A preparation method of highly active renewable activated carbon for phosgene synthesis and its online regeneration process
By using nitrogen-containing aromatic ring compounds to prepare highly active renewable activated carbon, combined with an online regeneration process, the problem of short service life and safety risks of activated carbon for phosgene synthesis catalysts is solved, achieving long-term stable use of activated carbon and safe and efficient phosgene production. .
Patent Information
- Application Number
- CN202210020265.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-10
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-01-10
AI Technical Summary
The catalytic activity of the existing phosgene synthesis catalyst activated carbon decreases after prolonged use, resulting in an increase in the free chlorine content in the exported phosgene, affecting isocyanate production, and there are safety risks and production interruptions in the activated carbon disassembly and filling process, affecting the continuous production of phosgene .
Using nitrogen-containing aromatic ring compounds as raw materials, high-activity renewable activated carbon is prepared through polymerization reaction, pickling and extrusion molding, and an online regeneration process is developed to use high-temperature carbon monoxide and nitrogen to heat treat the deactivated activated carbon to remove chlorine-containing impurities. Restore the catalytic activity of activated carbon.
It extends the service life of activated carbon, reduces the loss of activated carbon, improves the activity of phosgene synthesis reaction, reduces production shutdown time due to activated carbon deactivation, avoids safety risks, and improves the stable operation cycle of the phosgene synthesis tower.
Smart Images

Figure BDA0003462209570000111 
Figure BDA0003462209570000191 
Figure BDA0003462209570000192
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method of highly active regenerable activated carbon suitable for phosgene synthesis and an online regeneration process thereof. Background Art
[0002] Phosgene is mainly used in organic synthesis, pesticides, drugs, dyes and other chemical intermediates. It is well known in the art that phosgene is continuously produced by catalytic synthesis of carbon monoxide and chlorine in a shell-and-tube reactor using activated carbon as a catalyst.
[0003] CN1765740A discloses a method and apparatus for producing phosgene, wherein chlorine and carbon monoxide react in the presence of an activated carbon catalyst in a shell-and-tube reactor, the reactor comprising a plurality of reaction tubes and a coolant space surrounding the reaction tubes, wherein a) the reaction tubes are cooled from the outside by the coolant space cooled by water evaporation, and b) during operation, the pressure of the reaction tubes is greater than the pressure in the coolant space.
[0004] CN102092713A discloses a method for producing phosgene by reacting chlorine with carbon monoxide, and specifically relates to a method for producing phosgene by reacting chlorine with carbon monoxide in a shell-and-tube reactor in the presence of an activated carbon catalyst. After chlorine and excess carbon monoxide are mixed in a mixer M1, they enter a tubular reactor, react to generate phosgene under the action of an activated carbon catalyst, and then pass through a protective reactor to ensure that the chlorine reacts completely; the heat generated by the reaction is extracted by a closed-loop 60°C cooling water system, and the generated gaseous phosgene enters a phosgene gas-liquid separation tank after two-stage condensation and cooling, and the uncondensed gas enters a tail gas absorption tower, and the phosgene contained in the tail gas is absorbed by -5°C toluene and recycled.
[0005] As the usage time of activated carbon as a phosgene synthesis catalyst continues to increase, the ability of activated carbon to catalyze phosgene synthesis slowly decreases, resulting in a continuous increase in the free chlorine content in the exported synthetic phosgene.
[0006] Phosgene and amines can react to synthesize isocyanates, such as toluene diisocyanate (TDI), 4,4'-diphenylmethane diisocyanate (MDI), hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), etc. At present, isocyanates are mainly prepared by the phosgene method. The corresponding amines such as diphenylmethane diamine and polymethylene polyphenyl polyamines are mixed with an inert solvent and then fully mixed with phosgene for phosgenation to obtain a photochemical reaction liquid. The photochemical reaction liquid is removed by phosgene and solvent to obtain a crude isocyanate. The chlorine in phosgene will cause the reaction to produce a large amount of chlorinated by-products and acids, so that the crude isocyanate contains a large amount of acid and hydrolyzed chlorine, which affects its appearance color. Therefore, it is necessary to ensure that the free chlorine content in the raw material phosgene used for isocyanate production is low.
[0007] In the conventional isocyanate manufacturing technology, when the catalytic activity of the activated carbon in the phosgene synthesis tower drops significantly, the plant needs to be stopped to replace the activated carbon in the phosgene synthesis tower to ensure that the free chlorine contained in the phosgene has no adverse effect on the product. Since there are residual phosgene, chlorine and other hazardous materials in the activated carbon, it is necessary to remove these toxic and harmful hazardous materials before the synthesis tower can be opened and the catalyst can be replaced.
[0008] CN105817183A discloses a method for quickly removing phosgene from a catalyst when replacing a phosgene synthesis tower catalyst. The method uses nitrogen to purge the phosgene adsorbed on the activated carbon of the phosgene synthesis tower catalyst, which is easy to desorb, and then purges with ammonia, and the ammonia reacts with the phosgene in the phosgene synthesis tower catalyst that is difficult to desorb to remove it. After the purge, the phosgene content at the outlet of the phosgene synthesis tower is less than 0.5ppm, which can significantly reduce the time for purging phosgene from the phosgene synthesis tower, greatly reduce the nitrogen consumption, and improve the safety of the process operation.
[0009] In the above documents and other prior arts, it is described that the residual phosgene in the catalyst of the phosgene synthesis tower is removed by using purge gases such as hot nitrogen and ammonia, which significantly reduces the phosgene purge time of the phosgene synthesis tower. However, since activated carbon has a certain adsorption capacity and can adsorb part of the phosgene and chlorine, there are still certain risks in the process of removing the activated carbon. At the same time, it still takes about 15-30 days to purge the synthesis tower, remove the activated carbon, and fill the activated carbon. The long operation time affects the continuous production of phosgene, and then affects the production and operation load of the phosgene-using devices downstream of the industrial chain.
