A bismuth ferrite-barium titanate high-temperature lead-free piezoelectric ceramic material and a preparation method thereof
By introducing GeO2 and BiAlO3 into BF-BT ceramics and optimizing the sintering process and microstructure, the problem of insufficient electrical properties of BF-BT ceramics at high temperatures and high electric fields is solved, and ceramics with high Curie temperature and high voltage electrical properties are realized. Materials suitable for high temperature piezoelectric devices.
Patent Information
- Application Number
- CN202310311615.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing BiFeO3-BaTiO3 (BF-BT) ceramic material exhibits high conductivity and low electrical insulation under high temperature and high electric field, making it difficult to achieve good polarization performance, limiting its application in high-temperature piezoelectric devices.
By introducing GeO2 as a sintering aid in BF-BT ceramics, combined with partial replacement of BiAlO3, and using multi-step synthesis and rapid sintering processes, the sintering characteristics and microstructure are optimized, the density is increased, and the Curie temperature and piezoelectric properties are improved. .
The high Curie temperature (638°C) and high voltage electrical performance (d33=125pC/N) of BF-BT ceramics are achieved, the contradiction between piezoelectricity and Curie temperature is optimized, and the overall performance of the ceramics is improved.
Smart Images

Figure CN116444260B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of piezoelectric ceramics, and in particular relates to an optimized bismuth ferrite-barium titanate high-temperature lead-free piezoelectric ceramic material and a preparation method thereof. Background Art
[0002] With the rapid development of aerospace, geothermal drilling, petrochemical and other fields, high-temperature lead-free piezoelectric materials and devices are urgently needed. Bi-based perovskite materials are high-temperature lead-free piezoelectric ceramics with great application potential. 3+ Ionic 6s 2 Lone pair electrons give this type of material good ferroelectric and piezoelectric properties. BiFeO3 (BF) is a multiferroic ceramic material that has been studied extensively. It has a high Curie temperature (~830°C), large rhombohedral distortion and theoretical polarization strength at room temperature, and a large piezoelectric coefficient d 33 (44pC / N) and electric field induced strain (0.36%). It is very difficult to synthesize high insulating BF ceramics with a single perovskite structure. The introduction of ABO3-type ferroelectrics can inhibit the generation of impurities, stabilize the perovskite structure, increase the resistivity, and form BF-based solid solutions with good ferroelectric and piezoelectric properties, such as BF-PbTiO3, BF-BaTiO3 (BT), BF-K 0.5 Na 0.5 NbO3, etc. Compared with other lead-free BF-ABO3 solid solutions, BF-BT ceramics have better piezoelectric properties. By adjusting the ratio between BF and BT, a higher Curie temperature can be obtained. However, the key problems of high conductivity, low electrical insulation, and difficulty in achieving polarization under high temperature and high electric field cannot be overcome, thus limiting its application in high-temperature piezoelectric devices.
[0003] BiAlO3 is a lead-free piezoelectric ferroelectric material with a perovskite structure and a high spontaneous polarization intensity (~76μC / cm 2 ), whose Curie temperature (>520℃) is much higher than that of barium titanate (~120℃), so replacing part of BT with BiAlO3 can increase the Curie temperature of BF-BT ceramics. However, due to the unstable structure of BiAlO3, it is difficult to synthesize under normal conditions. It needs to be synthesized by high temperature and high pressure technology or form a solid solution with other perovskite structures. Zhenyong Cen et al. studied BF-BT ceramics with Al replacing Fe: 0.72Bi(Fe 1-x Al x )O3-0.28BaTiO3, which is equivalent to replacing part of BF with BiAlO3, but significantly reduces the Curie temperature. When x = 0.01, it shows good piezoelectric properties and temperature stability: d 33 =151pC / N,k p =0.31, T d =420℃, but at this time Tc The value (450°C) is relatively low (Zhenyong Cen et al., J. Am. Ceram. Soc., 2013, 96(7): 2252-2256.).
