A harmless high value-added treatment method for polyvinyl chloride and its application

By reacting polyvinyl chloride and asphalt in a dispersant and performing heat treatment or activation treatment, disordered carbon and porous carbon materials are produced, which solves the problems of waste polyvinyl chloride treatment and asphalt resource utilization, and achieves efficient, environmentally friendly high-efficiency Added value utilization and material preparation with excellent properties.

CN116409778BActive Publication Date: 2024-10-22DALIAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310397060.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2024-10-22
Estimated Expiration
2043-04-13

AI Technical Summary

Technical Problem

Existing technology cannot effectively process waste polyvinyl chloride, resulting in environmental pollution and resource waste. At the same time, heavy organic asphalt fails to exert its excellent characteristics to achieve high value-added utilization, and the preparation process is complicated and costly.

Method used

Polyvinyl chloride, dechlorinating agent and asphalt are ultrasonically dispersed in a dispersant and then stirred and reacted. After heat treatment or activation treatment, disordered carbon and porous carbon materials are produced, which can be used in fields such as sodium-ion batteries, lithium-ion batteries and supercapacitors.

Benefits of technology

The harmless treatment of polyvinyl chloride is realized, the production cost is reduced, the added value utilization of the material is improved, the preparation process is simple, environmentally friendly, and the material performance is excellent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116409778B_ABST
    Figure CN116409778B_ABST
Patent Text Reader

Abstract

The present invention discloses a harmless high value-added treatment method for polyvinyl chloride and its application. The harmless high value-added treatment method for polyvinyl chloride comprises the following steps: adding polyvinyl chloride and a dechlorinating agent to a dispersant, ultrasonically dispersing, adding asphalt, stirring and mixing thoroughly, reacting at a certain temperature for a certain time, filtering, washing, and drying to obtain a precursor. The precursor is subjected to heat treatment in the presence of an inert gas to obtain a disordered carbon material; or the precursor is subjected to activation treatment in the presence of an activator to obtain a porous carbon material. The advantage of the present invention is that after simple treatment of polyvinyl chloride and asphalt, the dechlorination and detoxification of polyvinyl chloride are achieved, and disordered carbon and porous carbon are respectively prepared through carbonization or carbonization-activation, thereby successfully realizing the high value-added utilization of polyvinyl chloride and asphalt, and the prepared disordered carbon and porous carbon have excellent performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of chemical industry and environmental protection, and specifically relates to a harmless high-value-added treatment method for polyvinyl chloride and its application. Background Art

[0002] Polyvinyl chloride is a polymer material with excellent performance, which is widely used in packaging, construction and furniture industries. However, due to the widespread use of polyvinyl chloride, a large amount of waste polyvinyl chloride is produced every year in the world. At present, the main methods for treating waste plastics are incineration, landfill and microbial decomposition, wherein the release of hydrogen chloride and the formation of tetrachlorodibenzo-p-dioxin during incineration may cause secondary environmental pollution, landfill treatment may cause damage to soil and pollution of groundwater resources, and the microbial decomposition process is harsh and inefficient, so that waste polyvinyl chloride cannot be reasonably and effectively recovered and recycled. Polyvinyl chloride is a chlorinated hydrocarbon, so it is an excellent reaction precursor. At the same time, a large amount of asphalt (such as coal tar, petroleum asphalt and coal liquefaction asphalt) is also produced every year in the world. These heavy organic substances have the characteristics of high aromaticity, high carbon content and high reactivity. However, it is currently mainly used in the construction industry (such as paving, waterproof coatings, etc.), which cannot give play to the excellent properties of waste polyvinyl chloride to achieve its high added value utilization. Chinese patent CN109368646A discloses a method for preparing molybdenum carbide nanomaterials based on waste polyvinyl chloride, wherein a molybdenum-containing compound, waste polyvinyl chloride, metallic sodium and / or magnesium are placed in a reactor in a certain proportion, and then heated in an electric furnace. After the reaction is completed, the product is treated to successfully obtain molybdenum carbide nanomaterials. Chinese patent CN111359581B discloses a method for preparing heavy metal adsorbents using waste polyvinyl chloride plastics, wherein the waste polyvinyl chloride plastics are crushed, a catalyst is added to react to obtain a hydrothermal carbonization product, a sulfonated carbonization product is obtained after sulfuric acid sulfonation, and finally the sulfonated carbonization product is activated to obtain an adsorbent with heavy metal adsorption performance. The preparation process of the above method is relatively complicated and the yield is low, which also leads to high costs.

