Application of electromagnetic coupling treatment method in electroplating process

By introducing electromagnetic coupling treatment into the electroplating process, the problems of poor coating bonding force and cracks are solved, the coating bonding force is improved and the cost is reduced, and a new efficient and environmentally friendly electroplating process is provided.

CN116397186BActive Publication Date: 2024-11-12SICHUAN UNIV
View PDF 18 Cites 0 Cited by

Patent Information

Application Number
CN202310339997.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-11-12
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

In traditional electroplating technology, the binding force of the coating is poor and easy to produce cracks. The thermal aging cost is high, the energy consumption is large, and the environmental pollution is large, and the uneven temperature causes the uneven distribution of the coating binding force.

Method used

An electromagnetic coupling treatment method is introduced, and electromagnetic coupling treatment is carried out after grinding and plating, and residual stress is regulated and diffusion of plating elements is promoted through pulsed electromagnetic fields, grains are refined, and plating bonding force is enhanced.

Benefits of technology

Effectively regulate residual stress, improve the binding force and hardness of the plating, reduce production costs, reduce environmental pollution, improve yield, and short processing time without the risk of high temperature overheating, providing a new high-efficiency, low energy consumption, and green electroplating process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116397186B_ABST
    Figure CN116397186B_ABST
Patent Text Reader

Abstract

The present invention discloses the application of an electromagnetic coupling treatment method in an electroplating process, wherein the electromagnetic coupling treatment is performed after the workpiece to be processed is polished or electroplated. The present invention places the polished workpiece in an electromagnetic coupling field, and uses a pulsed electromagnetic external field to treat the workpiece. The vibration generated by the electrostriction and magnetostriction of the workpiece interacts with the residual stress, and the dislocations in the material move, thereby playing a role in regulating the residual stress. The present invention causes the workpiece after electroplating to produce atomic diffusion between the substrate and the coating material under the action of the electromagnetic field, thereby enhancing the bonding force of the coating, while the grains are refined, and the hardness and wear resistance of the coating are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal material processing, relates to an electroplating process, and specifically relates to the application of an electromagnetic coupling treatment method in the electroplating process. Background Art

[0002] In daily life, due to the needs of various working environments, people often electroplate materials, such as electroplating a layer of wear-resistant material on the surface of the material to improve the wear resistance of the material surface; or electroplating a layer of conductive material on the surface of the material to make the surface of the material (such as plastic) have a certain conductivity. The electroplating process has the following main functions: (1) improve the corrosion resistance of metal parts in the use environment; decorate the appearance of parts to make them bright and beautiful; (2) improve the working performance of parts, such as hardness, wear resistance, conductivity, electromagnetic properties, heat resistance, brazing and other special properties. At present, there are several difficulties with the traditional electroplating process: on the one hand, the grinding process when removing the oxide layer on the surface of the substrate will introduce residual stress, which will reduce the bonding strength of the coating; on the other hand, the bonding strength of the coating is unevenly distributed, and cracks and rust appear on the surface during post-plating inspection.

[0003] The quality problem of electroplating coating is mainly the regulation of coating bonding strength. Since the removal of the substrate surface oxide layer is an indispensable condition in the coating preparation process, the introduction of residual stress is unavoidable, and the coating bonding strength will inevitably be affected. Now the researchers aim to overcome the problems of weak coating bonding strength and uneven bonding strength distribution by finding a suitable coating processing technology. While solving the above problems, new stress is not introduced, the growth of surface cracks after plating is inhibited, and production efficiency is improved.

