Waterproof and moisture-proof recycled rubber mortar and preparation method thereof

By using Escherichia coli biomineralization to deposit silica in recycled rubber mortar, the problem of reduced compressive strength of recycled rubber mortar is solved, high compressive strength and waterproof and moisture-proof properties are achieved, the scope of application is expanded and the environmental pollution.

CN116477906BActive Publication Date: 2024-10-15ZHONGSHAN WANYI CONCRETE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310485404.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-04
Publication Date
2024-10-15
Estimated Expiration
2043-05-04

AI Technical Summary

Technical Problem

While the recycled rubber mortar improves its waterproof and moisture-proof performance, its compressive strength decreases, which limits its application scope.

Method used

By soaking the regenerated rubber powder in an acetic acid solution and treating it in an E. coli culture solution, the biomineralization of E. coli is used to deposit silica, so that the surface of the regenerated rubber powder is embedded with silica, thereby improving its strength and bonding with cement. Adhesion and enhanced compressive strength.

Benefits of technology

It effectively improves the compressive strength and waterproof and moisture-proof properties of recycled rubber mortar, making it applicable to a wider range of applications. It also consumes waste rubber materials through modification processing and reduces environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004208411120000071
    Figure BDA0004208411120000071
Patent Text Reader

Abstract

The present invention relates to the technical field of building materials, and specifically discloses a waterproof and moisture-proof recycled rubber mortar and a preparation method thereof. The waterproof and moisture-proof recycled rubber mortar comprises the following components: water, cement, fly ash, fine aggregate, modified recycled rubber powder, and a water reducer. The modified recycled rubber powder is modified as follows: 1) the recycled rubber powder is put into an acetic acid solution with a concentration of 10-15%, soaked for 10-15 minutes, filtered and cleaned to obtain pre-treated rubber powder; 2) Escherichia coli is put into a liquid culture medium and cultured to an OD value of 2-2.2 to obtain a cultured bacterial solution; 3) the pre-treated rubber powder is put into the cultured bacterial solution and soaked for 8-12 hours, the pre-treated rubber powder is filtered out and put into a modified solution containing a silicon source and soaked for 7-10 days, filtered, and dried to obtain the modified recycled rubber powder. The present invention has the advantages of making the recycled rubber mortar have better waterproof and moisture-proof properties while having higher compressive strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of building materials, in particular to a waterproof and moisture-proof recycled rubber mortar and a preparation method thereof. Background Art

[0002] Cement mortar is a mortar made of cement, fine aggregate and water, and does not contain coarse aggregate.

[0003] Recycled rubber mortar is a cement mortar made by partially replacing the sand in the mortar with waste rubber powder. The addition of waste rubber powder can better fill the pores of the cement mortar and effectively improve the density of the cement mortar, thereby making the cement mortar surface have stronger waterproof and moisture-proof properties. Moreover, since rubber has a certain elasticity, the prepared cement mortar has higher ductility and improved crack resistance.

[0004] However, it was found in experiments that the addition of rubber will affect the strength of cement mortar. For example, in the study of "Research on the Performance of Rubber Modified Cement Mortar", Zhang Jing et al. found that when the rubber dosage increased to 30%, the corresponding 3 and 7d compressive strength distribution decreased by 53.65% and 42.92%, and the corresponding 3 and 7d flexural strength decreased by 28.50% and 23.38%, respectively.

[0005] Therefore, although the addition of rubber powder can improve the waterproof and moisture-proof properties of the mortar and can reduce costs by replacing part of the fine aggregate, the addition of rubber powder also brings about the problem of reduced mortar strength, which limits the application of rubber mortar. Therefore, there is still room for improvement. Summary of the invention

[0006] In order to make the recycled rubber mortar have better waterproof and moisture-proof properties and higher compressive strength, the present application provides a waterproof and moisture-proof recycled rubber mortar and a preparation method thereof.

