A viscosity reducing material and its preparation method and application

By combining matrix asphalt, mineral oil and composite polymers in viscosity-reducing materials, and through microwave irradiation and high-speed shearing processes, the existing technology's problems of high-temperature rutting resistance and low-temperature brittleness of viscosity-reducing materials in severe cold areas are solved. It achieves excellent low-temperature performance and deformation recovery ability, improving the sealing effect and service life of road gaps.

CN116444994BActive Publication Date: 2024-10-01CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210011985.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-06
Publication Date
2024-10-01
Estimated Expiration
2042-01-06

AI Technical Summary

Technical Problem

When used in severe cold areas, existing viscosity-reducing materials have poor high-temperature rutting resistance and low-temperature brittleness properties, and the construction environment and process are complicated, resulting in unsatisfactory road gap sealing effects.

Method used

Using a combination of matrix asphalt, mineral oil and composite polymers, and through processes such as microwave irradiation and high-speed shearing, a viscosity-reducing material with excellent low-temperature performance and deformation recovery ability is prepared. Compounds are added to improve adhesion and tensile strength. Rate.

Benefits of technology

It achieves good bonding force and deformation recovery ability under low temperature conditions, avoids bonding loss, improves the waterproof performance and service life of road gaps, and reduces the frequency of maintenance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003457927710000051
    Figure BDA0003457927710000051
  • Figure BDA0003457927710000052
    Figure BDA0003457927710000052
  • Figure BDA0003457927710000061
    Figure BDA0003457927710000061
Patent Text Reader

Abstract

The present invention discloses a viscosity-reducing material and a preparation method and application thereof. The viscosity-reducing material comprises the following components, calculated by mass fraction: 63% to 88% of base asphalt; 5% to 20% of mineral oil; 2% to 12% of composite polymer; and 0.5% to 5% of chemical agent. The viscosity-reducing material provided by the present invention meets the structural and construction characteristics of existing road gaps and reserved gaps of structural structures, has excellent low-temperature performance and deformation recovery ability, has strong bonding force and high low-temperature elongation and low-temperature ductility, and can effectively fill and repair road gaps and reserved gaps of structural structures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a viscosity reducing material and a preparation method thereof, in particular to a viscosity reducing material used as a filling and repairing material for road gaps and reserved gaps in structural structures and a preparation method thereof. Background Art

[0002] There is frost heave on roads in severe cold regions. The reason is related to external water entering the roadbed, poor sealing effect at expansion joints and failure to repair road cracks in time. These road gaps and reserved gaps in structures are usually filled and repaired with various sealing materials, which rely on the elasticity of the sealing materials to "follow" the changes in the gap width caused by temperature and load, and achieve the purpose by improving the strength, elongation, fatigue resistance and other properties of the materials. Unfortunately, the actual use of these materials has not been satisfactory so far. There are many reasons. The first is the material factor. These products themselves have good performance, but the requirements for construction environment conditions are too high. For example, the concrete must be dry and clean, and there must be no floating slurry; or primer or surface treatment must be added, otherwise the interface will crack due to poor bonding; the ambient temperature cannot be too high or too low, otherwise it will affect the curing of the resin, and then affect the performance of the resin matrix and the bonding performance, etc.; the second is the construction factor. The on-site construction is too casual, the surface treatment is not good or simply not treated, and water is used in the operation, which leads to poor curing of the sealant, poor bonding, and difficulty in achieving material performance; there are many other factors that make the actual sealing effect of the gap poor.

[0003] CN108299790A discloses a modified asphalt viscosity reducer and a preparation method thereof, wherein polyacrylate, amino resin and eicosanoic acid are added to a reaction kettle and mixed, polyacrylate stearic acid and carloamine are added and mixed, surfactant and synthetic paraffin are added and mixed, and finally zeolite powder and a compatibilizer are added and mixed to obtain a product. Since synthetic paraffin is added in this method, when used in severe cold areas, the high temperature rutting resistance and low temperature brittle cracking performance of the asphalt product will deteriorate.