[0004] The traditional electroplating process includes grinding and polishing → hanging → degreasing and deoiling → water washing → pickling and activation → pre-plating → electroplating → water washing → drying → hanging → inspection and packaging, etc. There is an existing electroplating process that adds thermal aging treatment after pre-plating and before electroplating, aiming to eliminate the residual stress generated by the aforementioned electroplating process through aging treatment, thereby enhancing the bonding strength of the coating. However, since the aging treatment needs to be maintained at a higher temperature for a longer time, it not only prolongs the entire electroplating process production cycle, has high energy consumption, high economic and time costs, but also causes greater pollution to the environment. In addition, due to the uneven temperature in the thermal aging furnace, the heating and cooling speed cannot be strictly controlled. In the same furnace, thermal aging eliminates stress unevenly and is prone to microcracks. Summary of the invention

[0005] The purpose of the present invention is to introduce electromagnetic coupling treatment into the electroplating process to address the problems of poor coating adhesion and easy cracking in the existing electroplating process. Under the premise of ensuring the quality of the coating, the residual stress can be regulated, the coating adhesion can be improved, the economic cost and time cost required for production can be reduced, the pollution to the environment can be reduced, the yield rate can be improved, and at the same time, the coating performance (including hardness, wear resistance, etc.) can be improved to a certain extent.

[0006] In order to achieve the above object, the object of the present invention can be achieved through the following technical solutions.

[0007] The electromagnetic coupling treatment method provided by the present invention is applied in an electroplating process, and the electromagnetic coupling treatment is performed after the workpiece to be treated is polished or electroplated.

[0008] After the workpiece is ground and polished, electromagnetic coupling treatment is performed, including the following steps:

[0009] S10 sets the electric field parameters; the electric field parameters include: the pulse voltage amplitude is 0.5-2.5V, the current density is 10-25A / mm 2 Each group of pulses includes a positive pulse and a negative pulse, and the unilateral pulse frequency is 50-100 Hz; the number of pulse groups is 1000-3000 groups, the interval time between adjacent pulse groups is 10-100 ms, and the pulse electric field application time is 100-150 s;

[0010] S11 sets magnetic field parameters; the magnetic field parameters include: pulse magnetic field intensity of 1 to 2.5 T, single pulse magnetic field action time of 8 to 12 s, interval between two adjacent magnetic field pulses of 1 to 3 s, pulse magnetic field magnetization times of 10 to 14 times, and pulse magnetic field application time of 100 to 150 s;

[0011] S12 places the workpiece to be processed in an environment where an electric field and a magnetic field are applied, and performs several iterative cycles of electric field and magnetic field alternating processing as a cycle according to the electric field parameters and magnetic field parameters set in steps S10 and S11.

[0012] Electromagnetic coupling treatment is performed after the workpiece to be treated is electroplated, including the following steps:

[0013] S20 sets the electric field parameters; the electric field parameters include: the pulse voltage amplitude is 0.5 to 5V, the current density is 10 to 50A / mm 2 Each group of pulses includes a positive pulse and a negative pulse, and the unilateral pulse frequency is 50-100 Hz; the number of pulse groups is 1000-3000 groups, the interval time between adjacent pulse groups is 10-100 ms, and the pulse electric field application time is 100-150 s;

[0014] S21 sets magnetic field parameters; the magnetic field parameters include: pulse magnetic field intensity of 1 to 5T, single pulse magnetic field action time of 8 to 12s, interval between two adjacent magnetic field pulses of 1 to 3s, pulse magnetic field magnetization times of 10 to 14 times, and pulse magnetic field application time of 100 to 150s;

[0015] S22 places the workpiece to be processed in an environment where an electric field and a magnetic field are applied, and performs several iterative cycles of electric field and magnetic field alternating processing as a cycle according to the electric field parameters and magnetic field parameters set in steps S20 and S21.

[0016] In the above application, the number of iterations of performing electromagnetic coupling processing on the workpiece to be processed after grinding and polishing in step S12 is 10 to 14 times.

[0017] In the above application, the number of iterations of performing electromagnetic coupling treatment on the workpiece to be treated after electroplating in step S22 is 10 to 14 times.

[0018] In the above application, the workpiece to be processed is a metal material loaded with a plating or coating, mainly a metal material loaded with a plating or coating for electronic packaging components, such as a molybdenum-copper carrier plate plated with a nickel layer and / or a gold layer, a beryllium copper part or an aluminum alloy workpiece.

