A method for preparing high-performance oxygen evolution catalyst by using lattice strain and its application
The NiTe/Ni2P heterojunction catalyst with lattice strain was prepared by hydrothermal method and vapor deposition method, which solved the problem of slow and unstable kinetics of nickel-based catalysts in OER, and achieved high performance and stable oxygen reduction catalysis. The formation of NiOOH is avoided, providing high-performance catalysts for OER, ORR and HOR.
Patent Information
- Application Number
- CN202310270865.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-15
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-03-15
AI Technical Summary
Existing nickel-based catalysts have slow and unstable kinetics in the oxygen reduction reaction (OER). The high price and low content of precious metal catalysts limit their commercial applications. Most nickel-based catalysts are converted into NiOOH after the OER reaction, which cannot meet the requirements. Practical application requirements.
NiTe and Ni(OH)2 are prepared by hydrothermal method, and phosphating is performed using vapor deposition method to form a heterojunction catalyst NiTe/Ni2P with lattice strain. The ratio is controlled to achieve the preparation of high-performance catalyst and avoid the generation of NiOOH. .
A high-performance and stable oxygen reduction catalyst was achieved, the catalyst life was extended, and the formation of NiOOH was not observed, and a preparation scheme for high-performance and high-stability catalysts for OER, ORR and HOR was provided.
Smart Images

Figure HDA0004134653290000011 
Figure HDA0004134653290000012 
Figure HDA0004134653290000013
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of water electrolysis, and in particular to a NiTe / Ni 2 Preparation method and application of P oxygen evolution catalyst. Background Art
[0002] Water decomposition to produce hydrogen and oxygen is considered one of the most promising ways to alleviate the energy crisis and environmental degradation problems, which includes two half reactions of hydrogen evolution reaction (HER) and oxygen evolution reaction (OER). Due to the sluggish kinetics caused by the multi-step four-electron OER process, it still requires a larger overpotential to drive OER compared with HER, even with noble metal Ru-based or Ir-based catalysts. However, the disadvantages of noble metal catalysts, such as high price, low content, and poor stability, severely limit their commercial application. Therefore, discovering high-performance non-noble metal (NPM) catalysts for OER is an extremely important issue.
[0003] To date, many transition metal nitrides, phosphides, carbides, sulfides, etc. have been studied in order to find good NPM catalysts for OER catalysis. 3 N. Ni 3 P.Mo 2 C.Co 3 S 4 Many attempts have been made. Among them, nickel-based catalysts are considered to be the most promising candidate materials due to their appropriate binding energy and excellent catalytic performance. However, their electrocatalytic performance still cannot meet the needs of practical applications. In addition, most nickel-based catalysts will be converted into NiOOH after the OER reaction. Therefore, such catalysts are not truly active substances, but can only be called precursor catalysts.
[0004] In the present invention, a series of NiTe / Ni 2 P heterojunction catalyst, thereby regulating the Ni 2 The ratio of P and NiTe realizes the heterojunction catalyst NiTe / Ni with controllable strain effect. 2 The successful preparation of P. Summary of the invention
[0005] The purpose of the present invention is to provide a method and application of preparing a high-performance oxygen evolution catalyst by using lattice strain. The preparation method is simple and has excellent oxygen evolution performance. More importantly, compared with other Ni-based catalysts that are widely studied at present, NiOOH is not observed after stability testing, which has guiding significance for preparing catalysts by using strain engineering design.
[0006] In order to achieve the above-mentioned invention object, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing a high-performance oxygen evolution catalyst by using lattice strain, characterized in that it comprises the following steps:
[0008] Step (1), preparing NiTe using nickel foam (NF) as a nickel source by a hydrothermal method;
[0009] Step (2), using NiTe as a carrier, reintroducing a nickel source hydrothermally to obtain NiTe / Ni(OH) 2 ;
[0010] Step (3), NiTe / Ni(OH) prepared in step (2) 2 The precursor was used for phosphating by vapor deposition to obtain the heterojunction catalyst NiTe / Ni with lattice strain. 2 P. The lattice strain is that NiTe has compressive strain, or NiTe and Ni 2 P has compressive and tensile strains on the lattice, respectively.