[0004] CN110093043B discloses an asphalt viscosity reducer and its preparation method and application. In this method, preheated anti-aging agent, dispersant, anti-stripping agent, solvent, initiator, and foaming agent are sequentially added to a shear emulsifier, and sheared and stirred evenly to obtain the asphalt viscosity reducer. The dispersant of this method uses solid paraffin, which will deteriorate the high-temperature anti-rutting ability and low-temperature brittle cracking performance of asphalt products when used in severe cold areas.

[0005] CN111349300A discloses a modified asphalt viscosity reducer and a preparation method thereof, wherein maleic anhydride and diisopropylbenzene peroxide are mixed, ground into powder, added into macromolecular polyethylene and mixed evenly, melt-grafted under the initiation of diisopropylbenzene peroxide, and then pulverized into powder after cooling to obtain maleic anhydride grafted polyethylene wax, and then long-chain fatty acids are placed in a reactor and heated to melt and then ethyleneamine is added, and after heating and dehydration, maleic anhydride grafted polyethylene wax, compatibilizer, and zeolite powder are added and stirred to obtain the product. The preparation process of this method is complicated, and the maleic anhydride grafted polyethylene wax generated by the reaction will make the asphalt easy to crack at low temperatures. Summary of the invention

[0006] In view of the deficiencies of the prior art, the present invention provides a viscosity-reducing material and a preparation method and application thereof. The viscosity-reducing material conforms to the structural and construction characteristics of existing road gaps and reserved gaps of structural structures, has excellent low-temperature performance and deformation recovery ability, has strong adhesion and high low-temperature elongation and low-temperature ductility, and can effectively fill and repair road gaps and reserved gaps of structural structures.

[0007] The present invention provides a viscosity reducing material, which comprises the following components, measured by mass fraction:

[0008] Base asphalt 63% to 88%, preferably 72% to 86%;

[0009] Mineral oil 5% to 20%, preferably 6% to 18%;

[0010] Composite polymer 2% to 12%, preferably 3% to 10%;

[0011] The compound is 0.5% to 5%, preferably 0.8% to 2.5%.

[0012] Furthermore, the composite polymer includes natural polymers and synthetic polymers.

[0013] Furthermore, in the composite polymer, the mass fractions of the natural polymer and the synthetic polymer are 5% to 40% and 60% to 95% respectively.

[0014] Furthermore, the natural polymer in the composite polymer is preferably natural rubber, and the synthetic polymer is preferably one or more of synthetic rubbers.

[0015] Furthermore, the matrix asphalt is a petroleum asphalt prepared from natural petroleum by at least one process such as distillation, blending, oxidation, solvent deasphalting, etc. The saturated content of the matrix asphalt is not more than 25%, preferably 15% to 23% (by mass). The asphaltene content of the matrix asphalt is not more than 13%, preferably 5% to 10% (by mass).

[0016] Furthermore, the mineral oil is a mineral oil produced from natural petroleum, which is a mixture of cycloalkanes and chain alkanes. The saturated content of the mineral oil is not more than 35%, preferably 15% to 30% (by mass). The viscosity of the mineral oil at 100°C is 50 to 60000 mm 2 / s, pour point less than 30°C, and mass content of condensed aromatic hydrocarbons less than 5%.

[0017] Furthermore, the compound comprises a vulcanizing agent, a vulcanization accelerator and an antioxidant, wherein the mass ratio of the vulcanizing agent, the vulcanization accelerator and the antioxidant is 1:(0.3-1.0):(0.1-1.5).

[0018] Furthermore, among the chemical agents, the vulcanizing agent is preferably one or more of elemental sulfur, sulfide, sulfur monochloride, selenium, tellurium, and isocyanate; the vulcanization accelerator is preferably one or more of aldehyde amines, guanidines, thiurams, thiazoles, dithiocarbamates, xanthates, thioureas, sulfonamides, and metal oxides; and the antioxidant is preferably one or more of monophenols, bisphenols, polyphenols, heterocyclic antioxidants, and phosphite antioxidants.