[0019] Compared with the prior art, the present invention adds "electromagnetic coupling treatment" after "grinding and polishing" and "electroplating". The first electromagnetic coupling treatment is to regulate the residual stress introduced by grinding and polishing; the second electromagnetic coupling treatment is to promote the diffusion of coating elements and refine the grains to enhance the bonding strength of the coating, improve aging treatment, reduce production costs, and reduce pollution to the environment, which is an efficient and economical way to improve the hardness of the coating.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] 1. The present invention places the polished workpiece in an electromagnetic coupling field and uses a pulsed electromagnetic external field to process the workpiece. The vibration generated by the electrostriction and magnetostriction of the workpiece interacts with the residual stress, and the dislocations in the material move, thereby playing a role in regulating the residual stress.

[0022] 2. The present invention causes atomic diffusion between the substrate and the coating material of the electroplated workpiece under the action of an electromagnetic field, thereby enhancing the bonding strength of the coating, while at the same time refining the grains, and improving the hardness and wear resistance of the coating.

[0023] 3. The single treatment time of the workpiece of the present invention is 2-4 minutes, which is extremely short compared with the aging treatment, greatly saving the production cost; and there will be no large temperature change on the whole workpiece, so there will be no high temperature overheating phenomenon, thereby avoiding the change of the metallographic structure of the workpiece caused by high temperature;

[0024] 4. Compared with aging treatment, electromagnetic coupling treatment has the advantages of high efficiency, low energy consumption, greenness and pollution-free, providing a new development direction for the development of new green electroplating processes. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a flow chart of the electroplating process in Example 1 of the present invention.

[0026] Figure 2 The hardness test results of the molybdenum-copper substrate electroplated with a nickel layer and a gold layer in sequence before and after the electromagnetic coupling treatment in Example 1 of the present invention.

[0027] Figure 3 This is a flow chart of the electroplating process in Example 2 of the present invention.

[0028] Figure 4 The surface residual stress test results of the molybdenum-copper carrier plate after grinding and polishing before and after electromagnetic coupling treatment in Example 2 of the present invention. DETAILED DESCRIPTION

[0029] It is intended to clearly and completely describe the technical solutions of the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the present invention.

[0030] Example 1

[0031] In this embodiment, a nickel layer (20 μm) and a gold layer (5 μm) are electroplated in sequence on the surface of a 3 mm molybdenum-copper substrate.

[0032] The electroplating process used in this embodiment is as follows: Figure 1 As shown, it includes grinding and polishing, cleaning, hanging, degreasing, activation, pre-plating, electroplating, cleaning, material turnover, electromagnetic coupling processing, cleaning, drying and detection packaging.

[0033] The above-mentioned grinding and polishing, cleaning, hanging, degreasing, activation, pre-plating, electroplating, drying and testing packaging all adopt conventional means disclosed in the art, see CN104018195A.

[0034] (I) Electromagnetic coupling treatment after electroplating

[0035] Electromagnetic coupling treatment is performed after electroplating the molybdenum-copper substrate, including the following steps:

[0036] S20 sets the electric field parameters; the electric field parameters include: pulse voltage amplitude of 1.2V, current density of 20A / mm 2Each pulse group includes a positive pulse and a negative pulse, and the unilateral pulse frequency is 50Hz; the number of pulse groups is 2400, the interval time between adjacent pulse groups is 10ms, and the pulse electric field application time is 120s;

[0037] S21 sets magnetic field parameters; the magnetic field parameters include: pulse magnetic field intensity is 1.5T, single pulse magnetic field action time is 9s, interval between two adjacent magnetic field pulses is 1s, pulse magnetic field magnetization times is 12 times, and pulse magnetic field application time is 120s;

[0038] S22 places the molybdenum-copper carrier plate in an environment where an electric field and a magnetic field are applied. The molybdenum-copper carrier plate is clamped by a fixture and connected to both ends of electrodes that generate a pulse current, and the sample is placed at the center of the pulsed magnetic field; then, according to the electric field parameters and magnetic field parameters set in steps S20 and S21, the alternating treatment of the electric field and the magnetic field is used as a cycle, and the workpiece to be processed is iterated for 12 times.