[0003] Therefore, in view of the shortcomings of the existing technology, the present invention utilizes the many excellent properties of polyvinyl chloride and asphalt to propose a simple, environmentally friendly and efficient polyvinyl chloride harmless high value-added treatment method and application. Summary of the invention

[0004] The purpose of the present invention is to provide a harmless high value-added treatment method and application of polyvinyl chloride.

[0005] The object of the present invention is to achieve the following:

[0006] A harmless high value-added treatment method for polyvinyl chloride mainly comprises the following steps:

[0007] Add polyvinyl chloride and dechlorinating agent to dispersant, disperse by ultrasonic, add asphalt, stir and mix thoroughly, react at a certain temperature for a certain time, filter, wash and dry to obtain precursor. The precursor is heat treated in the presence of inert gas to obtain disordered carbon material; or the precursor is activated in the presence of activator to obtain porous carbon material.

[0008] Furthermore, the asphalt is selected from one or both of coal-based asphalt and petroleum asphalt, and coal asphalt is preferred.

[0009] Furthermore, the dispersant is one or more of carbon disulfide, 1,2-dichloroethane, chloroform or carbon tetrachloride, preferably 1,2-dichloroethane.

[0010] Furthermore, the dechlorinating agent is one or more of anhydrous ferric chloride, anhydrous aluminum chloride, anhydrous tin tetrachloride, concentrated sulfuric acid, trifluoromethanesulfonic acid, p-toluenesulfonic acid, and oxalic acid, preferably anhydrous ferric chloride.

[0011] Furthermore, the mass ratio of the polyvinyl chloride to asphalt is 5:1-45.

[0012] Furthermore, the mass ratio of the polyvinyl chloride to the dechlorinating agent is 5:1-45.

[0013] Furthermore, the mass ratio of the polyvinyl chloride to the dispersant is 5:1 to 5000.

[0014] Furthermore, the reaction temperature is 20-200° C., and the reaction time is 1-60 hours.

[0015] Furthermore, the drying conditions are: vacuum drying at 50-140° C. for 1-60 hours.

[0016] Furthermore, the inert gas is one or more of nitrogen, argon or helium; the activator is one or a mixture of two or more of water vapor, carbon dioxide, oxygen, air, potassium hydroxide or sodium hydroxide, preferably carbon dioxide.

[0017] Furthermore, the inert gas flow rate is 10 to 100,000 mL / min.

[0018] Furthermore, the heat treatment temperature is 300-1600° C., and the heating rate is 2-30° C. / min.

[0019] Furthermore, the heat treatment time is 0.1 to 50 hours.

[0020] Furthermore, the mass ratio of the precursor to the activator is 10:1 to 10000.

[0021] Furthermore, the activation conditions are: activation temperature of 600-1500° C., heating rate of 1-20° C. / min, and activation time of 0.1-30 h.

[0022] Another aspect of the present invention is to provide disordered carbon and porous carbon materials prepared by the above method, wherein the disordered carbon materials are 002 The value is greater than 0.36nm, and the specific surface area of ​​porous carbon materials is greater than 500m 2 / g.

[0023] Another aspect of the present invention is to provide applications of the above-mentioned disordered carbon and porous carbon materials.

[0024] Furthermore, the above-mentioned disordered carbon material can be applied to electrode materials of sodium ion batteries, lithium ion batteries and potassium ion batteries.