[0004] Chinese patent CN110128126A introduces Bi(Ti 0.5 Zn 0.5 )O3 and BiAlO3 regulate the phase structure and microstructure of ceramics. 0.5 Cu 0.5 )O3, CuO, Li2CO3 as sintering aids, a multi-step synthesis method combined with pure oxygen calcination to synthesize pre-sintered powders, and rapid sintering to obtain bismuth ferrite-barium titanate-based piezoelectric ceramics with high piezoelectric properties: 0.725BiFeO3-0.175BaTiO3-0.075Bi(Ti 0.5 Zn 0.5 )O3-0.025BiAlO3+0.01Li2CO3+0.01MnCO3+0.025Bi2O3, the best performance of ceramics sintered at 960℃: d 33 =137pC / N,k p =0.293%, T C =596℃, T d =580℃, tanδ=3.31%. Its preparation method includes, in addition to the traditional solid phase sintering process, multi-step synthesis of intermediates, pure oxygen calcination, rapid sintering and other processes.
[0005] Chinese patent application CN110563456A adopts the method of partially replacing Fe with Sc and partially replacing Ti with Zr to reduce Fe. 3+ By increasing the degree of distortion of BaTiO3 during reduction and adding MnO2 after pre-sintering, a material with a Curie temperature of 600°C and a piezoelectric constant of 105pC / N was obtained using traditional ceramic sintering technology: 0.75BiFe 0.985 Sc 0.015 O3-0.25BaZr 0.2 Ti 0.8 O3+1mol%MnO2.
[0006] The electrical properties of BF-BT ceramics are closely related to the synthesis process and material composition. Although the above process has improved the electrical properties of BF-BT ceramics, the Curie temperature and piezoelectric properties need to be further improved, especially ceramic materials with a Curie temperature above 600°C and good piezoelectric properties are needed to meet the application of high-temperature piezoelectric devices. The improvement of piezoelectric properties often leads to a decrease in the Curie temperature, which greatly limits the practical application of BF-BT piezoelectric ceramic materials. Summary of the Invention
[0007] In view of the existing problems, the present invention provides an optimized BF-BT high-temperature lead-free piezoelectric ceramic material and a preparation method thereof. The obtained ceramic material has a high Curie temperature (T C = 638 °C) and high piezoelectric properties (d 33 = 125 pC / N), and its piezoelectric properties are superior to those of other constituent materials with the same Curie temperature in this system.
[0008] The present invention utilizes the sintering aid and doping substitution modification of GeO2 to improve the sintering characteristics, increase the density, optimize the microstructure. The addition of GeO2 significantly increases the Curie temperature. Partially replacing BaTiO3 with BiAlO3 further increases the Curie temperature and reduces the loss, thereby realizing the optimization of structure and performance, improving the contradiction between piezoelectricity and Curie temperature, and significantly increasing both piezoelectricity and Curie temperature.
[0009] The object of the present invention can be achieved by the following technical solutions:
[0010] A bismuth ferrite-barium titanate high-temperature lead-free piezoelectric ceramic material, the composition of the piezoelectric ceramic material is 0.74Bi 1.02 FeO3-(0.26 - x)BaTiO3 - xBiAlO3 + y%GeO2; where x and y respectively represent the molar fractions of BiAlO3 and GeO2, 0 ≤ x ≤ 0.02, 0 < y < 0.7. Preferably, x = 0.01 ± 0.005, 0.3 ≤ y ≤ 0.5.
[0011] The preparation method of the bismuth ferrite-barium titanate high-temperature lead-free piezoelectric ceramic material includes the following steps:
[0012] (1) Select Bi2O3, Fe2O3, BaCO3, TiO2 and Al2O3 as raw materials, and weigh the raw materials according to the chemical formula 0.74Bi 1.02 FeO3-(0.26 - x)BaTiO3 - xBiAlO3 for ball milling, drying, and pre-sintering to obtain intermediate powder, where x represents the molar fraction of BiAlO3, and 0 ≤ x ≤ 0.02;
[0013] (2) Weigh the intermediate powder and GeO2 powder according to the chemical formula 0.74Bi 1.02 FeO3-(0.26 - x)BaTiO3 - xBiAlO3 + y%GeO2 of the piezoelectric ceramic material, conduct ball milling, granulation, molding, sintering, electrode deposition and polarization to obtain the piezoelectric ceramic, where y represents the molar fraction of GeO2, and 0 < y < 0.7.
[0014] Preferably, the pre-firing temperature in step (1) is 700-900° C., and the holding time is 2-8 hours; the sintering temperature in step (2) is 920-1020° C., and the holding time is 1-5 hours.
[0015] Preferably, the pre-firing temperature in step (1) is 750-850° C., and the holding time is 3-6 hours; the sintering temperature in step (2) is 960-1000° C., and the holding time is 2-4 hours.