[0011] Preferably, step (1): Na 2 TeO 3 Dissolve in deionized water, then slowly and continuously add N 2 H 4 ·H 2 O (hydrazine hydrate), per 2mmol Na 2 TeO 3 Dissolve in 20 ml deionized water, 12 ml N 2 H 4 ·H 2 O (hydrazine hydrate), add treated NF after mixing evenly, react at 100-250 ° C for 10h-25h, and dry in nitrogen atmosphere to obtain NiTe;
[0012] Preferably, in step (2), the NiTe obtained in step (1) is used as a carrier, and C is added to a hydrothermal autoclave. 4 H 6 O 4 Ni·4H 2 O、NH 4 F, CH 4 N 2 In a mixture of O and deionized water, each 0.9 mmol C 4 H 6 O 4 Ni·4H 2 O corresponds to 2.1mmolNH 4 F, 3.7mmol CH 4 N 2O, 30 ml of deionized water, then react at 50-180 ° C for 3 h-12 h, and dry in nitrogen atmosphere to obtain NiTe / Ni(OH) 2 ;
[0013] Preferably, in step (3), the NiTe / Ni(OH) obtained in step (2) 2 Place the precursor downstream of the tube furnace and place NaH 2 PO 2 , sintered at 300-500℃ for 2-5h to obtain NiTe / Ni 2 P, phosphorus source is potassium hypophosphite, potassium phosphite, sodium hypophosphite, sodium phosphite, ammonium hypophosphite, ammonium phosphite, phosphorus source and NiTe / Ni(OH) 2 The mass ratio is 1:40 to 25:1; the matching principle of temperature, time and sodium phosphite makes NiTe / Ni(OH) 2 Ni(OH) 2 Phosphate to Ni 2 P makes the NiTe phase show compressive strain; further in Ni(OH) 2 Phosphate to Ni 2 P, NiTe also has a small amount of phosphating, which makes the NiTe phase show compressive strain. 2 The P phase has tensile strain.
[0014] Sintered at 350℃ for 2h, sodium hypophosphite and NiTe / Ni(OH) 2 The mass ratio is 1:10-15:1, preferably sodium hypophosphite and NiTe / Ni(OH) 2 The mass ratio is 1:5~10:1.
[0015] The present invention provides a high-performance oxygen evolution catalyst NiTe / Ni with lattice strain prepared by the preparation method described in the above technical scheme 2 P.
[0016] The present invention provides a method for preparing a high-performance oxygen evolution catalyst NiTe / Ni by using lattice strain as described in the above technical solution. 2 The application of P in water electrolysis reduces NiOOH generation and increases stability and catalyst life.
[0017] The present invention utilizes the incompatibility between phosphide and telluride to prepare a series of heterostructure catalysts NiTe / Ni with different lattice strains. 2P, not only has excellent oxygen evolution performance, but more importantly, no NiOOH is observed after stability testing, compared with other Ni-based catalysts that have been widely studied so far. This work opens a new door for the preparation of high-performance and high-stability catalysts for OER, ORR, and even HOR using strain engineering. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Attached Figure 1 The synthetic flow chart of Example 1 is as follows;
[0019] Attached Figure 2 The X-ray diffraction (XRD) and scanning electron microscope (SEM) images of Comparative Example 1;
[0020] Attached Figure 3 Transmission electron microscope TEM and element mapping diagram of Comparative Example 1;
[0021] Attached Figure 4 XRD and SEM images of Comparative Example 2;
[0022] Attached Figure 5 TEM and element mapping diagram of Comparative Example 2;
[0023] Attached Figure 6 XRD diagrams of Examples 1 to 4 and enlarged images of some areas;
[0024] Attached Figure 7 TEM and element mapping of Example 1;
[0025] Attached Figure 8 are high resolution transmission electron microscopy (HRTEM) images of Examples 1 to 4;
[0026] Attached Fig. 9 Analysis of the proportion of final catalyst phosphide obtained with different amounts of P source;
[0027] Attached Fig.10 The X-ray photoelectron spectroscopy (XPS) diagrams of Example 1 and Comparative Examples 1-2;
[0028] Attached Fig.11 This is a comparison chart of oxygen evolution performance of Examples 1 to 4 after iR correction;
[0029] Attached Fig.12 This is a comparison chart of oxygen evolution performance after iR correction between Example 1 and Comparative Examples 1-2;
[0030] Attached Fig.13 The XRD and SEM images of Example 1 before and after stability;
[0031] Attached Fig.14 XPS before and after stability of Example 1;
[0032] Attached Fig.15 This is the element mapping diagram after stabilization of Example 1. DETAILED DESCRIPTION
[0033] The present invention provides a method for preparing a high-performance oxygen evolution catalyst NiTe / Ni by using lattice strain. 2 Preparation method of P.
[0034] In the present invention, unless otherwise specified, the required raw materials for preparation are all commercially available products well known to those skilled in the art.