[0025] Furthermore, the porous carbon material can be applied to fields such as adsorption materials, supercapacitor electrode materials and catalyst carriers.

[0026] Beneficial effects of the invention: The invention provides a harmless high-value-added treatment method and application of polyvinyl chloride, wherein a high-quality precursor is obtained by simple treatment, and then disordered carbon and porous carbon are obtained by heat treatment or activation. The preparation method can achieve the dechlorination and detoxification of polyvinyl chloride, as well as the high-value-added utilization of polyvinyl chloride and asphalt, and is time-saving, environmentally friendly, simple to operate, low in production cost, high in yield, and the prepared disordered carbon material has excellent sodium ion battery performance, and the prepared porous carbon material has good superelectric performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present invention, the drawings related to the embodiments are briefly introduced below.

[0028] Figure 1 XRD spectra of samples CP-1300 and PC-6h-1300 prepared in Example 6.

[0029] Figure 2 Nitrogen adsorption-desorption curves and DFT pore distribution curves of samples CP-900-4h and CP-6h-900-4h prepared in Example 7, (a) is the nitrogen adsorption-desorption curve, and (b) is the DFT pore distribution curve.

[0030] Figure 3 This is the sodium electrical rate performance diagram of sample PC-6h-1300 prepared for Application Example 1.

[0031] Figure 4 (a) Constant current charge-discharge curve and (b) specific capacitance diagram of sample CP-6h-900-4h prepared in Application Example 2 at different current densities. DETAILED DESCRIPTION

[0032] The present invention is described in detail below with reference to the embodiments, but the embodiments of the present invention are not limited thereto. Obviously, the embodiments described below are only partial embodiments of the present invention. For those skilled in the art, other similar embodiments obtained without creative labor all fall within the protection scope of the present invention.

[0033] Example 1

[0034] At room temperature, 1.5 g of polyvinyl chloride and 13 g of anhydrous ferric chloride were added to 150 mL of 1,2-dichloroethane and ultrasonically treated for 2 h. Then, 1.5 g of coal tar pitch (CP) was added and the mixture was placed in a 250 mL three-necked flask. Under a nitrogen atmosphere, the mixture was stirred at room temperature for 1 h, then heated to 80 ° C and stirred for 6 h. After the reaction, the solid product was filtered and washed with methanol and tetrahydrofuran respectively, and finally dried in a vacuum oven at 120 ° C for 12 h to obtain product A, marked as CP-6h.

[0035] Example 2

[0036] At room temperature, 1.5 g of polyvinyl chloride and 13 g of anhydrous ferric chloride were added to 150 mL of 1,2-dichloroethane and ultrasonically treated for 2 h. Then, 1.5 g of coal liquefaction pitch (CLA) was added and the mixture was placed in a 250 mL three-necked flask. Under a nitrogen atmosphere, the mixture was stirred at room temperature for 1 h, then heated to 80 ° C and stirred for 6 h. After the reaction, the solid product was filtered and washed with methanol and tetrahydrofuran respectively, and finally dried in a vacuum oven at 120 ° C for 12 h to obtain product B, marked as CLP-6h.

[0037] Example 3

[0038] At room temperature, 1.5 g of polyvinyl chloride and 13 g of anhydrous ferric chloride were added to 150 mL of 1,2-dichloroethane and ultrasonically treated for 2 h. Then, 1.5 g of petroleum asphalt (PA) was added and the mixture was placed in a 250 mL three-necked flask. Under a nitrogen atmosphere, the mixture was stirred at room temperature for 1 h, then heated to 80 ° C and stirred for 6 h. After the reaction, the solid product was filtered and washed with methanol and tetrahydrofuran respectively, and finally dried in a vacuum oven at 120 ° C for 12 h to obtain product C, which was marked as PP-6h.