[0007] In a first aspect, the present application provides a waterproof and moisture-proof recycled rubber mortar, which adopts the following technical solution:

[0008] A waterproof and moisture-proof recycled rubber mortar, comprising the following components in parts by mass:

[0009] 165 parts of water;

[0010] Cement 258-262 parts;

[0011] Fly ash 58-62 parts;

[0012] Fine aggregate 1310-1320 parts;

[0013] 560-570 parts of modified recycled rubber powder;

[0014] Water reducing agent 2.8-3.2 parts;

[0015] The modification method of the modified regenerated rubber powder is as follows:

[0016] Step 1), putting the regenerated rubber powder into an acetic acid solution with a concentration of 10-15%, soaking for 10-15 minutes, filtering and washing, and obtaining pretreated rubber powder;

[0017] Step 2), adding Escherichia coli into a liquid culture medium and culturing until the OD value is 2-2.2 to obtain a culture solution;

[0018] Step 3), soaking the pretreated rubber powder in a culture solution for 8-12 hours, filtering out the pretreated rubber powder and soaking it in a modification solution containing a silicon source for 7-10 days, filtering, and drying to obtain modified recycled rubber powder.

[0019] By adopting the above technical scheme, the recycled rubber powder is immersed in an acetic acid solution, and the acetic acid slightly corrodes the recycled rubber powder, making the surface of the recycled rubber powder rougher and forming more pits. The recycled rubber powder is immersed in a culture solution so that Escherichia coli can firmly adhere to the surface of the recycled rubber powder. Then, a silicon source is provided by a modified liquid containing a silicon source, and the biomineralization of Escherichia coli is utilized to deposit silica on the surface of the recycled rubber powder. Since silica is gradually "grown", silica can be firmly "embedded" in the recycled rubber powder, which has a good reinforcing effect on the recycled rubber powder, making the strength of the recycled rubber powder higher, so that the recycled rubber powder can withstand more force when used as a filler, thereby effectively improving the compressive strength of the recycled rubber mortar.

[0020] At the same time, since the surface of the recycled rubber powder is inlaid with silica, the compatibility with cement is greatly improved, so that the bonding strength between the recycled rubber powder and cement is significantly improved, thereby further improving the compressive strength of the recycled rubber mortar. The obtained recycled rubber mortar has good waterproof and moisture-proof properties while having high compressive strength, which makes the quality of the rubber mortar better and its application range wider.

[0021] Preferably, in step 2), the liquid culture medium comprises the following components in parts by weight:

[0022] Peptone 10-15 parts;

[0023] 5-10 parts of yeast extract;

[0024] Sodium chloride 10-15 parts;

[0025] 1000 parts of water.

[0026] By adopting the above technical solution, Escherichia coli can be quickly activated, so that the Escherichia coli can reproduce faster, the time for culturing Escherichia coli can be shortened, and the economic value is higher.

[0027] Preferably, in step 2), the modified liquid comprises the following components in parts by weight:

[0028] Peptone 10-15 parts;

[0029] 5-10 parts of yeast extract;

[0030] Sodium chloride 10-15 parts;

[0031] 30-40 parts of starch;

[0032] 1000 parts water;

[0033] Liquid sodium silicate 1000-1100 parts.

[0034] By adopting the above technical solution and selecting a special modification liquid, the deposition of silica by Escherichia coli can be better promoted, so that the deposition rate of silica on the reclaimed rubber powder is accelerated, the modification cycle is shortened, and the economic value is better improved.

[0035] Preferably, the concentration of the liquid sodium silicate is 40%.

[0036] By adopting the above technical solution and specifically selecting the concentration of liquid sodium silicate, the effect of providing a silicon source is better, thereby better promoting the deposition of silicon dioxide and achieving a better effect of modifying the regenerated rubber powder.

[0037] Preferably, in the step 1), the regenerated rubber powder is soaked in the acetic acid solution and then cleaned with an ethanol solution with a concentration of 10-20%.

[0038] By adopting the above technical solution and cleaning with ethanol solution, the acetic acid solution on the regenerated rubber powder can be better cleaned, thereby reducing the situation where the acetic acid residue causes continuous corrosion to the regenerated rubber powder.

[0039] Preferably, in step 1), the specification of the recycled rubber powder is 40-60 mesh.

[0040] By adopting the above technical solution and specifically selecting the specifications of the recycled rubber powder, the effect of filling the mortar pores is better, the mortar deformation is evenly distributed, and the compressive strength is higher.