[0035] The present invention provides a method for preparing a high-performance oxygen evolution catalyst NiTe / Ni by using lattice strain as described in the above technical solution. 2 Application of P in electrolyzed water. The present invention has no particular limitation on the application method, and the application can be carried out according to methods well known in the art.
[0036] The present invention is further described below in conjunction with specific examples, and the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] Embodiment 1:
[0038] Step (1), 2 mmol Na 2 TeO 3 Dissolve in 20 ml of deionized water, then slowly add 12 ml of N 2 H 4 ·H 2 O, add treated NF after mixing evenly, react at 180℃ for 24h, and dry in nitrogen atmosphere to obtain NiTe;
[0039] Step (2), using the NiTe obtained in step (1) as a carrier, 0.9 mmol C 4 H 6 O 4 Ni·4H 2 O, 2.1mmol NH 4 F and 3.7 mmol CH 4 N 2 O was dissolved in 30 ml of deionized water, then reacted at 120 °C for 6 h and dried under nitrogen atmosphere to obtain NiTe / Ni(OH) 2 ;
[0040] Step (3), using the NiTe / Ni(OH) obtained in step (2) 2 Place the precursor downstream of the tube furnace and 1.0g NaH 2 PO2 Sodium phosphite and NiTe / Ni(OH) 2 The mass ratio is 2:1, and the lattice strained NiTe / Ni is obtained by sintering at 350℃ for 2h. 2 P, named NiTe / Ni(OH) 2 -1.0.
[0041] Embodiment 2:
[0042] Except that the amount of sodium hypophosphite was changed to 0.0 g, the other embodiments were the same as those in Example 1, but NiTe / Ni(OH) 2 , named NiTe / Ni(OH) 2 -0.0.
[0043] Embodiment 3:
[0044] In addition, the amount of sodium hypophosphite was changed to 0.5g (i.e. sodium hypophosphite and NiTe / Ni(OH) 2 The mass ratio is 1:1), and the other embodiments are the same as those in Example 1, and the lattice strained NiTe / Ni 2 P, named NiTe / Ni(OH) 2 -0.5.
[0045] Embodiment 4:
[0046] In addition to changing the amount of sodium hypophosphite to 2.0g (i.e. sodium hypophosphite and NiTe / Ni(OH) 2 The mass ratio is 4:1), and the other embodiments are the same as those in Example 1, and the lattice strained NiTe / Ni 2 P, named NiTe / Ni(OH) 2 -2.0.
[0047] Example 5
[0048] Sodium phosphite and NiTe / Ni(OH) 2 The mass ratio is 10:1, and the other embodiments are the same as those in Example 1, and the lattice strained NiTe / Ni 2 P, but the obtained catalyst is fragile and has relatively poor physical strength and flexibility.
[0049] Comparative Example 1:
[0050] NiTe was obtained by the same method as in Example 1, but the subsequent treatment of secondary introduction of nickel source and phosphating was not performed.
[0051] Comparative Example 2:
[0052] The nickel source was added to NF as a carrier and reacted at 120℃ for 6h to obtain Ni(OH) 2Finally, Ni was obtained by phosphating with 1.0 g of sodium hypophosphite using the vapor deposition method. 2 P.
[0053] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
[0054] Material Characterization and Testing
[0055] Figure 1 NiTe / Ni with strain effect 2 Preparation process of P heterojunction catalyst;
[0056] Figure 2 It is shown that, in comparative example 1, NiTe is successfully prepared and has the morphology of nanobelts;
[0057] Figure 3 This further confirmed the successful preparation of NiTe, and it can be seen that each element is evenly distributed;
[0058] Figure 4 Explanation, Comparative Example 2, Ni 2 The successful preparation of P and its nanosheet morphology;
[0059] Figure 5 Explanation, further determine Ni 2 P was successfully prepared, and it can be seen that the elements are evenly distributed;
[0060] Figure 6 The second line on XRD, i.e., the characterization line corresponding to Example 1, shows that the final catalyst obtained with a higher amount of P source is NiTe phase and Ni 2 The coexistence of P phase confirms the lattice strain of NiTe / Ni 2 Successful preparation of P heterojunction, NiTe phase with compressive strain, Ni 2 The P phase has tensile strain;
[0061] The third line from XRD, i.e., Example 3, confirms the lattice strained NiTe / Ni 2 The successful preparation of P heterojunction; only NiTe phase showed compressive strain, while for Ni 2 The P phase does not show observable tensile strain at this time.