[0039] The hardness of the molybdenum-copper substrate plated with nickel layer and gold layer before and after electromagnetic coupling treatment was tested. Ten points on the substrate were selected for hardness testing. The test results are as follows: Figure 2 As shown. The maximum and minimum values ​​of hardness before electromagnetic coupling treatment, the average Vickers hardness is calculated to be 204.0, and the variance is 352.86; the maximum and minimum values ​​of hardness after electromagnetic coupling treatment, the average Vickers hardness is calculated to be 222.8, and the variance is 123.02. The hardness growth rate is (222.8-204) / 204*100%=9.2%, that is, the hardness after electromagnetic coupling treatment is increased by 9.2% compared with that before treatment, and the hardness variance after treatment becomes smaller, and the surface hardness of the molybdenum-copper carrier plate is more uniform.

[0040] Example 2

[0041] In this embodiment, a nickel layer (20 μm) and a gold layer (5 μm) are electroplated in sequence on the surface of a 3 mm molybdenum-copper substrate.

[0042] The electroplating process used in this embodiment is as follows: Figure 3 As shown, it includes grinding and polishing, electromagnetic coupling treatment, cleaning, hanging, degreasing, activation, pre-plating, electroplating, cleaning, material turnover, electromagnetic coupling treatment, cleaning, drying and detection packaging.

[0043] The above-mentioned grinding and polishing, cleaning, hanging, degreasing, activation, pre-plating, electroplating, drying and testing packaging all adopt conventional means disclosed in the art, see CN104018195A.

[0044] (I) Electromagnetic coupling treatment after grinding and polishing

[0045] After the molybdenum copper carrier plate is ground and polished, the electromagnetic coupling treatment is performed, including the following steps:

[0046] S10 sets the electric field parameters; the electric field parameters include: pulse voltage amplitude of 1.2V, current density of 20A / mm 2 Each pulse group includes a positive pulse and a negative pulse, and the unilateral pulse frequency is 50Hz; the number of pulse groups is 2400, the interval time between adjacent pulse groups is 10ms, and the pulse electric field application time is 120s;

[0047] S11 sets magnetic field parameters; the magnetic field parameters include: pulse magnetic field intensity is 1.5T, single pulse magnetic field action time is 9s, interval between two adjacent magnetic field pulses is 1s, pulse magnetic field magnetization times is 12 times, and pulse magnetic field application time is 120s;

[0048] S12 places the molybdenum-copper carrier plate in an environment where an electric field and a magnetic field are applied. The molybdenum-copper carrier plate is clamped by a fixture and connected to both ends of electrodes that generate a pulse current, and the sample is placed at the center of the pulsed magnetic field. Then, according to the electric field parameters and magnetic field parameters set in steps S10 and S11, alternating electric field and magnetic field treatment is used as a cycle to iterate the workpiece to be processed, and the number of iterations is 12.

[0049] After grinding and polishing, the residual stress on the surface of the molybdenum-copper carrier plate before and after the electromagnetic coupling treatment was tested. Ten points on the carrier plate were selected for residual stress detection. The test results are as follows: Figure 4 As shown in the figure, the maximum and minimum values ​​of residual stress before electromagnetic coupling treatment, the calculated average residual stress is 121.8MPa; the maximum and minimum values ​​of residual stress after electromagnetic coupling treatment, the calculated average residual stress is 94.8MPa. That is, the residual stress on the carrier surface after electromagnetic coupling treatment is reduced by 22% compared with that before treatment.