[0039] Example 4

[0040] At room temperature, polyvinyl chloride and 13 g of anhydrous ferric chloride were added to 150 mL of 1,2-dichloroethane according to the mass ratio and reaction time in Table 1, and ultrasonically treated for 2 h. After adding coal tar, the mixture was placed in a 250 mL three-necked flask. Under a nitrogen atmosphere, it was first stirred at room temperature for 1 h, then heated to 80 ° C and stirred for reaction. After the reaction, the solid product was filtered and washed with methanol and tetrahydrofuran, respectively, and finally dried in a vacuum oven at 120 ° C for 12 h to obtain the products, which were marked as CP-0.5-6h, CP-2-6h, CP-3-6h, CP-0.5-24h, CP-2-24h, CP-3-24h and CP-24h, respectively.

[0041] Table 1 Mass ratio and reaction time

[0042]

[0043] Example 5

[0044] At room temperature, according to the type and mass of the dechlorinating agent in Table 2, 1.5 g of polyvinyl chloride and the dechlorinating agent were added to 150 mL of 1,2-dichloroethane, and ultrasonically treated for 2 h. After adding 1.5 g of coal tar, the mixture was placed in a 250 mL three-necked flask. Under a nitrogen atmosphere, it was first stirred at room temperature for 1 h, then heated to 80 ° C and stirred for 6 h. After the reaction, the solid product obtained by filtration was washed with methanol and tetrahydrofuran, respectively, and finally dried in a vacuum oven at 120 ° C for 12 h to obtain product D, which was marked as CP-Al-6h, CP-Sn-6h, CP-H-6h, CP-S-6h, CP-D-6h, and CP-C-6h, respectively.

[0045] Table 2 Types and quality of dechlorinating agents

[0046]

[0047] Example 6

[0048] Take 1.0g of the product CP-6h, place it in a tube furnace, and heat it to 1300℃ at a heating rate of 5℃ / min in an Ar atmosphere of 60mL / min, keep it for 2h and then cool it down naturally. The disordered carbon material is obtained, marked as CP-6h-1300. For comparison, the sample obtained by direct carbonization of coal tar (CP) according to the above method is marked as CP-1300. The XRD spectrum of the material is shown in the attached figure. Figure 1 The structural parameters are shown in Table 3.

[0049] Table 3 Structural parameters of samples CP-1300 and PC-6h-1300

[0050]

[0051] Example 7

[0052] Take 1.0 g of the product CP-6h and place it in a tube furnace at 60 mL min -1 In an Ar atmosphere, the temperature was raised to 900 °C at a rate of 10 °C / min and the flow rate was switched to 80 mL min -1 The activated carbon was then switched to 60 mL / min Ar atmosphere and cooled to room temperature to obtain a porous carbon material, which was labeled as CP-6h-900-4h. For comparison, the sample obtained by activation of coal tar pitch (CP) according to the above method was labeled as CP-900-4h. Figure 2 The pore structure parameters are shown in Table 4.

[0053] Table 4. Pore structure parameters of samples CP-900-4h and CP-6h-900-4h

[0054]

[0055] Example 8

[0056] 1.0 g of the product of Examples 2 to 5 was placed in a tube furnace, heated to 1300° C. at a heating rate of 10° C. / min in an Ar atmosphere of 60 mL / min, maintained for 2 h, and then cooled naturally to obtain a disordered carbon material.

[0057] Example 9

[0058] Take 1.0 g of the products of Examples 2 to 5, place them in a tubular furnace, heat them to 900°C at a heating rate of 10°C / min under an Ar atmosphere of 60 mL / min, switch to CO2 with a flow rate of 80 mL / min, activate them for 4 hours, and after completion, switch to an Ar atmosphere of 60 mL / min, cool to room temperature, and obtain a porous carbon material.