[0062] The XRD patterns of the catalysts obtained with different amounts of P source showed that as the amount of P source increased, the XRD diffraction peaks of the NiTe phase in the obtained samples gradually shifted to the right (left 2), while the Ni 2The XRD diffraction peak of the P phase shows a trend of gradually shifting to the left (Figure 1 on the right). This means that the NiTe phase has compressive strain, and the degree of compressive strain gradually increases with the increase of P source. 2 The P phase has tensile strain, and the degree of tensile strain gradually increases with the increase of P source. The above results also show that we can successfully realize heterojunction catalysts NiTe / Ni with different lattice strains by controlling the amount of different P sources. 2 In particular, from the catalyst materials obtained using different P sources (left 1), it can be seen that when the P source dosage is 0.5g, there is still Ni(OH) 2 phase, and when the P source dosage was 1.0 g, the catalyst composition was completely converted to Ni 2 The heterojunction combination of P and NiTe phases indicates that Ni(OH) 2 The phase has been completely converted to Ni 2 P, and possibly a small amount of NiTe converted to Ni 2 P, which further adjusts the ratio of phosphide and antimonide to adjust the strain of the two phases. And it can be seen from the figure that when the amount of P source is 0.0g, NiTe / Ni(OH) 2 -0.0 does not show obvious strain compared with single NiTe. When the amount of P source increases to 0.5g, NiTe / Ni(OH) 2 -0.5 shows compressive strain for NiTe phase, while for Ni 2 The P phase does not show any observable tensile strain at this time (the lower straight line in the right figure is Ni 2 The standard XRD diffraction peak position of the (201) lattice of P), which further indicates that the appropriate degree of phosphating is an important factor in determining whether the catalyst material itself can have lattice strain;
[0063] Figure 7 It is shown that the NiTe / Ni obtained in Example 1 2 Each element in the P heterojunction catalyst is distributed according to the heterojunction form;
[0064] Figure 8 The successful construction of the heterojunction and the existence of lattice strain were further confirmed by HRTEM. 2 Ni in P heterojunction catalyst 2 The lattice parameter of the (201) crystal plane of the P phase increased from 0.204nm to 0.209nm, and the obtained NiTe / Ni 2 The lattice parameter of the (101) crystal plane of the NiTe phase in the P heterojunction catalyst decreased from 0.288nm to 0.281nm. This phenomenon is consistent with the conclusion we obtained from XRD analysis;
[0065] Fig. 9 It shows that as the amount of P source increases from 0.5g to 2.0g (Example 1, Example 3, Example 4), the XPS peak area ratios of metal phosphide to metal phosphate are 0.30, 0.58, and 0.70, respectively, which indicates that with the increase of P source, more metal phosphide can be formed. This is obvious, but it is important to explain from the side that NiTe and Ni 2 The incompatibility of P determines the degree of strain to a certain extent in the formation of heterojunction, thereby regulating the NiTe / Ni 2 The OER activity and stability of P are reflected in the different strain levels of different phosphide contents.
[0066] Fig.10 In Example 1, NiTe / Ni 2 The successful construction of the heterojunction catalyst of NiTe and Ni 2 P has a significant effect on the electronic structure, and these significant electronic structure adjustments also improve the catalytic performance and stability of the catalyst itself to a certain extent;
[0067] Fig.11 It shows that NiTe / Ni with different lattice strains were prepared by using different amounts of phosphorus source. 2 Among the catalysts P (Example 1, Example 2, Example 3, Example 4), the appropriate lattice strain effect, i.e., Example 1, exhibited the best oxygen evolution catalytic performance; (the measured potential was converted with the reversible hydrogen electrode (RHE) by the formula: E RHE =E Ag / AgCl +0.197+0.059×pH. Using 1M KOH solution as the electrolyte, linear sweep voltammetry (LSV) was performed at 10 mV s -1 By default, all LSV curves are corrected by 80% iR.
[0068] Fig.12 Explanation, NiTe and Ni 2 The interaction between P can effectively improve the 2 P has better oxygen evolution catalytic performance (Example 1, Comparative Example 1, Comparative Example 2) than the OER benchmark catalyst IrO 2 Better catalytic performance; (linear scanning conditions and Fig.11 same).
