cyclic pulse method can effectively introduce functional particles into the artificial wetland system, and has the advantages of being non-destructive to the wetland matrix, simple operation, and strong operability. The present invention can improve the phosphorus adsorption capacity of the subsurface artificial wetland, is conducive to the stable and efficient removal of phosphorus in the subsurface artificial wetland system, and is suitable for the enhancement of the phosphorus adsorption function of the newly built wetland system and the upgrading and transformation of the existing wetland system.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ecological water treatment, and relates to an iron-carbon particle and a method for enhancing phosphorus removal in an artificial wetland based on the iron-carbon particle. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] Phosphorus entering the environment can cause serious ecological problems, including water quality problems and soil pollution. In addition, it can also lead to eutrophication of water bodies and the proliferation of harmful algae in aquatic environments. Currently, there are physical, biological, and chemical methods for phosphorus removal, and some methods have great defects in the process of promotion and application. Chemical methods have high requirements for water pH and are prone to secondary pollution; biological phosphorus removal effects are unstable and difficult to meet emission standards. Common physical methods such as adsorption use porous or large specific surface area solid substances to achieve the phosphorus removal process of sewage through the attachment of phosphorus to the surface of the adsorbent. The adsorption method for phosphorus removal is simple in process, reliable in operation, widely applicable, and environmentally friendly, and is widely used at home and abroad.

[0004] As an ecological treatment technology equipment, artificial wetland system uses natural processes to achieve wastewater treatment. The matrix is ​​the skeleton of the wetland system. Matrix adsorption is the main way for artificial wetlands to purify sewage, and it can effectively remove phosphorus. The matrix in artificial wetlands is also called filler. The type of filler affects the reoxygenation capacity, microbial species, activity, etc. of the wetland system, which in turn affects the wetland system's ability to remove phosphorus. Conventional matrices such as gravel and zeolite have low adsorption capacity and are easy to reach adsorption saturation, which needs to be solved urgently. When the existing filler reaches adsorption saturation, it needs to be manually excavated and replaced. This method will damage the wetland matrix and affect the long-term operation of the wetland. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing iron-carbon particles and a method for enhancing phosphorus removal in artificial wetlands based on the iron-carbon particles. Hydrous iron oxide-loaded biochar particles are prepared as functional particles for phosphorus removal by adsorption, and the functional particles are fixed in the gaps of wetland fillers by a cyclic pulse method, thereby enhancing the phosphorus removal effect of artificial wetlands without destroying the matrix.

[0006] In order to achieve the above object, the technical solution of the present invention is:

[0007] In a first aspect, a method for preparing iron-carbon particles comprises the following steps:

[0008] S1. calcining biomass materials at low temperature by anaerobically obtaining biochar, grinding the biochar into powder, and sieving and classifying the powder to obtain biochar particles;

[0009] S2. Add biochar particles and ferric nitrate nonahydrate (Fe(NO 3 ) 3 9H 2 O), stirring evenly and then maintaining the temperature and continuing to heat to generate hydrated iron oxide and load it on the biochar particles. After the reaction is completed, it is quickly cooled and the mixed solution is screened;

[0010] S3, washing the obtained product with distilled water and freeze-drying it to obtain the iron-carbon particles;

[0011] Among them, in S1, the biomass material is a porous biomass material;

[0012] The low-temperature anaerobic calcination temperature is 400-500°C;

[0013] The sieving and grading method is as follows: adding the ground biochar powder to deionized water to prepare a turbid solution, grading the ground biochar powder by sieving, obtaining three grades of biochar particles with particle sizes ranging from less than 10 μm, 10-70 μm, and greater than 70 μm, and drying;

[0014] In S2, the preheating temperature of distilled water is 75-80°C;

[0015] Adding ferric nitrate nonahydrate to make the concentration of ferric nitrate in the mixed solution 10-50 g / L; adding biochar particles and ferric nitrate nonahydrate to an iron-carbon ratio of 1:1-1:2;

[0016] The stirring method is: stirring at 200-300 r / min for 10-15 min;

[0017] After the stirring time is over, keep heating at the same temperature for 10-15 minutes.

[0018] The end of the reaction is characterized by: the color of the mixed solution changes from gold to dark reddish brown; at this point, the hydrated iron oxide is loaded on the biochar particles;

[0019] The rapid cooling method is: put the container containing the mixed liquid into 0-4℃ water for rapid cooling;

[0020] The obtained iron-carbon particles are iron-carbon particles in which hydrated iron oxide is supported on porous carbon particles.