[0050] (II) Electromagnetic coupling treatment after electroplating

[0051] Electromagnetic coupling treatment is performed after electroplating the molybdenum-copper substrate, including the following steps:

[0052] S20 sets the electric field parameters; the electric field parameters include: pulse voltage of 1.2V, current density of 20A / mm 2 Each pulse group includes a positive pulse and a negative pulse, and the unilateral pulse frequency is 50Hz; the number of pulse groups is 2400, the interval time between adjacent pulse groups is 10ms, and the pulse electric field application time is 120s;

[0053] S21 sets magnetic field parameters; the magnetic field parameters include: pulse magnetic field intensity of 1.5T, single pulse magnetic field action time of 9s, interval between two adjacent magnetic field pulses of 1s, pulse magnetic field magnetization times of 12 times, and pulse magnetic field application time of 120s;

[0054] S22 places the molybdenum-copper carrier plate in an environment where an electric field and a magnetic field are applied. The molybdenum-copper carrier plate is clamped by a fixture and connected to both ends of electrodes that generate a pulse current, and the sample is placed at the center of the pulsed magnetic field; then, according to the electric field parameters and magnetic field parameters set in steps S20 and S21, the alternating treatment of the electric field and the magnetic field is used as a cycle, and the workpiece to be processed is iterated for 12 times.

[0055] Example 3

[0056] In this embodiment, a nickel layer (30 μm) and a gold layer (10 μm) are electroplated in sequence on the surface of a 10 mm beryllium copper part.

[0057] The electroplating process used in this embodiment is as follows: Figure 3 As shown, it includes grinding and polishing, electromagnetic coupling treatment, cleaning, hanging, degreasing, activation, pre-plating, electroplating, cleaning, material turnover, electromagnetic coupling treatment, cleaning, drying and detection packaging.

[0058] The above-mentioned grinding and polishing, cleaning, hanging, degreasing, activation, pre-plating, electroplating, drying and testing packaging all adopt conventional means disclosed in the art, see CN104018195A.

[0059] (I) Electromagnetic coupling treatment after grinding and polishing

[0060] Electromagnetic coupling treatment is performed after grinding and polishing of beryllium copper parts, including the following steps:

[0061] S10 sets the electric field parameters; the electric field parameters include: pulse voltage is 2.5V, current density is 10A / mm 2 Each pulse group includes a positive pulse and a negative pulse, and the unilateral pulse frequency is 100Hz; the number of pulse groups is 1500, the interval time between adjacent pulse groups is 80ms, and the pulse electric field application time is 150s;

[0062] S11 sets magnetic field parameters; the magnetic field parameters include: pulse magnetic field intensity is 2.5T, single pulse magnetic field action time is 8s, interval between two adjacent magnetic field pulses is 2s, pulse magnetic field magnetization times is 14 times, and pulse magnetic field application time is 140s;

[0063] S12 places the beryllium copper piece in an environment where an electric field and a magnetic field are applied. The beryllium copper piece is clamped by a fixture and connected to both ends of electrodes that generate a pulse current, and the sample is placed at the center of the pulsed magnetic field. Then, according to the electric field parameters and magnetic field parameters set in steps S10 and S11, alternating electric field and magnetic field treatment is used as a cycle, and the workpiece to be processed is iterated for 14 times.

[0064] (II) Electromagnetic coupling treatment after electroplating

[0065] Electromagnetic coupling treatment is performed after beryllium copper parts are electroplated, including the following steps:

[0066] S20 sets the electric field parameters; the electric field parameters include: pulse voltage is 5V, current density is 50A / mm 2 , each group of pulses includes a positive pulse and a negative pulse, the unilateral pulse frequency is 100Hz; the number of pulse groups is 1000, the interval time between adjacent pulse groups is 80ms, and the pulse electric field application time is 100s;

[0067] S21 sets magnetic field parameters; the magnetic field parameters include: pulse magnetic field intensity is 5T, single pulse magnetic field action time is 8s, interval between two adjacent magnetic field pulses is 2s, pulse magnetic field magnetization times is 10 times, and pulse magnetic field application time is 100s;

[0068] S22 places the beryllium copper piece in an environment where an electric field and a magnetic field are applied. The beryllium copper piece is clamped by a fixture and connected to both ends of electrodes that generate a pulse current, and the sample is placed at the center of the pulsed magnetic field. Then, according to the electric field parameters and magnetic field parameters set in steps S20 and S21, alternating electric field and magnetic field treatment is used as a cycle, and the workpiece to be processed is iterated for 14 times.