[0059] Application Example 1

[0060] The sample of Example 6 was used as a sodium ion battery electrode material for electrochemical testing. The assembly and testing methods were carried out according to the reference [Energy & Fuels [J]. 2021, 35 (10): 9029-9037]. The electrochemical test results are shown in the attached Figure 3 As shown, at a current density of 0.03 A / g, the specific capacity can reach 270 mA h / g and the first coulombic efficiency is 60%.

[0061] Application Example 2

[0062] The sample of Example 7 was used as a supercapacitor electrode material for electrochemical testing. The assembly and testing methods were carried out according to the reference [Carbon Technology [J]. 2022, 41(1): 6-11]. The test results are shown in the attached Figure 4 As shown, at a current density of 0.05 A / g, the specific capacitance is 159 F / g.

Claims

1. A method for harmless high value-added treatment of polyvinyl chloride, characterized in that: The method comprises the following steps: adding polyvinyl chloride and a dechlorinating agent into a dispersant, ultrasonically dispersing, adding asphalt, stirring and mixing thoroughly, reacting at a certain temperature for a certain time, filtering, washing and drying to obtain a precursor; subjecting the precursor to heat treatment in the presence of an inert gas to obtain a disordered carbon material; or subjecting the precursor to activation treatment in the presence of an activating agent to obtain a porous carbon material; the dechlorinating agent is one or more of anhydrous ferric chloride, anhydrous aluminum chloride, anhydrous tin tetrachloride, concentrated sulfuric acid, trifluoromethanesulfonic acid, p-toluenesulfonic acid and oxalic acid.

2. A harmless high value-added treatment method for polyvinyl chloride according to claim 1, characterized in that: The asphalt is selected from one or two of coal-based asphalt and petroleum asphalt; the dispersant is one or more of carbon disulfide, 1,2-dichloroethane, chloroform or carbon tetrachloride.

3. The harmless high value-added treatment method for polyvinyl chloride according to claim 1, characterized in that: The mass ratio of the polyvinyl chloride to asphalt is 5:1-45; the mass ratio of the polyvinyl chloride to the dechlorinating agent is 5:1-45; the mass ratio of the polyvinyl chloride to the dispersant is 5:1-5000.

4. The harmless high value-added treatment method for polyvinyl chloride according to claim 1, characterized in that: The reaction temperature is 20-200° C., and the reaction time is 1-60 hours. The drying conditions are: vacuum drying at 50-140° C. for 1-60 hours.

5. The harmless high value-added treatment method for polyvinyl chloride according to claim 1, characterized in that: The inert gas is one or more of nitrogen, argon or helium.

6. The harmless high value-added treatment method for polyvinyl chloride according to claim 1, characterized in that: The inert gas flow rate is 10 to 100,000 mL / min; the heat treatment temperature is 300 to 1,600° C., and the heating rate is 2 to 30° C. / min; and the heat treatment time is 0.1 to 50 h.

7. The harmless high value-added treatment method for polyvinyl chloride according to claim 1, characterized in that: The activator is one or a mixture of two or more of water vapor, carbon dioxide, oxygen, air, potassium hydroxide or sodium hydroxide.

8. The harmless high value-added treatment method for polyvinyl chloride according to claim 1, characterized in that: The mass ratio of the precursor to the activator is 10:1-10000; the activation conditions are: the activation temperature is 600-1500° C., the heating rate is 1-20° C. / min, and the activation time is 0.1-30h.

9. The disordered carbon and porous carbon material obtained by the harmless high value-added treatment method for polyvinyl chloride according to any one of claims 1 to 8, characterized in that: The disordered carbon material 002 The value is greater than 0.36nm, and the specific surface area of ​​porous carbon materials is greater than 500m 2 / g.

10. Application of disordered carbon and porous carbon materials obtained by the harmless high value-added treatment method for polyvinyl chloride according to any one of claims 1 to 8, characterized in that: Disordered carbon materials are used in sodium ion batteries, lithium ion batteries and potassium ion battery electrode materials; porous carbon materials are used in adsorption materials, supercapacitor electrode materials and catalyst carriers.