[0010] Therefore, a more convenient and safer technical solution is needed to reduce the impact of reduced activated carbon catalytic activity on the continuous synthesis production of phosgene. Summary of the invention
[0011] The inventors analyzed and studied fresh activated carbon and activated carbon used for phosgene synthesis for 1-2 years and found that the iodine adsorption value of activated carbon with reduced activity or lost activity showed a relatively obvious decrease, from 800-1200 mg / g to 500-700 mg / g; the total carbon content of activated carbon showed a significant decrease, from 85-95% to 40-60%, and correspondingly, the volatile matter of activated carbon increased from 0-5% to 15-45%. It is speculated that in the process of phosgene synthesis, the chlorine element forms a strong binding state with the activated carbon, occupies part of the catalytic active sites, resulting in a decrease in the catalytic activity of the activated carbon. Therefore, a method for preparing highly active activated carbon can be developed to improve the phosgene synthesis reaction activity of activated carbon and extend the service life of activated carbon. At the same time, a technology can be developed to monitor the activity of activated carbon in the process of phosgene synthesis online, and chlorine-containing impurities in deactivated activated carbon can be removed online to restore the phosgene catalytic activity of activated carbon and reduce the influence of activated carbon deactivation on the continuous production of phosgene.
[0012] The inventors also found that after 1-2 years of industrial use of conventional commercially available activated carbon in catalytic phosgene synthesis reaction, the total volume of activated carbon loses about 40%-60%, so it is inevitable to open the equipment to replenish the activated carbon, which brings the risk of safety and production loss. Therefore, reducing the loss of activated carbon during use so that the volume of activated carbon after use is more than 85% of that before use is a prerequisite for activated carbon regeneration.
[0013] One of the purposes of the present invention is to provide a method for preparing highly active activated carbon suitable for phosgene synthesis. The method uses nitrogen-containing aromatic ring compounds as raw materials, undergoes polymerization reaction, acid washing, and finally adopts extrusion molding. After aging, drying, and roasting, highly active renewable activated carbon is obtained. The service life of the activated carbon can be increased by more than 50%, and the loss of activated carbon after 1-2 years of use is less than 15% (volume ratio).
[0014] Aromatic compounds containing nitrogen can form a stable network polymer under the action of a catalyst, and nitrogen-doped activated carbon powder can be obtained after high-temperature treatment. When the nitrogen in the raw material is pyridine-type, pyridine-type nitrogen can be introduced into the activated carbon. This nitrogen has a very strong electron-withdrawing property, which will significantly increase the positive charge density on the adjacent carbon atoms, making it easier for Cl2 adsorbed on the surface of the activated carbon in the phosgene synthesis reaction to activate and form Cl free radicals, thereby accelerating the phosgene synthesis reaction rate and improving the reaction activity of the activated carbon.
[0015] After analyzing and comparing the metal content and service life of different activated carbons, it was found that the metal elements contained in activated carbon, such as iron and aluminum, have a significant effect of catalyzing the reaction of chlorine and carbon to form small molecular chlorinated alkanes, which leads to the destruction of the activated carbon skeleton structure, and then leads to carbon loss, resulting in significant volume loss of activated carbon. Therefore, the use of acid washing process to remove metals in activated carbon is one of the important means to increase the life of activated carbon and reduce the loss of activated carbon in the process of phosgene synthesis.
[0016] The second purpose of the present invention is to provide a process for online regeneration of activated carbon for phosgene synthesis. The process uses high-temperature carbon monoxide and high-temperature nitrogen to heat-treat the deactivated activated carbon, which can remove more than 80% of the chlorine-containing impurities in the deactivated activated carbon, and restore the iodine adsorption value and total carbon content of the activated carbon to 80-90% of the level of fresh activated carbon. The catalytic phosgene synthesis activity of the activated carbon is restored, which can effectively reduce the shutdown time of the phosgene production device due to the reduction of the activated carbon activity, extend the period of stable operation of the device, and avoid the safety risks caused by the disassembly of the activated carbon containing phosgene.
[0017] In order to achieve the above purpose, the present invention adopts the following technical solution:
[0018] The present invention provides a method for preparing highly active renewable activated carbon suitable for phosgene synthesis, comprising the following steps:
[0019] 1) The nitrogen-containing aromatic compound is reacted at high temperature for a certain period of time under the protection of inert gas with anhydrous ZnCl2 as a catalyst to obtain a black powder. The powder is washed to remove the unreacted raw materials, and then mixed with ordinary carbon powder in a certain proportion, and further acid-washed at a certain temperature to remove metal ions, and then the powder is washed and dried to obtain raw carbon powder;
[0020] 2) The carbon powder and the binder are uniformly mixed and kneaded into a plastic embryo, extruded into strips, and then aged, dried and calcined to obtain activated carbon suitable for phosgene synthesis.
[0021] In the preparation method, in step 1), the nitrogen-containing aromatic ring compound used is one or more of 1,4-dicyanobenzene, 2,6-naphthalenedicarboxylic acid, and 1,3,5-3-cyanobenzene, the molar ratio of the nitrogen-containing aromatic ring compound to the catalyst anhydrous ZnCl2 is selected from 3:1-7:1, the inert gas is nitrogen, the reaction temperature is selected from 300-500°C, and the reaction time is selected from 20-60h.
[0022] In the preparation method, in step 1), the cleaning method for removing unreacted raw materials from the powder is to use 2% dilute hydrochloric acid 10-30 times the mass of the powder to clean it 1-3 times, and then use deionized water 25-75 times the mass of the powder to clean it 1-3 times.
[0023] In the preparation method, in step 1), the carbon powder used for blending is commercially available coconut shell activated carbon or coal-based activated carbon powder, and the blending ratio is 1:1-1:4 of the carbon powder prepared from the nitrogen-containing aromatic ring compound in step 1).
[0024] In the preparation method, in step 1), the method of removing metal ions in the powder by pickling is to heat the powder under reflux in a 10% nitric acid solution at 90-100°C for 1-4h, and the powder after pickling is washed with deionized water 25-75 times the mass of the powder 1-3 times, and then dried to constant weight at 100-150°C in a nitrogen atmosphere.
[0025] The preparation method, step 2) can refer to the activated carbon preparation method provided in claims 8 and 9 of patent CN110449147. The binder is a hydrochloric acid solution of polyvinyl alcohol and glutaraldehyde, the mass ratio of polyvinyl alcohol to glutaraldehyde is 10-50:1, preferably 15-40:1; and / or, the molecular weight of the polyvinyl alcohol is 20000-150000, more preferably 50000-120000; and / or, the mass concentration of the hydrochloric acid solution of glutaraldehyde is 0.5-20%, preferably 1-5%. Polyvinyl alcohol and glutaraldehyde hydrochloric acid solutions are added to the mixed powder in sequence, the mass ratio of the binder solution to the carbon powder is 5:1-15:1; and the mixture is kneaded and extruded into strips, preferably with a diameter of 1-5 mm and a length of 1-10 mm. The aging is carried out at room temperature, preferably at 20-30°C; the aging time is 1-5h, preferably 2-4h; and / or, the drying is carried out at a drying temperature of 80-150°C, preferably 100-130°C; the drying time is 1-24h, preferably 2-18h; and / or, the calcination is carried out in an argon atmosphere, the calcination temperature is 700-1000°C, preferably 750-900°C; the calcination time is 1-5h, preferably 2-5h.