[0069] Fig.13 Description, stability test (at a fixed current density of 10mA cm -2The catalyst material was characterized and analyzed after testing for 70 h under the test conditions. From the XRD before and after the test and the SEM images before and after the test, it can be seen that the sample NiTe / Ni obtained in Example 1 2 There is no obvious effect on P composition and morphology, which proves that this catalytic material has good stability;
[0070] Fig.14 Description, stability test (at a fixed current density of 10mA cm -2 The electronic structure of the catalyst material was analyzed after the test for 70 h under the test conditions. From the XPS images before and after the test, it can be seen that the stability test before and after the test of the NiTe / Ni sample obtained in Example 1 2 The P electronic structure also did not change significantly, which also means that NiOOH did not appear after the OER test, once again confirming the good stability of this catalytic material;
[0071] Fig.15 Note that after stability test (at a fixed current density of 10 mA cm -2 The catalyst material was characterized and analyzed under the test conditions for 70 h. From the TEM images before and after the test, it can be seen that the stability test of the NiTe / Ni sample obtained in Example 1 2 The type and distribution of P element have negligible effects, further confirming the stability of this catalytic material.
[0072] After the above analysis, it can be seen that NiTe / Ni 2 The construction of P heterojunction can effectively adjust the degree of lattice strain, giving NiTe / Ni 2 P has better catalytic performance. More importantly, the generation of this lattice strain provides effective guarantee for structural stability in OER tests. Compared with other Ni-based catalysts that have been widely studied, NiOOH was not observed after stability tests. This work has certain guiding significance for the preparation of catalysts through strain engineering.
Claims
1. A method for preparing a high-performance oxygen evolution catalyst using lattice strain, characterized in that: The following steps are involved: Step (1), preparing NiTe by a hydrothermal method using nickel foam (NF) as a nickel source; Step (2), using NiTe as a carrier, and introducing a nickel source again for hydrothermal reaction to obtain NiTe / Ni(OH)2; Step (3), using the NiTe / Ni(OH)2 prepared in step (2) as a precursor, and performing phosphating by a vapor deposition method to obtain a heterojunction catalyst NiTe / Ni2P with lattice strain; the lattice strain is that NiTe and Ni2P have compression and tensile strain on the lattice respectively; In step (3), the NiTe / Ni(OH)2 obtained in step (2) is placed as a precursor downstream of a tube furnace, and NaH2PO2 is placed upstream, and sintered at 300-500°C for 2-5 h to obtain NiTe / Ni2P; While Ni(OH)2 is phosphated to Ni2P, NiTe is also slightly phosphated, causing the NiTe phase to exhibit compressive strain and the Ni2P phase to have tensile strain.
2. A method for preparing a high-performance oxygen evolution catalyst by using lattice strain according to claim 1, characterized in that: Step (1): Na2TeO3 is dissolved in deionized water, and then N2H4·H2O (hydrazine hydrate) is slowly and continuously added. For every 2 mmol of Na2TeO3 solution, 20 ml of deionized water and 12 ml of N2H4·H2O (hydrazine hydrate) are used. After mixing evenly, the treated NF is added and reacted at 100~250℃ for 10 h-25 h. NiTe is obtained by drying in a nitrogen atmosphere.
3. A method for preparing a high-performance oxygen evolution catalyst by using lattice strain according to claim 1, characterized in that: Step (2) Using the NiTe obtained in step (1) as a carrier, a mixture of C4H6O4Ni·4H2O, NH4F, CH4N2O and deionized water is added to a hydrothermal autoclave, with 2.1 mmol NH4F, 3.7 mmol CH4N2O and 30 ml deionized water corresponding to every 0.9 mmol C4H6O4Ni·4H2O, followed by reaction at 50-180°C for 3 h-12 h, and drying under nitrogen atmosphere to obtain NiTe / Ni(OH)2.
4. A method for preparing a high-performance oxygen evolution catalyst by using lattice strain according to claim 1, characterized in that: The mass ratio of NaH2PO2 to NiTe / Ni(OH)2 is 1:40 ~ 25:
1.
5. A method for preparing a high-performance oxygen evolution catalyst by using lattice strain according to claim 1, characterized in that: Sintered at 350 °C for 2 h, the mass ratio of sodium hypophosphite to NiTe / Ni(OH)2 is 1:10 ~ 15:
1.
6. A method for preparing a high-performance oxygen evolution catalyst by using lattice strain according to claim 5, characterized in that: The mass ratio of sodium hypophosphite to NiTe / Ni(OH)2 is 1:5 ~ 10:
1.
7. A high-performance oxygen evolution catalyst prepared by using lattice strain, prepared according to the method of any one of claims 1 to 6.
8. Use of a high-performance oxygen evolution catalyst prepared by lattice strain according to the method of any one of claims 1 to 6, in electrolysis of water, in an alkaline aqueous solution, to reduce NiOOH generation and increase stability and catalyst life.