[0021] In the second aspect, the enhanced artificial wetland phosphorus removal method based on the above iron-carbon particles comprises the following specific steps:

[0022] S1. Selecting iron-carbon particles of appropriate particle size according to the particle size of different artificial wetland fillers to prepare an iron-carbon particle turbid solution;

[0023] S2, using the cyclic pulse method to inject the iron-carbon particle turbid liquid into the normally operating artificial wetland system, and collect the effluent; inject the effluent into the system again to obtain new effluent, and circulate for 5 to 6 cycles until the effluent concentration is less than 1% of the iron-carbon particle turbid liquid concentration in S1, so as to achieve the fixation of the iron-carbon particles in the gaps between the artificial wetland fillers and enhance the phosphorus removal function of the artificial wetland;

[0024] Among them, the constructed wetland (CW) system is a subsurface constructed wetland system, in which the water flow in the filler bed basically presents a vertical flow from top to bottom, and its water outlet device is set at the bottom of the constructed wetland;

[0025] In S1, the appropriate iron-carbon particle sizes selected for different wetland filler particle sizes are: for wetland fillers with a particle size of 2-5 cm, the iron-carbon particles with a particle size of less than 10 μm are selected; for wetland fillers with a particle size of 5-8 cm, the iron-carbon particles with a particle size of 10-70 μm are selected; for wetland fillers with a particle size of 8-10 cm, the iron-carbon particles with a particle size of greater than 70 μm are selected;

[0026] The method for preparing the iron-carbon particle turbid liquid is as follows: preparing iron-carbon particles with a particle size range of 10-70 μm, adding distilled water, stirring, and preparing a suspension containing the iron-carbon particles;

[0027] The addition ratio of iron-carbon particles to the original water volume of the constructed wetland is 36-48 g / L;

[0028] In S2, the cyclic pulse method refers to the process of injecting all the prepared iron-carbon particle turbid liquid into the artificial wetland system by using a pump cycle, and then after the turbid liquid is completely discharged through the wetland drainage outlet, the discharged liquid is re-injected into the artificial wetland system at the same flow rate as the initial injection speed;

[0029] The injection rate of the iron-carbon particle turbid liquid is 5-10 times the normal wetland operating flow rate;

[0030] One cycle means that the pump circulates to inject all the iron-carbon particle turbid liquid into the artificial wetland system, and the iron-carbon particle turbid liquid flows downward through the wetland matrix layer arranged from top to bottom and is discharged, and the discharged liquid is collected. This process is regarded as one cycle of cyclic injection;

[0031] During this process, the porous fillers in artificial wetlands have a high efficiency in intercepting suspended particles, and functional particles are introduced into the wetland system in a cyclic pulse manner. They are fixed in the pores of the fillers to increase the phosphorus adsorption capacity of the subsurface artificial wetland. The immobilized iron-carbon particles have a small particle size and low hydraulic resistance, and have no negative impact on the permeability coefficient of the wetland fillers.

[0032] The beneficial effects of the present invention are:

[0033] 1. Biochar is one of the most common adsorbents, with the advantages of large specific surface area, developed pore structure and good adsorption performance. Hydrated iron oxides have strong binding properties for phosphorus, especially 6-line hydrated iron oxide, which is easily bioavailable and has stronger phosphorus adsorption capacity in the form of ferric ions and ferrous ions than conventional iron oxides. The iron-carbon particles obtained by the composite of the two are fixed in the wetland matrix, with low hydraulic resistance and no negative impact on the permeability coefficient of the wetland filler, and the effect of enhancing the phosphorus removal efficiency of the subsurface flow artificial wetland is good.

[0034] 2. The cyclic pulse method uses a pump to cyclically inject the discharged liquid into the artificial wetland system. Although in order to balance the relationship between the particle immobilization efficiency and the water flow field, there are certain technical requirements for process parameters such as particle size, particle introduction amount, flow rate and number of cycles. However, the cyclic pulse method can effectively introduce functional particles into the artificial wetland system, and has the advantages of no damage to the wetland matrix, simple operation and strong operability.