[0019] The second aspect of the present invention provides a method for preparing the above-mentioned viscosity reducing material, comprising the following steps:

[0020] (1) preparing a composite polymer;

[0021] (2) adding mineral oil to the melted matrix asphalt and stirring evenly, then adding the composite polymer to swell, and forming a binder through high-speed shearing;

[0022] (3) subjecting the binder described in step (2) to microwave irradiation to obtain a viscosity-reducing binder;

[0023] (4) adding an antioxidant to the viscosity-reducing binder described in step (3), then performing a first stirring, then high-speed shearing, then adding a vulcanizing agent, performing a second stirring, adding a vulcanization accelerator, and then performing a third stirring to obtain the viscosity-reducing material semi-finished product;

[0024] (5) Subjecting the semi-finished viscosity reducing material described in step (4) to microwave irradiation to obtain a viscosity reducing material.

[0025] Furthermore, the method for preparing the composite polymer described in step (1) comprises the following steps:

[0026] After the natural polymer and the synthetic polymer are uniformly mixed, they are added into a rubber extruder for meshing. After the meshed polymer forms a uniform and continuous strip, it is repeatedly meshed through the rubber extruder. Finally, the meshed polymer is irradiated with microwaves to obtain the composite polymer.

[0027] Furthermore, in the method for preparing the composite polymer described in step (1), preferably, the mass fractions of the natural polymer and the synthetic polymer are 5% to 40% and 60% to 95%, respectively.

[0028] Furthermore, in the preparation method of the composite polymer described in step (1), the extruder is a conventional device in the art, the meshing temperature is 120°C to 160°C, the residence time of the material in the extruder is 1min to 5min each time it meshes, the vacuum degree in the extruder chamber is -0.2MPa to -0.05MPa, and the number of meshing times is 3 to 10 times.

[0029] Furthermore, in the preparation method of the composite polymer described in step (1), the microwave irradiation time is 2 min to 10 min, the power is 0.5 kW to 5 kW, and the frequency is 2000 MHz to 2500 MHz.

[0030] Furthermore, in step (2), the melting temperature is 130°C to 150°C, and the time is 20min to 60min; the swelling temperature is 150°C to 170°C, and the time is 30min to 80min.

[0031] Furthermore, in step (2), the rotation speed of the high-speed shearing is 1000 r / min to 10000 r / min.

[0032] Furthermore, in step (3), the microwave irradiation time is 2 min to 5 min, the power is 0.5 kW to 2 kW, and the frequency is 2000 MHz to 2500 MHz.

[0033] Furthermore, in step (4), the mass ratio of the vulcanizing agent, the vulcanization accelerator and the antioxidant is 1:(0.3-1.0):(0.1-1.5).

[0034] Furthermore, in step (4), the temperature of the first stirring is 140° C. to 160° C., the time is 30 min to 90 min, and the stirring speed is 50 r / min to 150 r / min.

[0035] Furthermore, in step (4), the rotation speed of the high-speed shearing is 1000 r / min to 5000 r / min, and the time is 30 min to 60 min.

[0036] Furthermore, in step (4), the temperature of the second stirring is 160° C. to 180° C., the time is 1 to 5 hours, and the stirring speed is 300 r / min to 800 r / min.

[0037] Furthermore, in step (4), the temperature of the third stirring is 160° C. to 170° C., the time is 0.5 to 2 h, and the stirring speed is 100 r / min to 300 r / min.

[0038] Furthermore, in step (5), the microwave irradiation conditions are: time is 1 min to 4 min, power is 0.2 kW to 1 kW, and frequency is 2400 MHz to 2500 MHz.