[0026] The present invention also provides a method for phosgene synthesis and online regeneration of activated carbon catalyst, which comprises the following steps:
[0027] 1) introducing premixed CO and chlorine into a phosgene synthesis tower, and reacting CO and chlorine to synthesize phosgene under the action of a catalyst; the phosgene synthesis tower is a tube-and-tube fixed bed reactor, the tubes are filled with catalysts, and multi-point thermometers are installed in some of the tubes, and a high-temperature resistant heat-conducting medium is used outside the tubes to absorb the reaction heat generated by synthesizing phosgene; the catalyst is the above-mentioned highly active activated carbon;
[0028] 2) When the highest temperature point in the activated carbon bed in the phosgene synthesis tower moves back to a certain position, the phosgene synthesis activity of the activated carbon decreases, the residual chlorine content in the synthetic phosgene increases, and the activated carbon in the phosgene synthesis tower is converted into deactivated activated carbon; at this time, the activated carbon is regenerated online, the phosgene synthesis tower system is pretreated, and then the deactivated activated carbon is regenerated online using high-temperature carbon monoxide and high-temperature nitrogen.
[0029] The process of phosgene synthesis and online regeneration of activated carbon catalyst, in step 1), an electric heater is provided at the entrance of the phosgene synthesis tower, which can heat carbon monoxide or nitrogen to 300-600°C; the phosgene synthesis tower is two-stage, the first stage is a tube-type fixed bed reactor, the tube length is selected from 2-6m, and the second stage is a random fixed bed reactor; the heat transfer medium outside the tube of the first-stage phosgene synthesis tower (shell side) comes from a closed circulation system, the system is provided with a medium cooler for phosgene synthesis conditions, a heat transfer medium storage tank is provided for storing heat transfer medium under activated carbon regeneration conditions, and a vacuum system is provided for extracting gas in the shell side space to form a negative pressure or vacuum environment; a multi-point thermometer is installed in the first-stage phosgene synthesis tower to monitor the temperature of the activated carbon bed in the tube.
[0030] In the process of phosgene synthesis and online regeneration of activated carbon catalyst, in step 1), the heat-conducting medium is selected from high-temperature resistant silicone oil, high-temperature resistant mineral oil or molten salt; the heat-conducting medium is circulated in a closed manner in the system, and a cooler is designed on the circulation pipeline; the cooling medium of the cooler is selected from brine, water, and chlorobenzene, preferably brine and chlorobenzene; a heat-conducting medium storage tank is provided in the system, which can be used to recover and store all the heat-conducting medium in the system.
[0031] In the process of phosgene synthesis and online regeneration of activated carbon catalyst, in step 1), multi-point thermometers are installed in some tubes in the synthesis tower, and the number of installations is selected from 1 multi-point thermometer / 200 tubes to 1 multi-point thermometer / 100 tubes. The positions of the multi-point thermometers are set to be evenly distributed to monitor the radial hot spot temperature of the synthesis tower; the number of temperature measurement points on the multi-point thermometer is selected from 4 / m to 10 / m and is evenly distributed.
[0032] The process of phosgene synthesis and online regeneration of activated carbon catalyst, in step 1), the catalyst used is highly active regenerable activated carbon, which is evaluated by the phosgene synthesis activity evaluation method of activated carbon described in this patent, and the specific method is as follows: the activated carbon is powdered and crushed, and dehydrated at 110°C in a nitrogen atmosphere for 2 hours to obtain activated carbon with a water content of less than 0.5%; the activated carbon is loaded into a tube array, and an electric heating furnace is used to heat the activated carbon in the tube array and maintain the temperature of the activated carbon in the tube array constant at 50°C ; A chlorine / nitrogen mixture is introduced into the inlet of the tube array. The volume ratio of chlorine in the mixture is 10%. The residence time of the mixed gas flow rate in the activated carbon bed is 60s, so that the activated carbon can fully adsorb the chlorine. The concentration of chlorine in the mixed gas at the outlet is detected by ultraviolet-visible spectroscopy. When the chlorine concentration in the mixed gas is the same as that in the inlet gas, the chlorine introduction is stopped, and the chlorine adsorption amount is calculated based on the concentration change curve measured by ultraviolet-visible spectroscopy, which is recorded as m1; a small amount of nitrogen is used to blow out the chlorine in the tube array and unload the activated carbon. The activated carbon which has adsorbed chlorine to saturation is heated to 325-375°C by an electric heating furnace, and nitrogen is introduced at a certain rate at the inlet of the tube array, and the nitrogen flow rate is 10m / s, so that the chlorine adsorbed by the activated carbon is removed; the activated carbon after chlorine desorption is loaded into the tube array, and the activated carbon in the tube array is heated by an electric heating furnace and the temperature of the activated carbon in the tube array is maintained constant at 50°C; a chlorine / nitrogen mixed gas is introduced at the inlet of the tube array, the volume ratio of chlorine in the mixed gas is 10%, and the residence time of the mixed gas flow rate in the activated carbon bed is 60s, so that the activated carbon fully adsorbs chlorine, and the concentration of chlorine in the mixed gas at the outlet is detected by ultraviolet-visible spectroscopy. When the chlorine concentration in the mixed gas is the same as that in the inlet gas, the chlorine introduction is stopped, and the chlorine adsorption amount is calculated according to the concentration change curve measured by ultraviolet-visible spectroscopy, which is recorded as m2; a small amount of nitrogen is used to blow out the chlorine in the tube array and unload the activated carbon. The highly active regenerable activated carbon described in this patent has an m2 / m1 value of 0.7-1, preferably 0.8-1.
