Preparation method of electrode modification film based on electric field effect
By preparing an electrode-modified film under the influence of an electric field, the movement of reactive particles in the electrolyte is optimized, solving the problem of slow oxygen evolution reaction rate. This achieves efficient electrode preparation and excellent performance, making it suitable for various electrocatalytic and photoelectrocatalytic applications.
Patent Information
- Application Number
- CN202410673600.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-28
- Publication Date
- 2024-11-12
AI Technical Summary
In existing technologies for electrochemical water splitting, the oxygen evolution reaction (OER) has a slow reaction rate, and research has paid little attention to the mass transfer process of the electrolyte, resulting in a technological gap in improving the OER reaction rate.
An electrode modification film based on electric field effect is prepared by uniformly stirring polymer materials, filler particles and negatively charged particles in an organic solvent, coating them on a substrate and curing them to form a thin film for electrode assembly, thereby optimizing the movement of reactive particles.
It significantly reduces electrode overpotential, simplifies electrode preparation, improves oxygen evolution performance, and the film is resistant to corrosion, acid and alkali environments, recyclable, and low in cost, making it suitable for electrocatalysis and photoelectrocatalysis.
Smart Images

Figure CN118932410A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrochemical water decomposition to produce hydrogen, in particular to a method for preparing an electrode modified film based on electric field modulation. Background Art
[0002] People are gradually paying more attention to the environment, and the development of clean and renewable energy has become an important topic worthy of research and innovation.
[0003] The field of electrochemical water splitting for hydrogen production mentioned above refers to the field of using electrical energy to cause water to undergo a cracking reaction to obtain hydrogen energy. At present, in the water splitting reaction, researchers often divide the cracking into two parts, that is, using two half reactions, oxygen evolution reaction (Oxygen Evolution Reaction, OER) and hydrogen evolution reaction (Hydrogen Evolution Reaction, HER), to conduct research on higher energy utilization. Compared with the HER reaction process, OER is more complicated and the reaction kinetics are slower. Increasing the OER reaction rate is more conducive to breaking the technical barriers to water splitting. So we focus more on speeding up the reaction rate of OER.
[0004] In actual OER, it can be roughly divided into several steps, including the transfer process of electrons and holes, the directional movement of reaction particles in the electrolyte, and the adsorption process on the catalyst surface. For example, CN102443818A, CN106995229B, and CN113786853B, most inventions focus on the changes in the electrode itself to accelerate the transfer process of electrons and holes, while few people have studied the electrolyte part, analyzing and improving the OER reaction rate from the mass transfer process, and there are some gaps in the research of electrocatalysis. Summary of the invention
[0005] Purpose of the invention: To solve the above problems, the present invention provides a method for preparing an electrode modified membrane based on electric field action, based on changing the coordination of water molecules of reaction particles in the electrolyte through electric field to accelerate their movement speed to achieve the purpose of enhancing the oxygen evolution reaction. The preparation method of the present invention is very simple and has obvious enhancement effect.
[0006] The technical solution of the present invention is: a method for preparing an electrode modified film based on electric field action, and the specific steps are as follows:
[0007] S1: Add polymer materials, filler particles and negatively charged particles into an organic solvent and stir until a uniformly dispersed viscous solution that can adhere to the wall is obtained;
[0008] S2: Evenly dip the solution obtained in step S1 onto the substrate, then hold the substrate horizontally and scrape off excess solution on the substrate, and then spray the solution onto both sides of the substrate to solidify it to obtain a thin film;
[0009] S3: After ultrasonically cleaning the film obtained in step S2 in a solution, air-drying or baking to obtain an electrode modification film based on electric field action that can be assembled with an electrode.
[0010] Preferably, the polymer material described in step S1 is a mixture of one or more of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-chlorotrifluoroethylene or polyvinylidene fluoride-trifluoroethylene; the number average molecular weight of the polymer material is 400,000-900,000.
[0011] Preferably, the mass of the polymer material added in step S1 accounts for 10-20% of the organic solvent.
[0012] Preferably, the filling particles in step S1 are a mixture of one or more of barium titanate or lead zirconate titanate; and the negatively charged particles are a mixture of one or more of kaolinite, illite, hydrotalcite or Mxene.
[0013] Preferably, the added mass of the filling particles in step S1 accounts for 0-90% of the polymer material; the added mass of the negatively charged particles accounts for 0-2% of the organic solvent; and the added masses of the filling particles and the negatively charged particles cannot be zero at the same time.