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] (1) The present invention adjusts the content of matrix asphalt, mineral oil, and polymer and adds chemical agents to make the viscosity-reducing material have excellent low-temperature performance and deformation recovery ability, strong adhesion and high low-temperature elongation and ductility, and strong deformation following ability, thereby avoiding the binder from falling off from the bonding point on the surface of the gap due to a large temperature difference, making the gap have better waterproof performance, increasing the service life of the road, and reducing the frequency of maintenance.

[0041] (2) The polymer of the present invention can remove impurities in the polymer, increase the plasticity and flexibility of the polymer, improve the tensile strength of the polymer, improve the anti-aging ability of the polymer, and adjust the polymer performance through the process according to the actual performance requirements.

[0042] (3) The natural polymer of the present invention and the synthetic polymer are repeatedly meshed to remove impurities in the polymer, causing unstable functional groups in the polymer molecules to undergo chemical reactions such as degradation and cross-linking, thereby making the performance of the product of the present invention more stable.

[0043] (4) The present invention controls the viscosity of the composite polymer and the binder through the microwave irradiation method, thereby improving the low-temperature flexibility and low-temperature crack resistance of the product.

[0044] (5) The mineral oil in the present invention can enhance the flexibility of the polymer and improve the low-temperature crack resistance of the product.

[0045] (6) The present invention performs the first stirring at 140°C to 160°C, which can gradually release active chemical bonds, facilitate the control of the reaction rate, and smoothly complete polymerization, cross-linking, grafting and other reactions; the second stirring at 160°C to 180°C can make the active groups and chemical bonds in the material system react completely, avoiding subsequent continuous effects on material properties; the third stirring at 160°C to 170°C can make the material system more uniform and stable, avoiding adverse conditions such as stratification and gelation. DETAILED DESCRIPTION

[0046] The technical scheme and effects of the present invention are further illustrated by examples. The examples are implemented based on the technical scheme of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following examples.

[0047] Example 1

[0048] The natural polymer and the synthetic polymer are mixed evenly and added into a rubber extruder for meshing. After the meshed polymer forms a uniform and continuous strip, it is repeatedly meshed 5 times through the rubber extruder. The meshing temperature is 150°C, the residence time is 3 minutes, and the vacuum degree is -0.1MPa. Finally, the meshed polymer is irradiated with microwaves for 5 minutes, with a power of 2kW and a frequency of 2450MHz to obtain the composite polymer. The raw material names, proportions and models are shown in Table 1 below.

[0049] Table 1 Raw material names, ratios and models of composite polymers

[0050] Material Category Material Name Specifications Mass fraction, % Synthetic polymers Butadiene Styrene Copolymer SBR1500 90 Natural polymers Natural rubber Solid State 10

[0051] Add matrix asphalt and mineral oil to the reactor, heat to 140℃, dissolve them completely, and the time is 30min. Then add the composite polymer and stir evenly to swell, the swelling temperature is 160℃, and the time is 60min. After the whole mixture is subjected to high shear at a speed of 3000 rpm for 30min, microwave irradiation is carried out for 3min, the power is 1kW, and the frequency is 2400MHz. Then add the chemical agent (anti-aging agent) and stir for the first time for 60min, the stirring temperature is 150℃, and the stirring speed is 100r / min. After the first stirring is completed, the whole mixture is subjected to high shear at a speed of 3000 rpm for 30min, and then the chemical agent (vulcanizing agent) is added for the second stirring for 2h, the stirring temperature is 170℃, and the stirring speed is 500r / min. After the second stirring, a chemical agent (vulcanization accelerator) was added and stirred for a third time for 1 hour, the stirring temperature was 165°C, the stirring speed was 200 r / min, and then microwave irradiation was performed for 2 minutes, the power was 0.5 kW, and the frequency was 2450 MHz to obtain a viscosity-reducing material. The viscosity-reducing material prepared in this embodiment has the following raw material names, proportions and models as shown in Table 2, and the properties of the obtained product are shown in Table 6.

[0052] Table 2 Raw material names, proportions and models of viscosity reducing materials

[0053]

[0054] Example 2

[0055] The composite polymer is the same as in Example 1.