[0069] Example 4

[0070] In this embodiment, a nickel layer (10 μm) and a gold layer (5 μm) are electroplated in sequence on the surface of a 3 mm aluminum alloy workpiece.

[0071] The electroplating process used in this embodiment is as follows: Figure 3 As shown, it includes grinding and polishing, electromagnetic coupling treatment, cleaning, hanging, degreasing, activation, pre-plating, electroplating, cleaning, material turnover, electromagnetic coupling treatment, cleaning, drying and detection packaging.

[0072] The above-mentioned grinding and polishing, cleaning, hanging, degreasing, activation, pre-plating, electroplating, drying and testing packaging all adopt conventional means disclosed in the art, see CN104018195A.

[0073] (I) Electromagnetic coupling treatment after grinding and polishing

[0074] Electromagnetic coupling treatment is performed after grinding and polishing of the aluminum alloy workpiece, including the following steps:

[0075] S10 sets the electric field parameters; the electric field parameters include: pulse voltage of 0.5V, current density of 10A / mm 2 Each pulse group includes a positive pulse and a negative pulse, and the single-side pulse frequency is 50Hz; the number of pulse groups is 3000, the interval time between adjacent pulse groups is 10ms, and the pulse electric field application time is 150s;

[0076] S11 sets magnetic field parameters; the magnetic field parameters include: pulse magnetic field intensity of 1T, single pulse magnetic field action time of 12s, interval between two adjacent magnetic field pulses of 3s, pulse magnetic field magnetization times of 10 times, and pulse magnetic field application time of 150s;

[0077] S12 places the aluminum alloy workpiece in an environment where an electric field and a magnetic field are applied. The aluminum alloy workpiece is clamped by a fixture and connected to both ends of electrodes that generate a pulse current, and the sample is placed at the center of the pulsed magnetic field; then, according to the electric field parameters and magnetic field parameters set in steps S10 and S11, alternating electric field and magnetic field treatment is used as a cycle, and the workpiece to be processed is iterated 10 times.

[0078] (II) Electromagnetic coupling treatment after electroplating

[0079] Electromagnetic coupling treatment is performed on the aluminum alloy workpiece after electroplating, including the following steps:

[0080] S20 sets the electric field parameters; the electric field parameters include: pulse voltage of 0.5V, current density of 10A / mm 2 Each pulse group includes a positive pulse and a negative pulse, and the single-side pulse frequency is 50Hz; the number of pulse groups is 3000, the interval time between adjacent pulse groups is 10ms, and the pulse electric field application time is 150s;

[0081] S21 sets magnetic field parameters; the magnetic field parameters include: pulse magnetic field intensity of 1T, single pulse magnetic field action time of 12s, interval between two adjacent magnetic field pulses of 3s, pulse magnetic field magnetization times of 10 times, and pulse magnetic field application time of 150s;

[0082] S22 places the aluminum alloy workpiece in an environment where an electric field and a magnetic field are applied. The aluminum alloy workpiece is clamped by a fixture and connected to both ends of electrodes that generate a pulse current, and the sample is placed at the center of the pulsed magnetic field; then, according to the electric field parameters and magnetic field parameters set in steps S20 and S21, alternating electric field and magnetic field treatment is used as a cycle, and the workpiece to be processed is iterated for 10 times.

[0083] Those skilled in the art will appreciate that the embodiments described herein are intended to help readers understand the principles of the present invention, and should be understood that the protection scope of the present invention is not limited to such specific statements and embodiments. Those skilled in the art can make various other specific variations and combinations that do not deviate from the essence of the present invention based on the technical revelations disclosed by the present invention, and these variations and combinations are still within the protection scope of the present invention.