[0035] 3. The present invention is not only applicable to the enhancement of the phosphorus adsorption function of newly built wetland systems, but can also be conveniently applied to the upgrading and transformation of existing wetland systems, and has the advantages of low cost and convenient operation and maintenance. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0037] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0038] Figure 1 The Langmuir fitting diagram of the adsorption result of iron-carbon particles in Example 2;

[0039] Figure 2 The Langmuir fitting diagram of the gravel matrix adsorption result of Example 2;

[0040] Figure 3 is the Freundlich fitting diagram of the adsorption result of iron-carbon particles in Example 2;

[0041] Figure 4 The Langmuir fitting diagram of the gravel matrix adsorption result of Example 2;

[0042] Figure 5 is a structural diagram of a constructed wetland (CW) model of Example 3;

[0043] Figure 6The total phosphorus concentration change curve of the IP-CW system and the C-CW system in Example 3;

[0044] Among them, 1. water sedge; 2. plexiglass mesh disk; 3. matrix; 4. plexiglass cylinder; 5. water inlet circulation pump; 6. water outlet circulation pump; 7. water inlet pipeline; 8. iron-carbon particle turbid liquid adding device; 9. water outlet pipeline. DETAILED DESCRIPTION

[0045] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0046] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0047] Example 1: Preparation method of iron-carbon particles.

[0048] The following steps are involved:

[0049] S1. calcining biomass materials at low temperature by anaerobically obtaining biochar, grinding the biochar into powder, and sieving and classifying the powder to obtain biochar particles;

[0050] S2. Add biochar particles and ferric nitrate nonahydrate (Fe(NO 3 ) 3 9H 2 O), stirring evenly and then maintaining the temperature and continuing to heat to generate hydrated iron oxides and load them on biochar particles. After the reaction is completed, the mixed solution is sieved;

[0051] S3, washing the obtained product with distilled water and freeze-drying it to obtain the iron-carbon particles;

[0052] Among them, in S1, the biomass material is selected from porous biomass materials; preferably calamus stems, lotus stems, corn stalks, rice straw, etc.;

[0053] The low-temperature anaerobic calcination temperature is 400-500°C;

[0054] The sieving and grading method is as follows: adding the ground biochar powder to deionized water to prepare a turbid solution, grading the ground biochar powder by sieving, obtaining three grades of biochar particles with particle sizes ranging from less than 10 μm, 10-70 μm, and greater than 70 μm, and drying;

[0055] In S2, the preheating temperature of distilled water is 80°C;

[0056] Add ferric nitrate nonahydrate crystals to distilled water to make the concentration of ferric nitrate in the liquid 25g / L. During this process, the ferric nitrate decomposes under heat to release nitrogen and hydrogen.

[0057] After the ferric nitrate solution was allowed to stand for 0.5-1h, a biochar particle of a certain particle size grade was added to the liquid at an amount of 50g / L. At this time, the mass ratio of iron and carbon elements in the mixed solution was 1:1.5;

[0058] The stirring method is: stirring at 200-300 r / min for 10-15 min;

[0059] After the stirring time is over, keep heating at the same temperature for 10-15 minutes.

[0060] The characteristics of the end of the reaction are: the color of the mixed solution changes from gold to dark reddish brown, indicating that the iron nitrate undergoes a chemical change to generate hydrated iron oxide; and the hydrated iron oxide has been successfully loaded onto the biochar particles;

[0061] The rapid cooling method is: put the container containing the mixed liquid into 0℃ water for rapid cooling;

[0062] The obtained iron-carbon particles are iron-carbon particles in which hydrated iron oxide is loaded on porous carbon particles;

[0063] The iron-carbon particles are divided into three grades, namely, the particle sizes are less than 10 μm, 10-70 μm, and greater than 70 μm.

[0064] The hydrated iron oxide, including 6-line hydrated iron oxide (6-line hydrated iron, 6-Line Ferrihydrite), is a weakly crystalline iron oxide compound with a small particle size, which has a large specific surface area and high surface activity; it has a high phosphorus adsorption capacity and strong adsorption stability, and forms a coordination complex or electrostatic attraction with phosphorus for adsorption, and is easily bioavailable, and the iron ions and ferrous ions formed are stronger than conventional iron oxides in terms of phosphorus adsorption capacity. Hydrated iron oxide has a strong binding property for phosphorus, and the iron ions and ferrous ions formed are stronger than conventional iron oxides in terms of phosphorus adsorption capacity.