[0056] Add matrix asphalt and mineral oil to the reactor, heat to 140℃, dissolve them completely, and the time is 30min. Then add the composite polymer and stir evenly to swell, the swelling temperature is 160℃, and the time is 60min. After the whole mixture is subjected to high shear at a speed of 3000 rpm for 30min, microwave irradiation is carried out for 3min, the power is 1kW, and the frequency is 2400MHz. Then add the chemical agent (anti-aging agent) and stir for the first time for 60min, the stirring temperature is 150℃, and the stirring speed is 100r / min. After the first stirring, the whole mixture is subjected to high shear at a speed of 3000 rpm for 30min, and then the chemical agent (vulcanizing agent) is added for the second stirring for 2h, the stirring temperature is 170℃, and the stirring speed is 500r / min. After the second stirring, add the chemical agent (vulcanization accelerator) and stir for the third time for 1h, the stirring temperature is 165℃, and the stirring speed is 200r / min. After microwave irradiation for 2 minutes, power of 0.5 kW and frequency of 2450 MHz, a viscosity-reducing material was obtained. The raw material names, proportions and models of the viscosity-reducing material prepared in this embodiment are shown in Table 3 below, and the properties of the obtained product are shown in Table 6.

[0057] Table 3 Raw material name, ratio and model of viscosity reducing materials

[0058]

[0059]

[0060] Example 3

[0061] After the natural polymer and the synthetic polymer are uniformly mixed, they are added to a rubber extruder for meshing. After the meshed polymer forms a uniform and continuous strip, it is repeatedly meshed 7 times through the rubber extruder, the meshing temperature is 130°C, the residence time is 3 minutes, the vacuum degree is -0.15MPa, and the meshing number is 7 times. The final meshed polymer is then irradiated with microwaves for 5 minutes, a power of 2kW, and a frequency of 2450MHz to obtain the composite polymer, the raw material name, ratio and model are shown in Table 4 below.

[0062] Table 4 Raw material names, ratios and models of composite polymers

[0063]

[0064] Add matrix asphalt and mineral oil to the reactor, heat to 140℃, dissolve them completely, and the time is 30min. Then add the composite polymer and stir evenly to swell, the swelling temperature is 160℃, and the time is 60min. After the whole mixture is subjected to high shear at a speed of 3000 rpm for 30min, microwave irradiation is performed for 3min, the power is 1kW, and the frequency is 2400MHz. Then add the chemical agent (anti-aging agent) and stir for the first time for 60min, the stirring temperature is 150℃, and the stirring speed is 100r / min. After the first stirring is completed, the whole mixture is subjected to high shear at a speed of 3000 rpm for 30min, and then the chemical agent (vulcanizing agent) is added for the second stirring for 2h, the stirring temperature is 170℃, and the stirring speed is 500r / min. After the second stirring, a chemical agent (vulcanization accelerator) was added and stirred for a third time for 1 hour, the stirring temperature was 165° C., the stirring speed was 200 r / min, and then microwave irradiation was performed for 2 minutes, the power was 0.5 kW, and the frequency was 2450 MHz to obtain a viscosity-reducing material. The viscosity-reducing material prepared in this embodiment has the raw material name, ratio and model as shown in Table 5 below, and the performance of the obtained product is shown in Table 6.

[0065] Table 5 Raw material names, proportions and models of viscosity reducing materials

[0066]

[0067] Comparative Example 1

[0068] The raw materials and methods of this comparative example 1 are basically the same as those of Example 1, except that microwave irradiation was not performed when preparing the binder. The properties of the obtained product are shown in Table 6.

[0069] Comparative Example 2

[0070] The raw materials and methods of this comparative example 2 are basically the same as those of example 1, except that microwave irradiation was not performed when preparing the composite polymer. The properties of the obtained product are shown in Table 6.