[0014] Preferably, the organic solvent in step S1 is one or a mixture of acetone or dimethyl diamide.
[0015] Preferably, the solidified solution in step S2 is a solution of water and / or ethanol in any ratio.
[0016] Preferably, the substrate described in step S2 is a carbon cloth or nylon mesh porous substrate.
[0017] Preferably, the washing solution in step S3 is water and / or ethanol.
[0018] The present invention also provides an electrode modification film based on electric field action, characterized in that it is prepared by the above-mentioned preparation method.
[0019] Beneficial effects: The electrode modification film based on electric field in the present invention can significantly reduce the electrode overpotential. Compared with the modification of the electrode or catalyst, the present invention uses the modified film to assemble with the commercial electrode, which simplifies the preparation process of the excellent electrode. The film is corrosion-resistant, acid-base-resistant, and recyclable. It can improve the oxygen evolution performance when assembled with different electrodes in various occasions. In addition, the preparation cost of the present invention is low, and it has a wide range of application prospects in the fields of electrocatalysis and photoelectrocatalysis. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The overall network SEM image of the film (Example 3) prepared for polyvinylidene fluoride-hexafluoropropylene and barium titanate;
[0021] Figure 2A local magnified SEM image of a thin film prepared from polyvinylidene fluoride-hexafluoropropylene and barium titanate (Example 3). DETAILED DESCRIPTION
[0022] The present invention will be further described below in conjunction with the accompanying drawings.
[0023] A method for preparing an electrode modification film based on electric field action of the present invention comprises the following steps:
[0024] S1: Add polymer materials, filler particles and negatively charged particles into an organic solvent and stir until a uniformly dispersed viscous solution that can adhere to the wall is obtained;
[0025] S2: Evenly dip the solution obtained in step S1 onto the substrate, then hold the substrate horizontally and scrape off excess solution on the substrate, and then spray the solution onto both sides of the substrate to solidify it to obtain a thin film;
[0026] S3: After ultrasonically cleaning the film obtained in step S2 in a solution, air-drying or baking can obtain an electrode modification film based on electric field action that can be assembled with an electrode.
[0027] Example 1
[0028] Polyvinylidene fluoride-hexafluoropropylene, kaolin and nylon mesh are selected as raw materials. The specific implementation process is as follows:
[0029] Preparation of kaolin-doped polyvinylidene fluoride film: Weigh 0.5g polyvinylidene fluoride-hexafluoropropylene (molecular weight 400,000-455,000) and 0.07g kaolin powder, place in 5g dimethylformamide solution, stir until completely dissolved, evenly apply to 1×2cm nylon mesh, solidify with water: ethanol = 5:5, then wash under ultrasonic conditions with water: ethanol = 1:9 solution, dry at 60°C to obtain a film. The polyvinylidene fluoride-hexafluoropropylene accounts for 10% of the film, and kaolin accounts for 1.4%.
[0030] Example 2
[0031] Polyvinylidene fluoride-chlorotrifluoroethylene, hydrotalcite and carbon cloth are selected as raw materials, and the specific implementation process is as follows:
[0032] Preparation of kaolin-doped polyvinylidene fluoride film: Weigh 0.5g polyvinylidene fluoride-chlorotrifluoroethylene (molecular weight 600,000-700,000) and 0.07g hydrotalcite, place in 5g dimethylformamide solution, stir until completely dissolved, evenly apply to 1×2cm carbon cloth, solidify with ethanol, and then clean with a solution of water: ethanol = 3:7 under ultrasonic conditions, dry at 50°C to obtain a film. The polyvinylidene fluoride-chlorotrifluoroethylene accounts for 10% of the film, and the hydrotalcite accounts for 1.4%.
[0033] Example 3
[0034] Polyvinylidene fluoride-hexafluoropropylene, barium titanate and nylon mesh are selected as raw materials. The specific implementation process is as follows:
[0035] Weigh 0.5g of polyvinylidene fluoride-hexafluoropropylene (molecular weight 400,000-455,000) and 0.20g of barium titanate powder, place in 5g of dimethylformamide solution, stir until completely dissolved, evenly apply to 1×2cm nylon mesh, solidify with water, then clean with ethanol solution under ultrasonic conditions, dry at 70℃ to obtain a film. The film contains 10% polyvinylidene fluoride-hexafluoropropylene and 40% barium titanate.