[0016] Preferably, in step (1), the ball milling medium is anhydrous ethanol, and the ball milling time is 6 to 10 hours; in step (2), the ball milling medium is anhydrous ethanol, and the ball milling time is 8 to 12 hours.
[0017] Preferably, in step (1), the ball mill uses zirconium dioxide balls with a diameter of 1±0.5 mm as grinding balls, and the weight ratio of raw materials, grinding balls and ball milling media is 1:(2-4):(1.0-1.5).
[0018] Preferably, the granulation in step (2) uses a polyvinyl alcohol aqueous solution with a mass concentration of 5 to 10% as a binder.
[0019] Preferably, the molding in step (2) is performed by pressing the ceramic disc under a pressure of 50 to 150 MPa.
[0020] Preferably, the polarization in step (2) is performed by immersing the obtained ceramic sheet in silicone oil at 80 to 120° C., the polarization voltage used is 3 to 5 kV / mm, and the polarization time is 10 to 20 min.
[0021] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0022] (1) The present invention utilizes the sintering aid and substitution modification of GeO2, combined with the high Curie temperature and low loss of BiAlO3, to achieve the optimization of structure and performance, and the prepared bismuth ferrite-barium titanate high temperature lead-free piezoelectric ceramics have both high Curie temperature and high piezoelectricity. By selecting appropriate x, y values and process parameters, the piezoelectric ceramics of this system can be made to have a high Curie temperature T c =638℃,d 33 The highest value reaches 125pC / N, which is higher than other materials with the same Curie temperature in this system.
[0023] (2) The high-temperature lead-free piezoelectric ceramics prepared by the present invention adopt a mature traditional ceramic sintering process. The synthesis process is simple and does not require additional production conditions such as high temperature and high pressure, atmosphere, annealing, quenching, multiple multi-step synthesis, etc. It is low in cost and has good repeatability and stability, and has strong practical value. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The dielectric temperature curves of the piezoelectric ceramic material prepared in Example 1 of the present invention at 10 kHz, 100 kHz and 1 MHz.
[0025] Figure 2 The dielectric temperature curves of the piezoelectric ceramic material prepared in Example 2 of the present invention at 10 kHz, 100 kHz and 1 MHz.
[0026] Figure 3 This is a scanning electron microscope (SEM) photograph of the piezoelectric ceramic material prepared in Example 1 of the present invention.
[0027] Figure 4 This is a scanning electron microscope (SEM) photograph of the piezoelectric ceramic material prepared in Example 2 of the present invention. DETAILED DESCRIPTION
[0028] The present invention is further described below in conjunction with specific embodiments, but the protection scope claimed by the present invention is not limited thereto. It should be understood that the embodiments described herein are only used to explain the present invention and are not used to limit the scope of the present invention.
[0029] Example 1
[0030] Preparation of 0.74Bi 1.02 FeO3-0.25BaTiO3-0.01BiAlO3+0.3%GeO2 high temperature lead-free piezoelectric ceramic material.
[0031] According to the chemical formula 0.74Bi 1.02FeO3-0.25BaTiO3-0.01BiAlO3 ingredients, weigh Bi2O3, Fe2O3, BaCO3, TiO2 and Al2O3 with purity higher than 99% as raw materials. Use anhydrous ethanol as ball milling medium and 1mm diameter zirconium dioxide balls as grinding balls. According to the weight ratio of raw materials, grinding balls and medium of 1:3:1.2, ball mill for 8 hours, dry and sieve at 85℃, then pre-sinter at 800℃ at a rate of 3℃ / min and keep warm for 4 hours. Sieve and weigh the pre-sintered intermediate, and then weigh 0.3% GeO2 powder by molar ratio and add it. With anhydrous ethanol as the ball milling medium and 1mm diameter zirconium dioxide balls as the grinding balls, the raw materials, grinding balls, and medium weight ratio was 1:3:1.2. After secondary ball milling for 8 hours, the raw materials, grinding balls, and medium were dried and sieved, and then granulated with a polyvinyl alcohol solution with a mass concentration of 8%, and formed into a ceramic disc with a diameter of 10mm and a thickness of 1.0mm at 150MPa. The ceramic disc was placed in a sintering furnace and heated from room temperature to 600℃ for 5 hours and kept for 2 hours for debinding, and then heated to 980℃ at a rate of 3℃ / min for sintering, kept for 2 hours, and naturally cooled to room temperature. After the sintered ceramic disc surface was polished and cleaned, it was silvered by screen printing and silvered at 750℃ for 10 minutes. Finally, the ceramic disc was immersed in 100℃ silicone oil and polarized at a DC voltage of 5kV / mm for 10 minutes. After the polarization, the sample was placed at room temperature for 24 hours before the electrical properties were tested.