[0041] Preferably, in step 3), the filtered pretreated rubber powder is put into a filter bag, and the filter bag containing the pretreated rubber powder is completely submerged in the modified liquid by a weight.

[0042] By adopting the above technical solution, the pretreated rubber powder is completely immersed in the modifying liquid to ensure the modification effect of the recycled rubber powder, and the quality of the prepared mortar is better.

[0043] In a second aspect, the present application provides a method for preparing waterproof and moisture-proof recycled rubber mortar, which adopts the following technical solution:

[0044] A method for preparing the above-mentioned waterproof and moisture-proof recycled rubber mortar is characterized in that it comprises the following steps:

[0045] Step 1), taking part of the water, adding cement, fly ash, modified recycled rubber powder, and water reducing agent, mixing well, and obtaining a premix;

[0046] Step 2), add fine aggregate into the premix, mix well, then add remaining water, mix well, and obtain waterproof and moisture-proof recycled rubber mortar.

[0047] By adopting the above technical scheme, by first mixing cement, fly ash, modified recycled rubber powder, and water reducing agent and then adding fine aggregate to mix, the prepared mortar has uniform distribution of components, high density, better waterproof and moisture-proof effect, and better quality.

[0048] In summary, this application has the following beneficial effects:

[0049] 1. In the present application, the recycled rubber powder is immersed in an acetic acid solution, and the acetic acid slightly corrodes the recycled rubber powder, making the surface of the recycled rubber powder rougher and forming more pits. The recycled rubber powder is immersed in a culture solution so that Escherichia coli can firmly adhere to the surface of the recycled rubber powder. Then, a silicon source is provided by a modified solution containing a silicon source, and the biomineralization of Escherichia coli is utilized to deposit silica on the surface of the recycled rubber powder. Since the silica is gradually "grown", the silica can be firmly "embedded" in the recycled rubber powder, which has a good reinforcing effect on the recycled rubber powder, making the strength of the recycled rubber powder higher, so that the recycled rubber powder can withstand more force when used as a filler, thereby effectively improving the compressive strength of the recycled rubber mortar.

[0050] 2. In the present application, it is preferred to select a special modification liquid to better promote the deposition of silica by Escherichia coli, thereby accelerating the deposition of silica on the regenerated rubber powder, shortening the modification cycle, and better improving the economic value.

[0051] 3. In the present application, it is preferred to specifically select the concentration of liquid sodium silicate to provide a better effect of silicon source, thereby better promoting the deposition of silicon dioxide and achieving a better effect of modifying the regenerated rubber powder. DETAILED DESCRIPTION

[0052] The present application is further described in detail below with reference to the embodiments.

[0053] Example 1

[0054] A waterproof and moisture-proof recycled rubber mortar is prepared from the following components by mass: 165kg water, 258kg cement, 58kg fly ash, 1310kg fine aggregate, 560kg modified recycled rubber powder, and 2.8kg water reducing agent.

[0055] Among them, the cement is ordinary Portland cement, purchased from Runfeng Cement, specification P.O42.5R.

[0056] Among them, the fly ash is secondary fly ash, which was purchased from Baiyi Mineral Products Processing Plant in Lingshou County.

[0057] Among them, the fine aggregate is river sand, which was purchased from Lingshou County Chenyang Mineral Products Co., Ltd. with a specification of 10-20 mesh.

[0058] Among them, the water reducer is polycarboxylic acid water reducer, which was purchased from Shandong Xinhongyue Chemical Co., Ltd.

[0059] Among them, the modification method of modified recycled rubber powder is as follows:

[0060] Step 1), putting 1000 kg of recycled rubber powder into 2000 kg of 10% acetic acid solution, soaking for 15 minutes, filtering and washing twice with 10% ethanol solution to clean, to obtain pretreated rubber powder;

[0061] Step 2), 10 mg of Escherichia coli was added to 2000 kg of liquid culture medium and cultured until the OD value was 2 to obtain a culture solution;

[0062] Step 3), the pretreated rubber powder is immersed in a culture solution for 12 hours, the pretreated rubber powder is filtered out and immersed in 2000 kg of a modification solution containing a silicon source for 7 days, filtered, and dried to obtain modified recycled rubber powder.