[0036] Combined with the SEM image in the attached figure, it can be found that barium titanate is uniformly distributed in polyvinylidene fluoride-hexafluoroethylene to form a porous film.
[0037] Example 4
[0038] Polyvinylidene fluoride and nylon mesh are selected as raw materials, and the specific implementation process is as follows:
[0039] Weigh 1g of polyvinylidene fluoride (molecular weight 800,000-900,000), 0.2g of barium titanate powder, and 0.05g of kaolin, place in 5g of dimethylformamide solution, stir until completely dissolved, evenly apply to 1×2cm nylon mesh, solidify with water, and then clean with a solution of water: ethanol = 3:7 under ultrasonic conditions, and dry to obtain a film. The film contains 20% polyvinylidene fluoride-hexafluoropropylene, 40% barium titanate, and 1% kaolin.
[0040] Example 5
[0041] Polyvinylidene fluoride-hexafluoropropylene, barium titanate and nylon mesh are selected as raw materials. The specific implementation process is as follows:
[0042] Weigh 0.5g of polyvinylidene fluoride-hexafluoropropylene (molecular weight 400,000-455,000) and 0.40g of barium titanate powder, place in 5g of dimethylformamide solution, stir until completely dissolved, evenly apply to 1×2cm nylon mesh, solidify with water, then clean with ethanol solution under ultrasonic conditions, dry at 80℃ to obtain a film. The film contains 10% polyvinylidene fluoride-hexafluoropropylene and 80% barium titanate.
[0043] Example 1-5 uses nickel foam as the test electrode, which is assembled with nylon rope and subjected to ultrasonic treatment for 1 minute. The performance test results under controlled temperature conditions are shown in the following table:
[0044]
[0045] The film of Example 3 was selected and assembled with different electrodes by nylon rope, and ultrasonicated for 1 minute. The performance test under the controlled temperature condition is shown in the following table:
[0046]
[0047] According to the above table, it can be found that under different electrodes, different types and contents of negatively charged particles, and different filling particles, the overpotential and current are well optimized after thin film ultrasound.
Claims
1. A method for preparing an electrode modified film based on electric field action, the specific steps of which are as follows: S1: Add polymer materials, filler particles and negatively charged particles into an organic solvent and stir until a uniformly dispersed viscous solution that can adhere to the wall is obtained; S2: The solution obtained in step S1 is evenly dipped on the substrate, and then the substrate is horizontally scraped to remove the excess solution on the substrate, and then the solution is sprayed on both sides of the substrate to solidify it to obtain a thin film; S3: After ultrasonically cleaning the film obtained in step S2 in a solution, air-drying or baking to obtain an electrode modification film based on electric field action that can be assembled with an electrode.
2. The preparation method according to claim 1, characterized in that: The polymer material described in step S1 is a mixture of one or more of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-chlorotrifluoroethylene or polyvinylidene fluoride-trifluoroethylene; the number average molecular weight of the polymer material is 400,000-900,000.
3. The preparation method according to claim 1, characterized in that: The mass of the polymer material added in step S1 accounts for 10-20% of the organic solvent.
4. The preparation method according to claim 1, characterized in that: The filling particles in step S1 are a mixture of one or more of barium titanate or lead zirconate titanate; the negatively charged particles are a mixture of one or more of kaolinite, illite, hydrotalcite or Mxene.
5. The preparation method according to claim 1, characterized in that: The added mass of the filling particles in step S1 accounts for 0-90% of the polymer material; the added mass of the negatively charged particles accounts for 0-2% of the organic solvent; and the added masses of the filling particles and the negatively charged particles cannot be zero at the same time.
6. The preparation method according to claim 1, characterized in that: The organic solvent in step S1 is one or a mixture of acetone or dimethyl diamide.
7. The preparation method according to claim 1, characterized in that: The solidified solution in step S2 is a solution of water and / or ethanol in any ratio.
8. The preparation method according to claim 1, characterized in that: The substrate described in step S2 is a carbon cloth or nylon mesh porous substrate.
9. The preparation method according to claim 1, characterized in that: The washing solution in step S3 is water and / or ethanol.
10. An electrode modification film based on electric field action, characterized in that: Prepared by the preparation method according to any one of claims 1 to 9.