[0032] Example 2
[0033] Preparation of 0.74Bi 1.02 FeO3-0.25BaTiO3-0.01BiAlO3+0.5%GeO2 high temperature lead-free piezoelectric ceramic material.
[0034] According to the chemical formula 0.74Bi 1.02FeO3-0.25BaTiO3-0.01BiAlO3 ingredients, weigh Bi2O3, Fe2O3, BaCO3, TiO2 and Al2O3 with a purity higher than 99% as raw materials. Use anhydrous ethanol as ball milling medium and 1mm diameter zirconium dioxide balls as grinding balls. According to the weight ratio of raw materials, grinding balls and medium of 1:3:1.2, ball milling for 10 hours, dry and sieve at 85℃, then pre-sinter at 750℃ at a rate of 3℃ / min, and keep warm for 6 hours. Sieve the pre-sintered intermediate and weigh it, and then weigh 0.5% GeO2 powder by molar ratio and add it. With anhydrous ethanol as the ball milling medium and 1mm diameter zirconium dioxide balls as the grinding balls, the raw material, grinding ball, and medium weight ratio was 1:3:1.2, and then the secondary ball milling was carried out for 10 hours, dried, sieved, and then granulated with a polyvinyl alcohol solution with a mass concentration of 10%, and formed into a ceramic disc with a diameter of 10mm and a thickness of 1.0mm at 100MPa. The ceramic disc was placed in a sintering furnace and heated from room temperature to 600℃ for 5 hours and kept for 2 hours for debinding, and then heated to 980℃ at a rate of 3℃ / min for sintering, kept for 3 hours, and naturally cooled to room temperature. After the sintered ceramic disc surface was polished and cleaned, it was silvered by screen printing process and silvered at 750℃ for 10 minutes. Finally, the ceramic disc was immersed in 80℃ silicone oil and polarized for 20 minutes under a DC electric field of 5kV / mm. After polarization, the sample was placed at room temperature for 24 hours before the electrical performance test.
[0035] Example 3
[0036] Preparation of 0.74Bi 1.02 FeO3-0.24BaTiO3-0.02BiAlO3+0.3%GeO2 high temperature lead-free piezoelectric ceramic material.
[0037] According to the chemical formula 0.74Bi 1.02FeO3-0.24BaTiO3-0.02BiAlO3 ingredients, weigh Bi2O3, Fe2O3, BaCO3, TiO2 and Al2O3 with a purity higher than 99% as raw materials. Use anhydrous ethanol as ball milling medium and 1mm diameter zirconium dioxide balls as grinding balls. According to the weight ratio of raw materials, grinding balls and medium of 1:4:1.5, ball mill for 12 hours, dry and sieve at 85℃, then pre-sinter at 800℃ at a rate of 3℃ / min and keep warm for 4 hours. Sieve the pre-sintered intermediate and weigh it, and then weigh 0.3% GeO2 powder by molar ratio and add it. With anhydrous ethanol as the ball milling medium and 1mm diameter zirconium dioxide balls as the grinding balls, the raw materials, grinding balls and medium weight ratio was 1:4:1.5, and then the secondary ball milling was carried out for 10 hours, dried and sieved, and then a polyvinyl alcohol solution with a mass concentration of 10% was added for granulation, and the ceramic disc with a diameter of 10mm and a thickness of 1.0mm was formed at 100MPa. The ceramic disc was placed in a sintering furnace and heated from room temperature to 600℃ for 5 hours and kept for 2 hours for debinding, and then heated to 960℃ at a rate of 3℃ / min for sintering, kept for 4 hours, and naturally cooled to room temperature. After the sintered ceramic disc surface was polished and cleaned, it was silvered by screen printing process and silvered at 750℃ for 10 minutes. Finally, the ceramic disc was immersed in 100℃ silicone oil and polarized for 20 minutes under a DC electric field of 3kV / mm. After polarization, the sample was placed at room temperature for 24 hours before the electrical performance test.