[0071] Comparative Example 3

[0072] The raw materials and method of this comparative example 3 are basically the same as those of example 1, except that no antioxidant is added during the first stirring. The properties of the obtained product are shown in Table 6.

[0073] Test Example 1

[0074] The materials prepared in Examples 1-3 and Comparative Examples 1-3 were tested according to the technical requirements of JT / T 589-2004 "Cement Concrete Pavement Caulking Sealing Materials". The test results are shown in Table 6.

[0075] Table 6 Performance of viscosity reducing materials

[0076] Product Name Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Technical requirements Needle penetration, 0.1mm 96 81 87 93 90 88 <90 Elasticity (recovery) rate, % 99 99 99 87 84 83 ≥60 Flowability, mm 2 2 2 2 2 2 ≤2 Tensile strength (-10℃), mm 20 23 28 16 15 15 ≥15 Tensile strength (-20℃), mm 6 7 10 3 3 3 — 5℃ elongation, cm 65 70 73 48 43 40 — Viscosity at 135℃, kPa 4.9 3.6 3.2 6.1 5.7 6.4 —

[0077] From the comparison results in Table 6, although the performance of Comparative Examples 1-3 can meet the technical requirements, the tensile properties at lower temperatures and medium-temperature tensile properties are much worse than those of Examples 1-3, and the viscosity is obviously high, which is not conducive to construction.

[0078] The viscosity-reducing materials of Examples 1-3 of the present invention not only meet the technical requirements of the standards, but also show obvious advantages in more stringent indicators, can be used to fill various reserved gaps in road surfaces, and have strong practicality.

[0079] Test Example 2

[0080] A universal material testing machine was used to perform tensile tests on Examples 1-3 and Comparative Examples 1-3. The test results are shown in Table 7.

[0081] Table 7 Tensile properties of viscosity-reducing materials

[0082] Product Name Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Tensile strength, MPa 108 103 88 135 129 138 Peeling area ratio, % Approx. 4 Approx. 2 Approx. 1 Approx. 10 Approx. 8 Approx. 10

[0083] From the comparison results in Table 7, since the tensile strength of Examples 1-3 is relatively small, it shows that the cohesive force is relatively small, the material has better followability and adhesion, and better peeling resistance, and is not prone to peeling and breaking.

Claims

1. A viscosity reducing material, comprising the following components, measured by mass fraction: Base asphalt 63% to 88%; Mineral oil 5% to 20%; Composite polymer 2% to 12%; Chemical agent 0.5%~5%; The composite polymer includes a natural polymer and a synthetic polymer; in the composite polymer, the mass fractions of the natural polymer and the synthetic polymer are 5% to 40% and 60% to 95% respectively; the natural polymer is natural rubber, and the synthetic polymer is synthetic rubber; The mineral oil is a mineral oil produced from natural petroleum, which is a mixture of cycloalkanes and chain alkanes; the saturated content of the mineral oil is not more than 35% by mass; the viscosity of the mineral oil at 100°C is 50-60000mm 2 / s, pour point less than 30°C, mass content of condensed aromatic hydrocarbons less than 5%; The chemical composition comprises a vulcanizing agent, a vulcanization accelerator and an antioxidant; wherein: The mass ratio of vulcanizing agent, vulcanization accelerator and antioxidant is 1: (0.3-1.0): (0.1-1.5); In the compound, the vulcanizing agent is one or more of elemental sulfur, sulfide, sulfur monochloride, selenium, tellurium, and isocyanate; the vulcanization accelerator is one or more of aldehyde amines, guanidines, thiurams, thiazoles, dithiocarbamates, xanthates, thioureas, sulfenamides, and metal oxides; the antioxidant is one or more of monophenols, polyphenols, heterocyclic antioxidants, and phosphite antioxidants; The method for preparing the viscosity reducing material comprises the following steps: (1) Preparation of composite polymers; (2) Add mineral oil to the melted matrix asphalt and stir evenly, then add the composite polymer to swell, and form a binder through high-speed shearing; (3) subjecting the binder described in step (2) to microwave irradiation to obtain a viscosity-reducing binder; (4) adding an antioxidant to the viscosity-reducing binder described in step (3), and then performing a first stirring, and then high-speed shearing, and then adding a vulcanizing agent, and performing a second stirring, and then adding a vulcanization accelerator, and then performing a third stirring, to obtain the viscosity-reducing material semi-finished product; (5) subjecting the semi-finished viscosity reducing material described in step (4) to microwave irradiation to obtain a viscosity reducing material; The method for preparing the composite polymer described in step (1) comprises the following steps: The natural polymer and the synthetic polymer are mixed evenly, and then added into a rubber extruder for meshing. After the meshed polymer forms a uniform and continuous strip, the meshed polymer is repeatedly meshed through the rubber extruder. Finally, the meshed polymer is irradiated with microwaves to obtain the composite polymer. In the preparation method of the composite polymer described in step (1), the microwave irradiation time is 2 min to 10 min, the power is 0.5 kW to 5 kW, and the frequency is 2000 MHz to 2500 MHz; In step (5), the microwave irradiation conditions are: time is 1 min to 4 min, power is 0.2 kW to 1 kW, and frequency is 2400 MHz to 2500 MHz.