[0033] The inventor measured the temperature in the phosgene synthesis tower and found that under normal circumstances, the temperature of the temperature measuring points at different heights in the phosgene synthesis tower first rises gently, then rises sharply after exceeding a certain temperature, and then slowly decreases after rising to the highest temperature point; as the operation time of the phosgene synthesis tower increases, the position of the highest temperature point will slowly move away from the outlet. It is well known that the phosgene synthesis reaction is an exothermic reaction. If this part of the heat is not removed in time, it will accumulate in the gas and activated carbon. As the temperature rises, the rate of the phosgene synthesis reaction is further accelerated. Therefore, under the condition of adiabatic or low heat transfer rate, the phosgene synthesis reaction can be considered as a self-accelerating reaction. The inventor believes that the activated carbon between the inlet and the point where the temperature rises sharply belongs to activated carbon with low catalytic activity. The reaction progress of phosgene synthesis in this part of activated carbon is low, so the temperature rises very slowly; as the operation time of the phosgene synthesis tower increases, the amount of activated carbon with low catalytic activity in this part continues to increase, causing the highest temperature point to move backward continuously. Therefore, the appropriate time point for implementing the activated carbon regeneration process can be indicated by establishing a relationship between the distance from the inlet to the point where the temperature rises sharply and the free chlorine content in the synthesized phosgene at the outlet of the phosgene synthesis tower.
[0034] In the process of phosgene synthesis and online regeneration of activated carbon catalyst, in step 2), the position of the highest temperature point in the activated carbon bed in the phosgene synthesis tower is moved back to a certain position by measuring the free chlorine content in the outlet phosgene. The specific guidance is that when the free chlorine in the outlet synthetic phosgene is higher than a certain value, the activated carbon in the phosgene synthesis tower is converted into deactivated activated carbon. The distance between the highest temperature point in the bed and the inlet of the phosgene synthesis tower tube array is 1.5-3.2m, and the corresponding chlorine content in the phosgene at the reactor outlet is 300-1500ppm.
[0035] In the process of phosgene synthesis and online regeneration of activated carbon catalyst, in step 2), before online regeneration of deactivated activated carbon using high-temperature carbon monoxide and high-temperature nitrogen, it is necessary to recover the heat transfer medium on the shell side of the phosgene synthesis tower into a heat transfer medium storage tank, and make the shell side in a low pressure or vacuum state through a vacuum system to avoid heat dissipation on the shell side. The shell side pressure is selected from 20-80 kpa (A), preferably 40-60 kpa.
[0036] In the process of phosgene synthesis and online regeneration of activated carbon catalyst, in step 2), high-temperature carbon monoxide is used to desorb the weakly adsorbed chlorine in the activated carbon bed, and the heating temperature of the high-temperature carbon monoxide is selected from 200-400°C, preferably 250-350°C, and more preferably 275-325°C; the axial flow rate of carbon monoxide in the activated carbon bed is 10-20m / s, preferably 12-18m / s; the carbon monoxide desorption treatment time is selected from 2-12h, preferably 4-10h;
[0037] In the process of phosgene synthesis and online regeneration of activated carbon catalyst, in step 2), high-temperature nitrogen is used to desorb the strongly adsorbed chlorine in the activated carbon bed and remove the chlorine-containing impurities strongly bound to the activated carbon. The heating temperature of the high-temperature nitrogen is selected from 400-600°C, preferably 450-550°C, and more preferably 475-525°C; the axial flow rate of nitrogen in the activated carbon bed is 5-15m / s, preferably 8-12m / s; the nitrogen desorption treatment time is selected from 24-48h, preferably 32-40h.
[0038] In the process of phosgene synthesis and online regeneration of activated carbon catalyst, in step 2), the iodine adsorption value of the activated carbon after online regeneration is increased to 70-90% of the level of fresh activated carbon, and the total carbon content is 85-95%.
[0039] In the process of phosgene synthesis and online regeneration of activated carbon catalyst, in step 2), after the activated carbon has been online regenerated, fresh chlorine and carbon monoxide are added again to carry out phosgene synthesis reaction, the ratio of the distance from the hot spot temperature position in the activated carbon bed to the tube inlet to the total length of the tube is between 0.1-0.4, and the free chlorine content in the outlet synthetic phosgene is less than 500ppm. DETAILED DESCRIPTION
[0040] The present invention will be further described below with examples, but the present invention is not limited thereto.
[0041] The chlorine content in phosgene is determined by the following method:
[0042] (1) Detection principle:
[0043] Cl2+2KI→2KCl+I2
[0044] I2+2Na2S2O3→2NaI+Na2S4O6
[0045] (2) Detection process:
[0046] Prepare enough KI solution, freeze the phosgene sampling bottle and connect it to the glass funnel, add KI solution to the glass funnel, open the middle connecting valve to allow the KI solution to fully absorb the chlorine in the phosgene, and then titrate with the prepared Na2S2O3 standard solution until the KI solution changes from purple-red to colorless.
[0047] (3) Calculation method of chlorine in phosgene
[0048]
[0049] Wherein, Cl is the content of chlorine in phosgene, mg / L;
[0050] V1 is the volume of Na2S2O3 standard solution consumed in titration, ml;
[0051] V2 is the volume of the gas sampling bottle, L;
[0052] C is the actual concentration of Na2S2O3 standard solution, mol / L.
[0053] The iodine adsorption value in activated carbon is measured with reference to the national standard GB / T 12496.8-1999;
[0054] The total carbon content of activated carbon was determined using a solid TOC analyzer;
[0055] The phosgene synthesis activity index m2 / m1 of activated carbon is determined by the following method:
[0056] The activated carbon is sieved for powder and crushed particles, and dehydrated at 110°C in a nitrogen atmosphere for 2 hours to obtain activated carbon with a water content of less than 0.5%; the activated carbon is loaded into a tube array, and an electric heating furnace is used to heat the activated carbon in the tube array and maintain the temperature of the activated carbon in the tube array constant at 50°C; a chlorine / nitrogen mixed gas is introduced at the inlet of the tube array, the volume ratio of chlorine in the mixed gas is 10%, and the residence time of the mixed gas flow rate in the activated carbon bed is 60s, so that the activated carbon fully adsorbs chlorine, and the concentration of chlorine in the mixed gas at the outlet is detected by ultraviolet-visible spectroscopy. When the chlorine concentration in the mixed gas is the same as that in the inlet gas, the chlorine introduction is stopped, and the chlorine adsorption amount is calculated according to the concentration change curve measured by ultraviolet-visible spectroscopy, which is recorded as m1; a small amount of nitrogen is used to blow out the chlorine in the tube array and unload the activated carbon.