[0063] Wherein, in step 2), the liquid culture medium is composed of the following components in the following proportions:

[0064] Peptone: yeast extract: sodium chloride: water = 10:5:10:1000.

[0065] Wherein, in step 2), the Escherichia coli was purchased from Shanghai Collection Biotechnology Center with the serial number SHBCCD80665.

[0066] Wherein, in step 3), the modified liquid is prepared by the following proportions of components:

[0067] Peptone: yeast extract: sodium chloride: starch: water: liquid sodium silicate = 10:5:10:30:1000:1000.

[0068] Among them, liquid sodium silicate was purchased from Shandong Xinyuhang Fine Chemical Co., Ltd., and the concentration of sodium silicate was 40%.

[0069] Among them, in step 1), the recycled rubber powder is purchased from Lingshou County Malin Mineral Products Processing Plant, and the specification is 40 mesh.

[0070] The preparation method of waterproof and moisture-proof recycled rubber mortar is as follows:

[0071] Step 1), 50% water is put into a stirring tank, and then cement, fly ash, modified recycled rubber powder, and water reducing agent are added, the speed is 120r / min, stirred for 3min, and mixed to obtain a premix;

[0072] Step 2), add fine aggregate to the premix, rotate at 120 r / min, stir for 1 min, mix well, then add remaining water, rotate at 120 r / min, stir for 2 min, mix well, and obtain waterproof and moisture-proof recycled rubber mortar.

[0073] Example 2

[0074] A waterproof and moisture-proof recycled rubber mortar is prepared from the following components by mass: 165kg of water, 260kg of cement, 60kg of fly ash, 1315kg of fine aggregate, 565kg of modified recycled rubber powder, and 3kg of water reducing agent.

[0075] Among them, the cement is ordinary Portland cement, purchased from Runfeng Cement, specification P.O42.5R.

[0076] Among them, the fly ash is secondary fly ash, which was purchased from Baiyi Mineral Products Processing Plant in Lingshou County.

[0077] Among them, the fine aggregate is river sand, which was purchased from Lingshou County Chenyang Mineral Products Co., Ltd. with a specification of 10-20 mesh.

[0078] Among them, the water reducer is polycarboxylic acid water reducer, which was purchased from Shandong Xinhongyue Chemical Co., Ltd.

[0079] Among them, the modification method of modified recycled rubber powder is as follows:

[0080] Step 1), putting 1000 kg of recycled rubber powder into 2000 kg of 12% acetic acid solution, soaking for 12 minutes, filtering and washing twice with 15% ethanol solution to clean, to obtain pretreated rubber powder;

[0081] Step 2), 10 mg of Escherichia coli was added to 2000 kg of liquid culture medium and cultured until the OD value was 2.1 to obtain a culture solution;

[0082] Step 3), the pretreated rubber powder is immersed in a culture solution for 10 hours, the pretreated rubber powder is filtered out and immersed in 2000 kg of a modification solution containing a silicon source for 8 days, filtered, and dried to obtain modified recycled rubber powder.

[0083] Wherein, in step 2), the liquid culture medium is composed of the following components in the following proportions:

[0084] Peptone: yeast extract: sodium chloride: water = 12:7:12:1000.

[0085] Wherein, in step 2), the Escherichia coli was purchased from Shanghai Collection Biotechnology Center with the serial number SHBCCD80665.

[0086] Wherein, in step 3), the modified liquid is prepared by the following proportions of components:

[0087] Peptone: yeast extract: sodium chloride: starch: water: liquid sodium silicate = 12:7:12:35:1000:1050.

[0088] Among them, liquid sodium silicate was purchased from Shandong Xinyuhang Fine Chemical Co., Ltd., and the concentration of sodium silicate was 40%.

[0089] Among them, in step 1), the recycled rubber powder is purchased from Lingshou County Malin Mineral Products Processing Plant, and the specification is 40 mesh.

[0090] The preparation method of waterproof and moisture-proof recycled rubber mortar is as follows:

[0091] Step 1), 50% water is put into a stirring tank, and then cement, fly ash, modified recycled rubber powder, and water reducing agent are added, the speed is 120r / min, stirred for 3min, and mixed to obtain a premix;

[0092] Step 2), add fine aggregate to the premix, rotate at 120 r / min, stir for 1 min, mix well, then add remaining water, rotate at 120 r / min, stir for 2 min, mix well, and obtain waterproof and moisture-proof recycled rubber mortar.