Claims

1. Application of electromagnetic coupling treatment method in electroplating process, characterized in that: Electromagnetic coupling treatment is performed after grinding or electroplating of the workpiece to be processed; After the workpiece is ground and polished, electromagnetic coupling treatment is performed, including the following steps: S10 sets the electric field parameters; the electric field parameters include: the pulse voltage amplitude is 0.5-2.5V, the current density is 10-25A / mm 2 Each group of pulses includes a positive pulse and a negative pulse, and the unilateral pulse frequency is 50-100 Hz; the number of pulse groups is 1000-3000 groups, the interval time between adjacent pulse groups is 10-100 ms, and the pulse electric field application time is 100-150 s; S11 sets magnetic field parameters; the magnetic field parameters include: pulse magnetic field intensity of 1 to 2.5 T, single pulse magnetic field action time of 8 to 12 s, interval between two adjacent magnetic field pulses of 1 to 3 s, pulse magnetic field magnetization times of 10 to 14 times, and pulse magnetic field application time of 100 to 150 s; S12: placing the workpiece to be processed in an electric field and magnetic field application environment, and performing iterative processing on the workpiece to be processed by alternating electric field and magnetic field processing as a cycle according to the electric field parameters and magnetic field parameters set in steps S10 and S11; The electromagnetic coupling treatment is performed after the workpiece to be treated is electroplated, including the following steps: S20 sets the electric field parameters; the electric field parameters include: the pulse voltage amplitude is 0.5 to 5V, the current density is 10 to 50A / mm 2 Each group of pulses includes a positive pulse and a negative pulse, and the unilateral pulse frequency is 50-100 Hz; the number of pulse groups is 1000-3000 groups, the interval time between adjacent pulse groups is 10-100 ms, and the pulse electric field application time is 100-150 s; S21 sets magnetic field parameters; the magnetic field parameters include: pulse magnetic field intensity of 1 to 5T, single pulse magnetic field action time of 8 to 12s, interval between two adjacent magnetic field pulses of 1 to 3s, pulse magnetic field magnetization times of 10 to 14 times, and pulse magnetic field application time of 100 to 150s; S22 places the workpiece to be processed in an environment where an electric field and a magnetic field are applied, and performs iterative processing on the workpiece to be processed by alternating the electric field and the magnetic field according to the electric field parameters and the magnetic field parameters set in steps S20 and S21, with the electric field and the magnetic field being processed as a cycle.

2. Application of the electromagnetic coupling treatment method according to claim 1 in electroplating process, characterized in that: In step S12, the number of iterations of performing electromagnetic coupling processing on the workpiece to be processed after grinding and polishing is 10 to 14 times.

3. Application of the electromagnetic coupling treatment method according to claim 1 in electroplating process, characterized in that: In step S22, the number of iterations of performing electromagnetic coupling treatment on the workpiece to be treated after electroplating is 10 to 14 times.

4. Application of the electromagnetic coupling treatment method according to claim 1 in electroplating process, characterized in that: The workpiece to be processed is a metal material loaded with a plating layer or a coating.

5. Application of the electromagnetic coupling treatment method according to claim 1 in electroplating process, characterized in that: The workpiece to be processed is a molybdenum-copper carrier plate, a beryllium-copper part or an aluminum alloy workpiece plated with a nickel layer and / or a gold layer.

Citation Information

Patent Citations

  • Electroplating technology-based metal surface treatment method

    CN104018195A

  • Methods for applying layers to substrates, especially for electron microscopic preparation

    AT212050B

  • Process for preparing metal workpiece with composite ceramic film

    CN103014633A

  • Equipment and method for preparing high quality precision coating through deposition by adopting arc ion plating

    CN106801216A

  • Method and device for continuously preparing high-silicon steel thin strip through powder diffusion method

    CN108796427A