[0038] Example 4
[0039] Preparation of 0.74Bi 1.02 FeO3-0.26BaTiO3+0.3%GeO2 high temperature lead-free piezoelectric ceramic material.
[0040] According to the chemical formula 0.74Bi 1.02FeO3-0.26BaTiO3 ingredients, weigh Bi2O3, Fe2O3, BaCO3, TiO2 with a purity higher than 99% as raw materials. Use anhydrous ethanol as ball milling medium, 1mm diameter zirconium dioxide balls as grinding balls, according to the weight ratio of raw materials, grinding balls, and medium of 1:4:1.2, ball milling for 6 hours, drying and sieving at 85℃, and then pre-burning at 850℃ at a rate of 3℃ / min, and keeping warm for 3 hours. Sieve and weigh the pre-burned intermediate, and then weigh 0.3% GeO2 powder by molar ratio. Use anhydrous ethanol as ball milling medium, 1mm diameter zirconium dioxide balls as grinding balls, according to the weight ratio of raw materials, grinding balls, and medium of 1:4:1.2, carry out secondary ball milling for 10 hours, dry and sieve, then add 5% polyvinyl alcohol solution to granulate, and form into ceramic discs with a diameter of 10mm and a thickness of 1.0mm at 50MPa. The ceramic disc was placed in a sintering furnace and heated from room temperature to 600℃ for 5 hours and kept for 2 hours for debinding. Then, the temperature was raised to 1000℃ at a rate of 3℃ / min for sintering, kept for 2 hours, and naturally cooled to room temperature. After the sintered ceramic surface was polished and cleaned, it was silvered by screen printing and silvered at 750℃ for 10 minutes. Finally, the ceramic piece was immersed in 120℃ silicone oil and polarized for 10 minutes under a DC electric field of 4kV / mm. After polarization, the sample was placed at room temperature for 24 hours before the electrical performance test.
[0041] Example 5
[0042] Preparation of 0.74Bi 1.02 FeO3-0.255BaTiO3-0.005BiAlO3+0.4%GeO2 high temperature lead-free piezoelectric ceramic material.
[0043] According to the chemical formula 0.74Bi 1.02FeO3-0.255BaTiO3-0.005BiAlO3 ingredients, weigh Bi2O3, Fe2O3, BaCO3, TiO2 and Al2O3 with purity higher than 99% as raw materials. Use anhydrous ethanol as ball milling medium and 1mm diameter zirconium dioxide balls as grinding balls. According to the weight ratio of raw materials, grinding balls and medium of 1:3:1.2, ball mill for 8 hours, dry and sieve at 85℃, then pre-sinter at 800℃ at a rate of 3℃ / min and keep warm for 4 hours. Sieve the pre-sintered intermediate and weigh it, and then weigh 0.4% GeO2 powder by molar ratio and add it. With anhydrous ethanol as the ball milling medium and 1mm diameter zirconium dioxide balls as the grinding balls, the raw materials, grinding balls, and medium weight ratio was 1:3:1.2. After secondary ball milling for 12 hours, the raw materials, grinding balls, and medium were dried and sieved, and then granulated with a polyvinyl alcohol solution with a mass concentration of 8%, and formed into a ceramic disc with a diameter of 10mm and a thickness of 1.0mm at 150MPa. The ceramic disc was placed in a sintering furnace and heated from room temperature to 600℃ for 5 hours and kept for 2 hours for debinding, and then heated to 1000℃ at a rate of 3℃ / min for sintering, kept for 2 hours, and naturally cooled to room temperature. After the sintered ceramic disc surface was polished and cleaned, it was silvered by screen printing and silvered at 750℃ for 10 minutes. Finally, the ceramic disc was immersed in 100℃ silicone oil and polarized at a DC voltage of 5kV / mm for 10 minutes. After the polarization, the sample was placed at room temperature for 24 hours and then the electrical properties were tested.
[0044] Example 6
[0045] Preparation of 0.74Bi 1.02 FeO3-0.24BaTiO3-0.02BiAlO3+0.5%GeO2 high temperature lead-free piezoelectric ceramic material.