[0093] Example 3

[0094] A waterproof and moisture-proof recycled rubber mortar is prepared from the following components by mass: 165kg water, 262kg cement, 62kg fly ash, 1320kg fine aggregate, 570kg modified recycled rubber powder, and 3.2kg water reducing agent.

[0095] Among them, the cement is ordinary Portland cement, purchased from Runfeng Cement, specification P.O42.5R.

[0096] Among them, the fly ash is secondary fly ash, which was purchased from Baiyi Mineral Products Processing Plant in Lingshou County.

[0097] Among them, the fine aggregate is river sand, which was purchased from Lingshou County Chenyang Mineral Products Co., Ltd. with a specification of 10-20 mesh.

[0098] Among them, the water reducer is polycarboxylic acid water reducer, which was purchased from Shandong Xinhongyue Chemical Co., Ltd.

[0099] Among them, the modification method of modified recycled rubber powder is as follows:

[0100] Step 1), putting 1000 kg of recycled rubber powder into 2000 kg of 15% acetic acid solution, soaking for 10 minutes, filtering and washing twice with 20% ethanol solution to clean, to obtain pretreated rubber powder;

[0101] Step 2), 10 mg of Escherichia coli was added to 2000 kg of liquid culture medium and cultured until the OD value was 2.2 to obtain a culture solution;

[0102] Step 3), the pretreated rubber powder is immersed in a culture solution for 8 hours, the pretreated rubber powder is filtered out and immersed in 2000 kg of a modification solution containing a silicon source for 10 days, filtered, and dried to obtain modified recycled rubber powder.

[0103] Wherein, in step 2), the liquid culture medium is composed of the following components in the following proportions:

[0104] Peptone: yeast extract: sodium chloride: water = 15:10:15:1000.

[0105] Wherein, in step 2), the Escherichia coli was purchased from Shanghai Collection Biotechnology Center with the serial number SHBCCD80665.

[0106] Wherein, in step 3), the modified liquid is prepared by the following proportions of components:

[0107] Peptone: yeast extract: sodium chloride: starch: water: liquid sodium silicate = 15:10:15:40:1000:1100.

[0108] Among them, liquid sodium silicate was purchased from Shandong Xinyuhang Fine Chemical Co., Ltd., and the concentration of sodium silicate was 40%.

[0109] Among them, in step 1), the recycled rubber powder is purchased from Lingshou County Malin Mineral Products Processing Plant, and the specification is 60 mesh.

[0110] The preparation method of waterproof and moisture-proof recycled rubber mortar is as follows:

[0111] Step 1), 50% water is put into a stirring tank, and then cement, fly ash, modified recycled rubber powder, and water reducing agent are added, the speed is 120r / min, stirred for 3min, and mixed to obtain a premix;

[0112] Step 2), add fine aggregate to the premix, rotate at 120 r / min, stir for 1 min, mix well, then add remaining water, rotate at 120 r / min, stir for 2 min, mix well, and obtain waterproof and moisture-proof recycled rubber mortar.

[0113] Comparative Example 1

[0114] A waterproof and moisture-proof recycled rubber mortar, compared with Example 2, the only difference is:

[0115] An equal amount of Rhizopus sphenanthera was used to replace Escherichia coli.

[0116] Among them, Rhizopus vinifera was purchased from Beijing Biobo Biotechnology Co., Ltd. with the number: ATCC 14037.

[0117] Comparative Example 2

[0118] A waterproof and moisture-proof recycled rubber mortar, compared with Example 2, the only difference is:

[0119] Ethyl orthosilicate was used to replace the liquid sodium silicate in equal amounts.

[0120] Among them, ethyl orthosilicate was purchased from Jinan Junteng Chemical Co., Ltd. with a content of 40%.

[0121] Comparative Example 3

[0122] A waterproof and moisture-proof recycled rubber mortar, compared with Example 2, the only difference is:

[0123] Use recycled rubber powder to replace the modified recycled rubber powder in equal amounts.