[0057] The activated carbon that has adsorbed chlorine to saturation is heated to 350°C by an electric heating furnace, and nitrogen is introduced at a certain rate at the inlet of the tube array, with a nitrogen flow rate of 10m / s, so that the chlorine adsorbed by the activated carbon is removed;
[0058] The activated carbon after chlorine desorption is loaded into the tube array, and the activated carbon in the tube array is heated by an electric heating furnace and the temperature of the activated carbon in the tube array is maintained at a constant 50°C; a chlorine / nitrogen mixed gas is introduced at the inlet of the tube array, the volume ratio of chlorine in the mixed gas is 10%, and the residence time of the mixed gas flow rate in the activated carbon bed is 60s, so that the activated carbon can fully adsorb chlorine, and the concentration of chlorine in the mixed gas at the outlet is detected by ultraviolet-visible spectroscopy. When the chlorine concentration in the mixed gas is the same as that in the inlet gas, the chlorine introduction is stopped, and the chlorine adsorption amount is calculated according to the concentration change curve measured by ultraviolet-visible spectroscopy, which is recorded as m2; a small amount of nitrogen is used to blow out the chlorine in the tube array and unload the activated carbon.
[0059] The activated carbon powder used for blending in the following Examples 1, 2, and 3 was purchased from NORIT Company and obtained by crushing the activated carbon with the brand name RB4C.
[0060] Example 1
[0061] Under nitrogen protection, 1,4-dicyanobenzene was added with anhydrous ZnCl2 as a catalyst in a molar ratio of 5:1, and reacted at 500°C for 40 hours to obtain a black powder. The powder was washed three times with 2% dilute hydrochloric acid in a mass ratio of 1:20 (powder: cleaning agent), and washed twice with deionized water in a mass ratio of 1:75 to remove the unreacted raw materials. The obtained carbon powder was blended with commercially available activated carbon powder in a mass ratio of 1:1. The powder was heated to reflux in a 10% nitric acid solution at 100°C for 3 hours for acid washing to remove metal ions in the activated carbon. The acid-washed powder was washed three times with deionized water in a mass ratio of 1:50, and then dried to constant weight at 140°C in a nitrogen atmosphere. Polyvinyl alcohol and hydrochloric acid solution of glutaraldehyde are added to the mixed powder in sequence, the mass ratio of polyvinyl alcohol to glutaraldehyde is 30:1, the molecular weight of polyvinyl alcohol is 150000, the mass concentration of hydrochloric acid solution of glutaraldehyde is 0.5%, and the mass ratio of binder solution to carbon powder is 10:1; the mixed powder is kneaded and extruded into strips with a diameter of 4mm and a length of 7mm. Ripen at 25°C for 5h, dry at 80°C for 24h, and then calcine in an argon atmosphere at a calcination temperature of 1000°C for 1h.
[0062] Example 2
[0063] Under nitrogen protection, 1,4-dicyanobenzene was added with anhydrous ZnCl2 as a catalyst in a molar ratio of 3:1, and reacted at 400°C for 55h to obtain a black powder. The powder was washed once with 2% dilute hydrochloric acid in a mass ratio of 1:20 (powder: cleaning agent), and once with deionized water in a mass ratio of 1:50 to remove the unreacted raw materials. The obtained carbon powder was blended with commercially available activated carbon powder in a mass ratio of 1:4. The powder was heated to reflux in a 10% nitric acid solution at 100°C for 4h for acid washing to remove metal ions in the activated carbon. The acid-washed powder was washed twice with deionized water in a mass ratio of 1:25, and then dried to constant weight at 100°C in a nitrogen atmosphere. The carbon powder was mixed evenly with the binder and kneaded into a plastic embryo, extruded into strips, and then aged, dried, and calcined to obtain activated carbon suitable for phosgene synthesis. Polyvinyl alcohol and hydrochloric acid solution of glutaraldehyde are added to the mixed powder in sequence, the mass ratio of polyvinyl alcohol to glutaraldehyde is 10:1, the molecular weight of polyvinyl alcohol is 20000, the mass concentration of hydrochloric acid solution of glutaraldehyde is 5%, and the mass ratio of binder solution to carbon powder is 15:1; the mixed powder is kneaded and extruded into strips with a diameter of 1mm and a length of 10mm. Ripen at 20°C for 1h, dry at 150°C for 1h, and then calcine in an argon atmosphere at a calcination temperature of 850°C for 3h.
[0064] Example 3
[0065] Under nitrogen protection, 1,4-dicyanobenzene was added with anhydrous ZnCl2 in a molar ratio of 7:1 as a catalyst, and reacted at 300°C for 30 hours to obtain a black powder. The powder was washed twice with 2% dilute hydrochloric acid in a mass ratio of 1:20 (powder: cleaning agent), and washed three times with deionized water in a mass ratio of 1:25 to remove the unreacted raw materials. The obtained carbon powder was blended with commercially available activated carbon powder in a mass ratio of 1:2.5. The powder was heated to reflux in a 10% nitric acid solution at 100°C for 2 hours for acid washing to remove metal ions in the activated carbon. The acid-washed powder was washed once with deionized water in a mass ratio of 1:75, and then dried to constant weight at 120°C in a nitrogen atmosphere. The carbon powder was mixed evenly with the binder and kneaded into a plastic embryo, extruded into strips, and then aged, dried, and calcined to obtain activated carbon suitable for phosgene synthesis. Polyvinyl alcohol and hydrochloric acid solution of glutaraldehyde are added to the mixed powder in sequence, the mass ratio of polyvinyl alcohol to glutaraldehyde is 50:1, the molecular weight of polyvinyl alcohol is 80000, the mass concentration of hydrochloric acid solution of glutaraldehyde is 20%, and the mass ratio of binder solution to carbon powder is 5:1; the mixed powder is kneaded and extruded into strips with a diameter of 5mm and a length of 1mm. Ripen at 30°C for 3h, dry at 120°C for 12h, and then calcine in an argon atmosphere at a calcination temperature of 700°C for 5h.
[0066] The highly active activated carbon prepared in Examples 1, 2, and 3 is applied to industry, and its use method and regeneration process are described in Examples 4, 5, and 6.