2. The viscosity reducing material according to claim 1, characterized in that: The matrix asphalt is petroleum asphalt prepared from natural petroleum through at least one of distillation, blending, oxidation and solvent deasphalting processes; the saturated content of the matrix asphalt is not more than 25% by mass; the asphaltene content of the matrix asphalt is not more than 13% by mass.

3. The method for preparing the viscosity reducing material according to claim 1 or 2, comprising the steps of: (1) Preparation of composite polymers; (2) Add mineral oil to the melted matrix asphalt and stir evenly, then add the composite polymer to swell, and form a binder through high-speed shearing; (3) subjecting the binder described in step (2) to microwave irradiation to obtain a viscosity-reducing binder; (4) adding an antioxidant to the viscosity-reducing binder described in step (3), and then performing a first stirring, and then high-speed shearing, and then adding a vulcanizing agent, and performing a second stirring, and then adding a vulcanization accelerator, and then performing a third stirring, to obtain the viscosity-reducing material semi-finished product; (5) subjecting the semi-finished viscosity reducing material described in step (4) to microwave irradiation to obtain a viscosity reducing material; The method for preparing the composite polymer described in step (1) comprises the following steps: The natural polymer and the synthetic polymer are mixed evenly, and then added into a rubber extruder for meshing. After the meshed polymer forms a uniform and continuous strip, the meshed polymer is repeatedly meshed through the rubber extruder. Finally, the meshed polymer is irradiated with microwaves to obtain the composite polymer. In the preparation method of the composite polymer described in step (1), the microwave irradiation time is 2 min to 10 min, the power is 0.5 kW to 5 kW, and the frequency is 2000 MHz to 2500 MHz; In step (5), the microwave irradiation conditions are: time is 1 min to 4 min, power is 0.2 kW to 1 kW, and frequency is 2400 MHz to 2500 MHz.

4. The preparation method according to claim 3, characterized in that: In step (2), the melting temperature is 130°C to 150°C, and the time is 20 min to 60 min; the swelling temperature is 150°C to 170°C, and the time is 30 min to 80 min; and the high-speed shearing speed is 1000 r / min to 10000 r / min.

5. The preparation method according to claim 3, characterized in that: In step (4), the temperature of the first stirring is 140°C to 160°C, the time is 30min to 90min, and the stirring speed is 50r / min to 150r / min; the speed of the high-speed shearing is 1000r / min to 5000r / min, and the time is 30min to 60min; the temperature of the second stirring is 160°C to 180°C, the time is 1 to 5h, and the stirring speed is 300r / min to 800r / min; the temperature of the third stirring is 160°C to 170°C, the time is 0.5 to 2h, and the stirring speed is 100r / min to 300r / min.