[0124] Among them, the one purchased from Malin Mineral Products Processing Plant in Lingshou County has a specification of 40 mesh.

[0125] Comparative Example 4

[0126] A waterproof and moisture-proof recycled rubber mortar, compared with Example 2, the only difference is:

[0127] Use an equal amount of fine aggregate to replace the modified recycled rubber powder.

[0128] Among them, the fine aggregate is river sand, which was purchased from Lingshou County Chenyang Mineral Products Co., Ltd. with a specification of 10-20 mesh.

[0129] Experiment 1

[0130] According to JC / T984-2005 "Polymer Cement Waterproof Mortar", the compressive strength, flexural strength and impermeability strength of the samples prepared from the recycled rubber mortar of each embodiment and comparative example were tested.

[0131] The specific test data of Experiment 1 are shown in Table 1.

[0132] Table 1

[0133]

[0134] According to the data comparison in Table 1, after adding the modified recycled rubber powder modified by Escherichia coli into the mortar, the prepared mortar has high waterproof and moisture-proof properties and high compressive strength. Moreover, the dosage of the rubber powder in the embodiment is as high as about 30%, which can effectively consume waste rubber materials, reduce the pollution of waste rubber to the environment, and prepare high-quality mortar while being more environmentally friendly.

[0135] From the comparative data, it can be seen that after replacing Escherichia coli with other microorganisms or replacing sodium silicate with other silicon sources, the compressive strength of the sterilization product decreases. It can be seen that the combination of Escherichia coli and sodium silicate can better deposit silicon dioxide in the waste rubber powder, and the modification effect is better.

[0136] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A waterproof and moisture-proof recycled rubber mortar, characterized in that: The composition includes the following components in parts by weight: 165 parts of water; Cement 258-262 parts; Fly ash 58-62 parts; Fine aggregate 1310-1320 parts; 560-570 parts of modified recycled rubber powder; Water reducing agent 2.8-3.2 parts; The modification method of the modified regenerated rubber powder is as follows: Step 1), putting the regenerated rubber powder into an acetic acid solution with a concentration of 10-15%, soaking for 10-15 minutes, filtering and washing to obtain pretreated rubber powder; Step 2), adding Escherichia coli into the liquid culture medium, and culturing until the OD value is 2-2.2, to obtain a culture solution; Step 3), soaking the pretreated rubber powder in a culture solution for 8-12 hours, filtering out the pretreated rubber powder and soaking it in a modification solution containing a silicon source for 7-10 days, filtering, and drying to obtain modified recycled rubber powder; In step 2), the liquid culture medium includes the following components in parts by weight: Peptone 10-15 parts; 5-10 parts of yeast extract; Sodium chloride 10-15 parts; 1000 parts water; In the step 3), the modified solution includes the following components in parts by weight: Peptone 10-15 parts; 5-10 parts of yeast extract; Sodium chloride 10-15 parts; 30-40 parts of starch; 1000 parts water; Liquid sodium silicate 1000-1100 parts.

2. The waterproof and moisture-proof recycled rubber mortar according to claim 1, characterized in that: The concentration of the liquid sodium silicate is 40%.

3. The waterproof and moisture-proof recycled rubber mortar according to claim 1, characterized in that: In the step 1), the regenerated rubber powder is soaked in the acetic acid solution and then cleaned with an ethanol solution having a concentration of 10-20%.

4. The waterproof and moisture-proof recycled rubber mortar according to claim 1, characterized in that: In the step 1), the specification of the recycled rubber powder is 40-60 mesh.

5. The waterproof and moisture-proof recycled rubber mortar according to claim 1, characterized in that: In the step 3), the filtered pre-treated rubber powder is put into a filter bag, and the filter bag containing the pre-treated rubber powder is completely sunk into the modified liquid by a weight.

6. A method for preparing the waterproof and moisture-proof recycled rubber mortar according to any one of claims 1 to 5, characterized in that: The following steps are involved: Step 1), take part of the water, add cement, fly ash, modified recycled rubber powder, water reducing agent, mix well, and obtain a premix; Step 2), add fine aggregate into the premix, mix well, then add remaining water, mix well, and obtain waterproof and moisture-proof recycled rubber mortar.