[0067] Example 4
[0068] The premixed CO and chlorine are introduced into a phosgene synthesis tower, and the CO and chlorine react to synthesize phosgene under the action of a catalyst; the phosgene synthesis tower is a tube-and-tube fixed bed reactor, the tube length is 3m, and the tubes are filled with an activated carbon catalyst, which is the catalyst prepared in Example 1. The catalyst has an m2 / m1 value of 0.86 using the aforementioned activated carbon evaluation method, and multi-point thermometers are installed in some tubes. The number of multi-point thermometers installed is 1 / 100 tubes, and the density of temperature measuring points on the thermometer is 6 / m. High-temperature resistant mineral oil is used outside the tube to absorb the reaction heat generated by synthesizing phosgene; a cooler is provided in the phosgene synthesis system to cool the heat-conducting medium after absorbing the reaction heat, and the heat-conducting medium is brine.
[0069] When the hot spot temperature position in the activated carbon bed in the phosgene synthesis tower is greater than 2m from the tube inlet, and the residual chlorine content in the synthetic phosgene is higher than 300ppm, it indicates that the activated carbon in the phosgene synthesis tower is converted into deactivated activated carbon; the operating cycle from the use of activated carbon to the deactivated state is calculated, and the volume loss of activated carbon in the tube is measured. At this time, it is necessary to recover the heat transfer medium on the shell side of the phosgene synthesis tower into the heat transfer medium storage tank, and make the shell side pressure 50kpaA through the vacuum system. Use 350℃ carbon monoxide to desorb the weakly adsorbed chlorine in the activated carbon bed; the axial flow rate of carbon monoxide in the activated carbon bed is 15m / s; the carbon monoxide desorption treatment time is 2h; the next step is to use 500℃ nitrogen to desorb the strongly adsorbed chlorine in the activated carbon bed and remove the chlorine-containing impurities strongly bound to the activated carbon; the axial flow rate of nitrogen in the activated carbon bed is 10m / s; the nitrogen desorption treatment time is 36h;
[0070] After the activated carbon is regenerated, it is put back into use with reference to the operating process parameters before regeneration, and the hot spot temperature position of the activated carbon bed in the tubes and the content of free chlorine in the outlet phosgene are measured.
[0071] Example 5
[0072] The premixed CO and chlorine are introduced into a phosgene synthesis tower, and CO and chlorine react to synthesize phosgene under the action of a catalyst; the phosgene synthesis tower is a tube-and-tube fixed bed reactor, the tube length is 5m, and the tubes are filled with an activated carbon catalyst, which is the catalyst prepared in Example 2. The catalyst has an m2 / m1 value of 0.77 using the aforementioned activated carbon evaluation method, and multi-point thermometers are installed in some tubes. The number of multi-point thermometers installed is 1 / 150 tubes, and the density of temperature measuring points on the thermometer is 4 / m. High-temperature resistant silicone oil is used outside the tube to absorb the reaction heat generated by synthesizing phosgene; a cooler is provided in the phosgene synthesis system to cool the heat-conducting medium after absorbing the reaction heat, and the heat-conducting medium is water.
[0073] When the hot spot temperature position in the activated carbon bed in the phosgene synthesis tower is greater than 3.2m from the tube inlet, and the residual chlorine content in the phosgene is higher than 1500ppm, it indicates that the activated carbon in the phosgene synthesis tower is converted into deactivated activated carbon; the operating cycle from the activated carbon being put into use to reaching the deactivated state is calculated, and the volume loss of the activated carbon in the tube is measured. At this time, it is necessary to recover the heat transfer medium on the shell side of the phosgene synthesis tower into the heat transfer medium storage tank, and make the shell side pressure 80kpaA through the vacuum system. Use 300℃ carbon monoxide to desorb the weakly adsorbed chlorine in the activated carbon bed; the axial flow rate of carbon monoxide in the activated carbon bed is 10m / s; the carbon monoxide desorption treatment time is 8h; the next step is to use 400℃ nitrogen to desorb the strongly adsorbed chlorine in the activated carbon bed and remove the chlorine-containing impurities strongly bound to the activated carbon; the axial flow rate of nitrogen in the activated carbon bed is 8m / s; the nitrogen desorption treatment time is 44h;
[0074] After the activated carbon is regenerated, it is put back into use with reference to the operating process parameters before regeneration, and the hot spot temperature position of the activated carbon bed in the tubes and the content of free chlorine in the outlet phosgene are measured.
[0075] Example 6
[0076] The premixed CO and chlorine are introduced into a phosgene synthesis tower, and CO and chlorine react to synthesize phosgene under the action of a catalyst; the phosgene synthesis tower is a tube-and-tube fixed bed reactor, the tube length is 2m, and the tubes are filled with an activated carbon catalyst, which is the catalyst prepared in Example 3. The catalyst has an m2 / m1 value of 0.81 using the aforementioned activated carbon evaluation method, and multi-point thermometers are installed in some tubes. The number of multi-point thermometers installed is 1 / 200 tubes, and the density of temperature measuring points on the thermometer is 8 / m. High-temperature resistant silicone oil is used outside the tube to absorb the reaction heat generated by synthesizing phosgene; a cooler is provided in the phosgene synthesis system to cool the heat-conducting medium after absorbing the reaction heat, and the heat-conducting medium is chlorobenzene.
[0077] When the hot spot temperature position in the activated carbon bed in the phosgene synthesis tower is greater than 1.5m from the tube inlet, and the residual chlorine content in the phosgene is higher than 750ppm, it indicates that the activated carbon in the phosgene synthesis tower is converted into deactivated activated carbon; the operating cycle from the activated carbon being put into use to reaching the deactivated state is calculated, and the volume loss of the activated carbon in the tube is measured. At this time, it is necessary to recover the heat transfer medium on the shell side of the phosgene synthesis tower into the heat transfer medium storage tank, and make the shell side pressure 20kpaA through the vacuum system. Use 200℃ carbon monoxide to desorb the weakly adsorbed chlorine in the activated carbon bed; the axial flow rate of carbon monoxide in the activated carbon bed is 20m / s; the carbon monoxide desorption treatment time is 12h; the next step is to use 600℃ nitrogen to desorb the strongly adsorbed chlorine in the activated carbon bed and remove the chlorine-containing impurities strongly bound to the activated carbon; the axial flow rate of nitrogen in the activated carbon bed is 15m / s; the nitrogen desorption treatment time is 28h;
[0078] After the activated carbon is regenerated, it is put back into use with reference to the operating process parameters before regeneration, and the hot spot temperature position of the activated carbon bed in the tubes and the content of free chlorine in the outlet phosgene are measured.