[0065] The effects of iron-carbon ratio and anaerobic calcination temperature on the iron-carbon particles are shown in Table 1. The iron-carbon mass ratio of 1:1.5 and the calcination temperature of 450 °C are the optimal parameters for preparing iron-carbon particles.

[0066] Table 1

[0067]

[0068] Example 2: Testing of the adsorption performance of phosphorus on iron-carbon particles and gravel.

[0069] 100 mL of solution with an initial phosphorus concentration of 1500 μg / L was prepared for both groups; phosphorus was added in the form of potassium dihydrogen phosphate;

[0070] 0.5g of iron-carbon particles or 5.0g of gravel were added to 100mL of solution in the two groups of solutions, and equilibrium adsorption tests were performed. The adsorption test was carried out at 28°C, and the adsorption process was shaken at 180r / min for 48h. The adsorption results were fitted with Langmuir and Freundlich isotherms to the adsorption characteristics of different adsorbents. The results are shown in Figure 1-4 As shown. It can be concluded that the Langmuir model has a higher fitting coefficient than the Freundlich model. The maximum adsorption capacity of phosphorus on iron-carbon particles and gravel is 10.6 mg / g and 0.052 mg / g, respectively. The adsorption capacity of the former is more than 200 times that of the latter, indicating that iron-carbon particles can enhance the removal of phosphorus in water.

[0071] Example 3: A method for enhanced phosphorus removal in artificial wetlands based on the above-mentioned iron-carbon particles.

[0072] First, two sets of constructed wetland (CW) models were prepared, such as Figure 5 As shown, each CW is made of a plexiglass cylinder 4 and is externally provided with a water circulation pipeline; the cylinder is a cylinder-shaped hollow structure, which is divided into a bottom layer, a middle layer, and a top layer from bottom to top; an inlet circulation pump and an outlet circulation pump are arranged in the water circulation pipeline, and an iron-carbon particle turbid liquid adding device is arranged between the inlet pipeline and the outlet pipeline;

[0073] The bottom layer and the middle layer are separated by a plexiglass mesh plate 2, which is installed 15 cm above the bottom of the CW. The bottom layer is 15 cm below the plexiglass mesh plate 2. The plexiglass mesh plate 2 is filled with a matrix 3, which is selected as gravel with a diameter of 3-8 mm. The matrix 3 is supported by the plexiglass mesh 2, and the thickness of the matrix is ​​60 cm. Water sedge 1 is planted on the top layer. The water circulation process in the CW is as follows: the water inlet circulation pump 5 in the water inlet pipeline injects water flow evenly into the surface of the top layer of the CW, and the water flow passes through the gravel base layer arranged from top to bottom and is discharged from the drain port. The discharge liquid is collected by the water outlet pipeline equipped with a water outlet circulation pump 6 and sent to the iron-carbon particle turbid liquid adding device 8.

[0074] Phosphorus was added to the constructed wetland to stabilize the phosphorus concentration at 0.8 mg / L;

[0075] The artificial wetland system is a subsurface artificial wetland system, filled with three layers of matrix. The matrix types arranged from top to bottom are: coarse gravel (diameter 7-8mm; porosity 38%) at 0-20cm, medium gravel (diameter 5-6mm; porosity 36%) at 20-40cm, and fine gravel (diameter 3-4mm; porosity 33%) at 40-60cm. The arrangement of the matrix is ​​conducive to the uniform deposition and fixation of iron-carbon particles in the wetland bed. The height of the wetland bed filler layer is about 60cm, and the water flow in the filler bed basically presents a vertical flow from top to bottom, and its water outlet device is located at the bottom of the artificial wetland);

[0076] The specific steps of enhanced artificial wetland phosphorus removal with iron-carbon particles are:

[0077] S1. Selecting iron-carbon particles of appropriate particle size according to the particle size of the artificial wetland filler to prepare an iron-carbon particle turbid solution;

[0078] S2, using the cyclic pulse method to inject the iron-carbon particle turbid liquid into a group of normally operating artificial wetland systems, as the experimental group IP-CW, and collect the effluent; inject the effluent into the system to obtain new effluent, and circulate for 5 to 6 cycles until the effluent concentration is less than 1% of the iron-carbon particle turbid liquid concentration in S1, so as to achieve the fixation of iron-carbon particles in the gaps between the artificial wetland fillers and enhance the phosphorus removal function of the artificial wetland; the other group is not injected with the iron-carbon particle turbid liquid, as the control group C-CW;

[0079] In S1, the particle size selection of this embodiment is: the particle size of the wetland filler is 2-5cm, and the particle size is less than 10μm. The particle size of the wetland filler is 5-8cm, and the particle size is 10-70μm. The particle size of the wetland filler is 8-10cm, and the particle size is greater than 70μm.