[0046] According to the chemical formula 0.74Bi 1.02FeO3-0.24BaTiO3-0.02BiAlO3 ingredients, weigh Bi2O3, Fe2O3, BaCO3, TiO2 and Al2O3 with purity higher than 99% as raw materials. Use anhydrous ethanol as ball milling medium and 1mm diameter zirconium dioxide balls as grinding balls. Mill for 8 hours at a weight ratio of raw materials, grinding balls and medium of 1:3:1.2, dry and sieve at 85℃, then pre-sinter at 800℃ at a rate of 3℃ / min and keep warm for 4 hours. Sieve and weigh the pre-sintered intermediate, and then weigh 0.5% GeO2 powder by molar ratio. With anhydrous ethanol as the ball milling medium and 1mm diameter zirconium dioxide balls as the grinding balls, the raw materials, grinding balls and medium weight ratio was 1:3:1.2, and then the secondary ball milling was carried out for 10 hours, dried and sieved, and then a polyvinyl alcohol solution with a mass concentration of 10% was added for granulation, and formed into a ceramic disc with a diameter of 10mm and a thickness of 1.0mm at 100MPa. The ceramic disc was placed in a sintering furnace and heated from room temperature to 600℃ for 5 hours and kept for 2 hours for debinding, and then heated to 960℃ at a rate of 3℃ / min for sintering, kept for 4 hours, and naturally cooled to room temperature. After the sintered ceramic disc surface was polished and cleaned, it was silvered by screen printing process and silvered at 750℃ for 10 minutes. Finally, the ceramic disc was immersed in 100℃ silicone oil and polarized for 20 minutes under a DC electric field of 3kV / mm. After polarization, the sample was placed at room temperature for 24 hours before the electrical performance test.
[0047] Example 7
[0048] Preparation of 0.74Bi 1.02 FeO3-0.26BaTiO3+0.5%GeO2 high temperature lead-free piezoelectric ceramic material.
[0049] According to the chemical formula 0.74Bi 1.02FeO3-0.26BaTiO3 ingredients, weigh Bi2O3, Fe2O3, BaCO3, TiO2 with a purity higher than 99% as raw materials. Use anhydrous ethanol as ball milling medium, 1mm diameter zirconium dioxide balls as grinding balls, according to the weight ratio of raw materials, grinding balls, and medium of 1:3:1.2, ball milling for 6 hours, drying and sieving at 85℃, and then pre-burning at 850℃ at a rate of 3℃ / min, and keeping warm for 3 hours. Sieve and weigh the pre-burned intermediate, and then weigh 0.5% GeO2 powder by molar ratio. Use anhydrous ethanol as ball milling medium, 1mm diameter zirconium dioxide balls as grinding balls, according to the weight ratio of raw materials, grinding balls, and medium of 1:3:1.2, carry out secondary ball milling for 8 hours, dry, sieve, and then add 5% polyvinyl alcohol solution to granulate, and form into ceramic discs with a diameter of 10mm and a thickness of 1.0mm at 50MPa. The ceramic disc was placed in a sintering furnace and heated from room temperature to 600℃ for 5 hours and kept for 2 hours for debinding. Then, the temperature was raised to 980℃ at a rate of 3℃ / min for sintering, kept for 2 hours, and naturally cooled to room temperature. After the sintered ceramic surface was polished and cleaned, it was silvered by screen printing and silvered at 750℃ for 10 minutes. Finally, the ceramic piece was immersed in 120℃ silicone oil and polarized for 10 minutes under a DC electric field of 4kV / mm. After polarization, the sample was placed at room temperature for 24 hours before the electrical performance test.
[0050] Comparative Example 1
[0051] Preparation of 0.74Bi 1.02 FeO3-0.25BaTiO3-0.01BiAlO3 high temperature lead-free piezoelectric ceramic material.