[0079] Comparative Example 1
[0080] Premixed CO and chlorine are introduced into a phosgene synthesis tower, and phosgene is synthesized by reaction of CO and chlorine under the action of a catalyst; the phosgene synthesis tower is a tube-and-tube fixed bed reactor, the tube length is 3m, the tube is filled with an activated carbon catalyst, which is a commercially available activated carbon catalyst with a grade of NORIT RB4C, and the catalyst has an m2 / m1 value of 0.65 using the above-mentioned activated carbon evaluation method, and multi-point thermometers are installed in some tubes, the number of multi-point thermometers installed is 1 per 100 tubes, the density of temperature measuring points on the thermometer is 6 per m, and high-temperature resistant mineral oil is used outside the tube to absorb the reaction heat generated by synthesizing phosgene; a cooler is provided in the phosgene synthesis system to cool the heat-conducting medium after absorbing the reaction heat, and the heat-conducting medium is brine.
[0081] When the hot spot temperature position in the activated carbon bed in the phosgene synthesis tower is greater than 2m from the tube inlet, and the residual chlorine content in the synthetic phosgene is higher than 300ppm, it indicates that the activated carbon in the phosgene synthesis tower is converted into deactivated activated carbon. The operating cycle from the activated carbon being put into use to reaching the deactivated state is calculated, and the volume loss of the activated carbon in the tube is measured.
[0082] Comparative Example 2
[0083] The premixed CO and chlorine are introduced into a phosgene synthesis tower, and the CO and chlorine react to synthesize phosgene under the action of a catalyst; the phosgene synthesis tower is a tube-and-tube fixed bed reactor, the tube length is 5m, the tube is filled with an activated carbon catalyst, which is a commercially available activated carbon catalyst with a grade of NORIT RB4C, and the catalyst has an m2 / m1 value of 0.65 using the above-mentioned activated carbon evaluation method, and multi-point thermometers are installed in some tubes, the number of multi-point thermometers installed is 1 / 150 tubes, the density of temperature measuring points on the thermometer is 4 / m, and high-temperature resistant silicone oil is used outside the tube to absorb the reaction heat generated by synthesizing phosgene; a cooler is provided in the phosgene synthesis system to cool the heat-conducting medium after absorbing the reaction heat, and the heat-conducting medium is water.
[0084] When the hot spot temperature position in the activated carbon bed in the phosgene synthesis tower is greater than 3.2m from the tube inlet, and the residual chlorine content in the phosgene is higher than 1500ppm, it indicates that the activated carbon in the phosgene synthesis tower is converted into deactivated activated carbon. The operating cycle from the activated carbon being put into use to reaching the deactivated state is calculated, and the volume loss of the activated carbon in the tube is measured.
[0085] Comparative Example 3
[0086] Premixed CO and chlorine are introduced into a phosgene synthesis tower, and phosgene is synthesized by reaction of CO and chlorine under the action of a catalyst; the phosgene synthesis tower is a tube-and-tube fixed bed reactor, the tube length is 2m, the tube is filled with an activated carbon catalyst, which is a commercially available activated carbon catalyst with a grade of NORIT RB4C, and the m2 / m1 value is 0.65 using the above-mentioned activated carbon evaluation method, and multi-point thermometers are installed in some tubes, the number of multi-point thermometers installed is 1 per 200 tubes, the density of temperature measuring points on the thermometer is 8 per m, and high-temperature resistant silicone oil is used outside the tube to absorb the reaction heat generated by synthesizing phosgene; a cooler is provided in the phosgene synthesis system to cool the heat-conducting medium after absorbing the reaction heat, and the heat-conducting medium is chlorobenzene.
[0087] When the hot spot temperature position in the activated carbon bed in the phosgene synthesis tower is greater than 1.5m from the tube inlet, and the residual chlorine content in the phosgene is higher than 750ppm, it indicates that the activated carbon in the phosgene synthesis tower is converted into deactivated activated carbon. The operating cycle from the activated carbon being put into use to reaching the deactivated state is calculated, and the volume loss of the activated carbon in the tube is measured.
[0088] Table 1 Effect of industrial application of synthetic activated carbon
[0089]
[0090] It can be seen from the above table that the prepared high-activity activated carbon has a long service life. Compared with the commercially available phosgene synthesis activated carbon, the operating cycle is increased by more than 50%, which is of great significance for extending the operating cycle of the phosgene synthesis tower and avoiding frequent shutdowns for maintenance.
[0091] Table 2 Analysis indicators before and after activated carbon regeneration
[0092]
[0093]
[0094] Table 3 Phosgene synthesis operating parameters before and after activated carbon regeneration
[0095]
[0096] As can be seen from the above table, the activated carbon regeneration process has a good effect on removing chlorine-containing impurities in activated carbon, and the catalytic activity of activated carbon is restored. When the regenerated activated carbon is used to produce phosgene, the hot spot temperature in the activated carbon bed moves forward significantly, indicating that the catalytic activity of the activated carbon is restored, and the free chlorine content in the phosgene product is greatly reduced. The use of the activated carbon online regeneration process can reduce the shutdown and maintenance time of the phosgene synthesis tower due to activated carbon deactivation from 15-30 days to 2-3 days, and avoid the safety risk of untreated phosgene leakage due to the opening of the phosgene synthesis tower, which has good implementation effect and significance.
Claims
1. A method for preparing highly active renewable activated carbon for phosgene synthesis, characterized in that: The following steps are involved: 1) reacting a nitrogen-containing aromatic compound under inert gas protection with anhydrous ZnCl2 as a catalyst at high temperature for a certain period of time to obtain a black powder; washing the powder to remove unreacted raw materials, blending it with ordinary carbon powder in a certain proportion, further acid washing at a certain temperature to remove metal ions, and then washing and drying the powder to obtain raw carbon powder; 2) The raw carbon powder and the binder are mixed evenly, kneaded, extruded into strips, and then aged, dried, and calcined to obtain activated carbon suitable for phosgene synthesis.
2. The method according to claim 1, characterized in that: In step 1), the nitrogen-containing aromatic ring compound used is one or more of 1,4-dicyanobenzene, 2,6-naphthalene dicarbonitrile, 1,3,5-3-cyanobenzene, the molar ratio of the nitrogen-containing aromatic ring compound to the catalyst anhydrous ZnCl2 is selected from 3:1-7:1, the inert gas is nitrogen, and / or the reaction temperature is 300-500°C, and the reaction time is 20-60h.