[0080] The method for preparing the iron-carbon particle turbid liquid is as follows: preparing iron-carbon particles with a particle size range of 10-70 μm, freeze-drying, and preparing a suspension containing 120-160 g / L of iron-carbon particles;

[0081] The volume of the iron-carbon particle turbid liquid is 15L, and the original water in the artificial wetland model is 50L;

[0082] At this time, the addition ratio of iron-carbon particles to the original water volume of the artificial wetland is 36-48 g / L;

[0083] In S2, the cyclic pulse method refers to the process of injecting all the prepared iron-carbon particle turbid liquid into the artificial wetland system by using a pump cycle, and then after the turbid liquid is completely discharged through the wetland drainage outlet, the discharged liquid is re-injected into the artificial wetland system at the same flow rate as the initial injection speed;

[0084] To speed up the test process, the injection rate of the iron-carbon particle turbid solution was 5-10 times the normal wetland operating flow rate;

[0085] In this embodiment, the normal wetland operation flow rate is 20 ml / min and the injection rate is 200 ml / min.

[0086] The initial injection method of the iron-carbon particle turbid liquid is as follows: the iron-carbon particle turbid liquid is sent to the iron-carbon particle turbid liquid adding device 8, the water inlet circulation pump is started, the iron-carbon particle turbid liquid is injected into the CW system at a set injection speed, and the discharged liquid containing the iron-carbon particles is collected in the outlet pipe;

[0087] The re-injection method of the effluent is that after all the iron-carbon particle turbid liquid flows downward through the wetland bed filler layer once, the effluent is collected, and then the effluent containing the iron-carbon particles is re-injected into the artificial wetland system at the same flow rate as the initial injection speed; the effluent is circulated and injected into the artificial wetland system;

[0088] During this process, the particulate turbid liquid is evenly distributed and added to the surface of the wetland bed through a pump device. The iron-carbon particulate turbid liquid freely passes through the wetland matrix vertically and seeps to the bottom of the bed. A part of the iron-carbon particles are fixed in the artificial wetland matrix. This process is continuously circulated, so that more and more iron-carbon particles are fixed.

[0089] One cycle means that the pump circulates to inject all the iron-carbon particle turbid liquid into the artificial wetland system, and the iron-carbon particle turbid liquid flows downward through the wetland matrix layer arranged from top to bottom and is discharged, and the discharged liquid is collected. This process is regarded as one cycle of cyclic injection;

[0090] Preferably, the iron-carbon particles are injected cyclically for 5-6 cycles, for a total of about 8-9 hours;

[0091] Sampling was performed at the CW inlet pipe 7 and the CW outlet pipe 9 to observe the change process of total phosphorus concentration in the water. The total phosphorus concentration change curve is shown in Figure 6 As shown in the figure, the total phosphorus (TP) concentration of the effluent of the IP-CW system gradually decreased from 0.8 mg / L to below 0.2 mg / L, and the removal rate increased to 90.4±1.9%. In contrast, the removal rate of TP in the C-CW system did not increase significantly, and only showed a downward trend after 120 days of operation; this shows that the artificial wetland without the addition of iron-carbon particles has a low phosphorus adsorption capacity, is easily saturated with adsorption, and has a poor sustainable phosphorus removal effect; in the artificial wetland with the addition of iron-carbon particles, the iron-carbon particles can be fixed in the voids of the porous matrix to play a role in phosphorus adsorption, with a high phosphorus adsorption capacity and difficulty in adsorption saturation, and the fixed iron-carbon particles have a small particle size and low hydraulic resistance, and have no negative impact on the permeability coefficient of the wetland filler.