[0052] According to the chemical formula 0.74Bi 1.02FeO3-0.25BaTiO3-0.01BiAlO3 ingredients, weigh Bi2O3, Fe2O3, BaCO3, TiO2 and Al2O3 with a purity higher than 99% as raw materials. Use anhydrous ethanol as ball milling medium, 1mm diameter zirconium dioxide balls as grinding balls, according to the weight ratio of raw materials, grinding balls, and medium of 1:3:1.2, ball milling for 6 hours, drying and sieving at 85℃, and then pre-burning at 800℃ at a rate of 3℃ / min, and keeping warm for 4 hours. The pre-burned intermediate is sieved and weighed. Use anhydrous ethanol as ball milling medium, 1mm diameter zirconium dioxide balls as grinding balls, according to the weight ratio of raw materials, grinding balls, and medium of 1:3:1.2, after secondary ball milling for 8 hours, drying and sieving, then adding 5% mass concentration of polyvinyl alcohol solution to granulate, and forming into ceramic discs with a diameter of 10mm and a thickness of 1.0mm at 100MPa. The ceramic disc was placed in a sintering furnace and heated from room temperature to 600℃ for 5 hours and kept for 2 hours for debinding. Then, the temperature was raised to 980℃ at a rate of 3℃ / min for sintering, kept for 2 hours, and naturally cooled to room temperature. After the sintered ceramic surface was polished and cleaned, it was silvered by screen printing and silvered at 750℃ for 10 minutes. Finally, the ceramic piece was immersed in 100℃ silicone oil and polarized at a DC voltage of 3kV / mm for 15 minutes. After polarization, the sample was placed at room temperature for 24 hours before the electrical performance test.
[0053] Comparative Example 2
[0054] Preparation of 0.74Bi 1.02 FeO3-0.24BaTiO3-0.02BiAlO3+0.7%GeO2 high temperature lead-free piezoelectric ceramic material.
[0055] According to the chemical formula 0.74Bi 1.02FeO3-0.24BaTiO3-0.02BiAlO3 ingredients, weigh Bi2O3, Fe2O3, BaCO3, TiO2 and Al2O3 with purity higher than 99% as raw materials. Use anhydrous ethanol as ball milling medium and 1mm diameter zirconium dioxide balls as grinding balls. Mill for 8 hours at a weight ratio of raw materials, grinding balls and medium of 1:3:1.2, dry and sieve at 85℃, then pre-sinter at 750℃ at a rate of 3℃ / min and keep warm for 6 hours. Sieve and weigh the pre-sintered intermediate, and then weigh 0.7% GeO2 powder by molar ratio. With anhydrous ethanol as the ball milling medium and 1mm diameter zirconium dioxide balls as the grinding balls, the raw materials, grinding balls and medium weight ratio was 1:3:1.2, and then the secondary ball milling was carried out for 10 hours, dried and sieved, and then granulated with a polyvinyl alcohol solution with a mass concentration of 8%, and formed into a ceramic disc with a diameter of 10mm and a thickness of 1.0mm at 100MPa. The ceramic disc was placed in a sintering furnace and heated from room temperature to 600℃ for 5 hours and kept for 2 hours for debinding, and then heated to 960℃ at a rate of 3℃ / min for sintering, kept for 4 hours, and naturally cooled to room temperature. After the sintered ceramic disc surface was polished and cleaned, it was silvered by screen printing process and silvered at 750℃ for 10 minutes. Finally, the ceramic disc was immersed in 100℃ silicone oil and polarized at a DC voltage of 3kV / mm for 15 minutes. After the polarization, the sample was placed at room temperature for 24 hours and then the electrical properties were tested.
[0056] Table 1 lists the sintering temperatures and piezoelectric and room temperature dielectric properties of the piezoelectric ceramics prepared in Examples 1-7 and Comparative Examples 1-2. It can be seen that Examples 1-7 all have relatively high Curie temperatures T c and the piezoelectric constant d 33 Although Comparative Example 1 has a d similar to that of each embodiment, 33 value (~121pC / N), but T c Although Comparative Example 2 has a Curie temperature similar to that of each embodiment (~615°C), d 33 The value is low (~62pC / N) and the loss is large (~5.0%).
[0057] Table 1
[0058]
[0059]
[0060] Figure 1 and Figure 2The following are the dielectric-temperature curves of the piezoelectric ceramics prepared in Example 1 and Example 2 of the present invention at 10kHz, 100kHz, and 1MHz. The BF-BT ceramics with GeO2 added have two dielectric anomaly peaks in their dielectric-temperature curves, and the temperature corresponding to the high-temperature dielectric anomaly peak, namely the Curie temperature, is significantly increased. The addition of BiAlO3 can further increase the Curie temperature, and move the low-temperature dielectric anomaly peak to high temperature, shortening the temperature interval between the high and low-temperature dielectric peaks, while reducing the piezoelectric coefficient and room-temperature dielectric constant. Example 1 sintered at 980°C exhibits the best comprehensive performance of high Curie temperature and high piezoelectricity: d 33 =125pC / N, k p =31%, T c =638℃,ε r =530, tanδ=3.3%.