3. The method according to claim 1 or 2, characterized in that: In step 1), the cleaning method for removing unreacted raw materials from the powder is to use 2% dilute hydrochloric acid 10-30 times the mass of the powder for cleaning, and then use deionized water 25-75 times the mass of the powder for cleaning.
4. The method according to claim 1 or 2, characterized in that: In step 1), the carbon powder used for blending is commercially available coconut shell activated carbon or coal-based activated carbon powder, and the blending ratio is the mass ratio of carbon powder prepared from nitrogen-containing aromatic ring compounds in step 1): commercially available activated carbon powder is 1:1-1:
4.
5. The method according to claim 1 or 2, characterized in that: In step 1), the method for removing metal ions in the powder by pickling is to heat the powder under reflux in a 10% nitric acid solution at 90-100°C for 1-4h, wash the pickled powder with deionized water 25-75 times the mass of the powder, and then dry it to constant weight at 100-150°C in a nitrogen atmosphere.
6. The method according to claim 1 or 2, characterized in that: The activity of the activated carbon is characterized by m2 / m1, and the m2 / m1 value is 0.7-1; the evaluation method is: determine the saturated chlorine adsorption value of the activated carbon as m1, desorb the chlorine-saturated activated carbon with nitrogen at 325-375°C, repeatedly determine the saturated chlorine adsorption value of the activated carbon as m2, and calculate the m2 / m1 value.
7. The method according to claim 6, characterized in that: The m2 / m1 value is 0.8-1.
8. A method for phosgene synthesis and online regeneration of activated carbon catalyst, the method comprising the following steps: 1) introducing premixed CO and chlorine into a phosgene synthesis tower, and reacting CO and chlorine to synthesize phosgene under the action of a catalyst prepared by the method of any one of claims 1 to 5; 2) When the highest temperature point in the activated carbon bed in the phosgene synthesis tower moves back to a certain position, it indicates that the phosgene synthesis activity of the activated carbon decreases, the residual chlorine content in the synthetic phosgene increases, and the activated carbon in the phosgene synthesis tower is converted into deactivated activated carbon; at this time, the activated carbon is regenerated online, the phosgene synthesis tower system is pretreated, and then the deactivated activated carbon is regenerated online using high-temperature carbon monoxide and high-temperature nitrogen.
9. The method according to claim 8, characterized in that In step 1), an electric heater is provided at the inlet of the phosgene synthesis tower to heat carbon monoxide or nitrogen to 300-600°C; and / or, the phosgene synthesis tower is two-stage, the first stage is a shell-and-tube fixed bed reactor, and the second stage is a random pile fixed bed reactor; and / or, a vacuum system is provided on the shell side of the shell and tube of the first-stage phosgene synthesis tower to extract the gas in the shell side space to form a negative pressure or vacuum environment; and / or, a multi-point thermometer is installed in the first-stage phosgene synthesis tower to monitor the temperature of the activated carbon bed in the shell and tube.
10. The method according to claim 8 or 9, characterized in that: In step 2), when the activated carbon in the phosgene synthesis tower is converted into deactivated activated carbon, the highest temperature point in the activated carbon bed in the phosgene synthesis tower moves back to a distance of 1.5-3.2 m from the inlet of the tubular reactor containing activated carbon, and the chlorine content in the phosgene at the outlet of the corresponding reactor is 300-1500 ppm.
11. The method according to claim 8, characterized in that In step 2), the operation of pre-treating the phosgene synthesis tower system is: recovering the heat transfer medium on the shell side of the phosgene synthesis tower into the heat transfer medium storage tank, and making the shell side in a low pressure or vacuum state through a vacuum system to avoid heat dissipation on the shell side, and the shell side pressure is selected from 20-80kpa (A).
12. The method according to claim 11, characterized in that In step 2), the shell side pressure is selected from 40-60 kpa (A).
13. The method according to claim 8, characterized in that In step 2), high-temperature carbon monoxide is used to desorb the weakly adsorbed chlorine in the activated carbon bed. The heating temperature of carbon monoxide is selected from 200-400°C; the axial flow rate of carbon monoxide in the activated carbon bed is 10-20m / s; and the carbon monoxide desorption treatment time is 2-12h.
14. The method according to claim 13, characterized in that In step 2), the heating temperature of carbon monoxide is selected from 250-350°C.
15. The method according to claim 13, characterized in that In step 2), the heating temperature of carbon monoxide is selected from 275-325°C.
16. The method according to claim 13, characterized in that In step 2), the axial flow velocity of carbon monoxide in the activated carbon bed is 12-18 m / s.
17. The method according to claim 13, characterized in that In step 2), the carbon monoxide desorption treatment time is 4-10 hours.
18. The method according to claim 8, characterized in that In step 2), high-temperature nitrogen is used to remove chlorine-containing impurities strongly bound to the activated carbon in the activated carbon bed. The heating temperature of the nitrogen is selected from 400-600°C; the axial flow rate of the nitrogen in the activated carbon bed is 5-15m / s; and the nitrogen desorption treatment time is 24-48h.
19. The method according to claim 18, characterized in that In step 2), the heating temperature of the nitrogen is selected from 450-550°C.
20. The method according to claim 18, characterized in that In step 2), the heating temperature of the nitrogen is selected from 475-525°C.
21. The method according to claim 18, characterized in that In step 2), the axial flow rate of nitrogen in the activated carbon bed is 8-12 m / s.
22. The method according to claim 18, characterized in that In step 2), the nitrogen desorption treatment time is 32-40h.
23. The method according to claim 8, characterized in that In step 2), after the online regeneration, the iodine adsorption value of the activated carbon increases to 70-90% of the level of fresh activated carbon, and the total carbon content is 85-95%.
24. The method according to claim 8, characterized in that In step 2), after the activated carbon has been regenerated online, fresh chlorine and carbon monoxide are added again to carry out phosgene synthesis reaction, the ratio of the distance from the hot spot temperature position in the activated carbon bed to the tube inlet to the total length of the tube is between 0.1-0.4, and the free chlorine content in the outlet synthetic phosgene is less than 500ppm.
Citation Information
Patent Citations
Method for continuously preparing phosgene
CN102092713A
Method for replacing phosgene synthetic tower catalyst
CN105817183A
Modular flue gas cleaning device with in-situ regeneration function, and regeneration method
CN103127823A
Catalyst for preparing phosgene and method for preparing phosgene
CN104415770A