[0092] When applied to the actual artificial wetland system, the ratio of the volume of iron-carbon microparticle turbidity to the artificial wetland water body is 1:10;

[0093] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and changes. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for enhanced phosphorus removal in artificial wetlands using iron-carbon particles, comprising the following steps: S1. Selecting iron-carbon particles of appropriate particle size according to the particle size of different artificial wetland fillers to prepare an iron-carbon particle turbid solution; S2, injecting the iron-carbon particle turbid liquid into the normally operating artificial wetland system by using the cyclic pulse method, and collecting the discharged liquid; S3, inject the effluent into the system to obtain new effluent, and circulate for 5 to 6 cycles until the concentration of the effluent is less than 1% of the concentration of the iron-carbon particle turbidity in S1, so as to achieve the fixation of the iron-carbon particles in the gaps of the artificial wetland filler and enhance the phosphorus removal function of the artificial wetland; Among them, in S1, the wetland filler with a particle size of 2-5 cm is selected to be iron-carbon particles with a particle size of less than 10 μm; the wetland filler with a particle size of 5-8 cm is selected to be iron-carbon particles with a particle size of 10-70 μm; the wetland filler with a particle size of 8-10 cm is selected to be iron-carbon particles with a particle size of more than 70 μm; In S1, the iron-carbon particle turbid liquid is a suspension in which the iron-carbon particle addition amount is 120-160 g / L; In S2, the injection rate of the iron-carbon particle turbid solution is 5-10 times the normal wetland operation flow rate; The method for preparing the iron-carbon particles comprises the following steps: S1′, calcining the biomass material at low temperature by anaerobically obtaining biochar, grinding the biochar into powder, and sieving and classifying the powder to obtain biochar particles; S2′, add biochar particles and ferric nitrate nonahydrate to preheated distilled water, stir evenly and continue heating at the same temperature to generate hydrated iron oxide and load it on the biochar particles. After the reaction is completed, filter the mixture; S3′, washing the filtered product with distilled water and freeze-drying it to obtain the iron-carbon particles; In S1′, the biomass material is a porous biomass material; The low-temperature anaerobic calcination temperature is 450°C; In S2′, the preheating temperature of distilled water is 75~80℃; Add ferric nitrate nonahydrate to make the concentration of ferric nitrate in the mixed solution 25 g / L; add biochar particles to make the mass ratio of iron to carbon 1:1.5; The obtained iron-carbon particles are iron-carbon particles in which hydrated iron oxide is loaded on porous carbon particles; The hydrous iron oxide includes 6-line hydrous iron oxide.

2. The method for enhancing phosphorus removal in artificial wetlands according to claim 1, characterized in that: When applied to the actual artificial wetland system, the ratio of iron-carbon microparticle turbid liquid to artificial wetland water is 1:

10. 。 3. The method for enhancing phosphorus removal in artificial wetlands according to claim 1, characterized in that: In S3, one cycle means that the pump circulates to inject all the prepared iron-carbon particle turbidity into the artificial wetland system, and the iron-carbon particle turbidity flows downward through the wetland matrix layer arranged from top to bottom and is discharged, and the discharged liquid is collected for backup. This process is regarded as one cycle of cyclic injection.

4. The method for enhancing phosphorus removal in artificial wetlands according to claim 1, characterized in that: The preparation method of the iron-carbon particles, In S1′, the biomass material is a porous biomass material, and the porous biomass material is one or more of calamus stems, lotus stems, corn stalks and rice straw.

5. The method for enhancing phosphorus removal in artificial wetlands according to claim 1, characterized in that: The preparation method of the iron-carbon particles, In S2′, the stirring method is: stirring at 200-300 r / min for 10-15 min; After the stirring time is over, keep heating at the same temperature for 10-15 min. The rapid cooling method is: place the container containing the mixed liquid into 0~4℃ water for rapid cooling.

6. The method for enhancing phosphorus removal in artificial wetlands according to claim 1, characterized in that: The preparation method of the iron-carbon particles, The reaction is complete when the color of the mixture changes from gold to dark reddish brown. 。 7. The method for enhancing phosphorus removal in artificial wetlands according to claim 1, characterized in that: The preparation method of the iron-carbon particles, The sieving and grading method is as follows: adding the ground biochar powder to deionized water to prepare a turbid solution, and grading the ground biochar powder by sieving to obtain three grades of biochar particles with particle size ranges of less than 10 μm, 10-70 μm, and greater than 70 μm.

Citation Information

Cited By

  • Double-ferromagnetic modified charcoal phosphorus adsorbent as well as preparation method and application thereof

    CN118105942A