[0061] Figure 3 This is a SEM picture of the piezoelectric ceramic material prepared in Example 1 of the present invention after sintering at 980° C., polishing and thermal corrosion. It can be seen from the picture that the ceramic material has a dense and uniform microstructure, and the average grain size is ≈5.3 μm. Figure 4 is a SEM image of the piezoelectric ceramic material prepared in Example 2 of the present invention after sintering at 980°C, polishing and thermal etching, for comparison Figure 3 It can be seen that the increase in GeO2 content causes a slight decrease in grain size, with the average grain size being ≈4.5μm, but the grain size is more uniform and the ceramic body is denser, so better piezoelectric properties can also be obtained.
[0062] The dielectric temperature curves and SEM images of the piezoelectric ceramic materials prepared in Examples 3-7 are similar to those in Examples 1 and 2 and will not be described in detail.
[0063] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing bismuth ferrite-barium titanate high temperature lead-free piezoelectric ceramic material, characterized in that: The following steps are involved: (1) Select Bi2O3, Fe2O3, BaCO3, TiO2 and Al2O3 as raw materials, according to the chemical formula 0.74Bi 1.02 FeO3-(0.26-x)BaTiO3-xBiAlO3 weighs raw materials, performs ball milling, drying, and pre-calcination at a temperature of 700-900°C and a heat preservation time of 2-8 hours to obtain an intermediate powder; (2) According to the chemical formula of the piezoelectric ceramic material 0.74Bi 1.02 FeO3-(0.26-x)BaTiO3-xBiAlO3+y%GeO2 weighs the intermediate powder and GeO2 powder, performs ball milling, granulation, molding, sintering, the sintering temperature is 960-1020℃, the heat preservation time is 1-5h, the electrode is applied and polarization is performed to obtain the piezoelectric ceramic material; The composition of the piezoelectric ceramic material is 0.74Bi 1.02 FeO3-(0.26-x)BaTiO3-xBiAlO3+y%GeO2; wherein x and y represent the molar fractions of BiAlO3 and GeO2 respectively, 0.005≤x≤0.02, 0.3≤y<0.
7.
2. The preparation method according to claim 1, characterized in that: x=0.01±0.005, 0.3≤y≤0.
5.
3. The preparation method according to claim 2, characterized in that: The pre-firing temperature in step (1) is 750-850°C, and the holding time is 3-6 hours; the sintering temperature in step (2) is 980-1000°C, and the holding time is 2-4 hours.
4. The preparation method according to claim 3, characterized in that: In step (1), the ball milling medium is anhydrous ethanol, and the ball milling time is 6 to 10 hours; in step (2), the ball milling medium is anhydrous ethanol, and the ball milling time is 8 to 12 hours.
5. The preparation method according to claim 4, characterized in that: In step (1), the ball mill uses zirconium dioxide balls with a diameter of 1±0.5 mm as grinding balls, and the weight ratio of raw materials, grinding balls, and ball milling media is 1: (2-4): (1.0-1.5).
6. The preparation method according to any one of claims 1 to 5, characterized in that The granulation described in step (2) uses a polyvinyl alcohol aqueous solution with a mass concentration of 5-10% as a binder.
7. The preparation method according to claim 6, characterized in that: The molding described in step (2) is to press the ceramic disc under a pressure of 50-150 MPa.
8. The preparation method according to claim 7, characterized in that: The polarization described in step (2) is to immerse the obtained ceramic sheet in silicone oil at 80 to 120° C. for polarization, the polarization voltage used is 3 to 5 kV / mm, and the polarization time is 10 to 20 minutes.
9. Bismuth ferrite-barium titanate high temperature lead-free piezoelectric ceramic material obtained by the method according to any one of claims 1 to 8.
Citation Information
Patent Citations
Bismuth ferrate-barium titanate-bismuth zinc titanate-bismuth aluminate high-temperature lead-free piezoelectric ceramic and preparation method thereof
CN110128126A
Lead-free bismuth ferrite-based piezoelectric ceramic with high Curie temperature and high piezoelectric property, and preparation method thereof
CN110563456A
Preparation method of lead-free piezoelectric ceramic energy storage capacitor based on BiAlO3-doped BaTiO3
CN110156459A