Preparation of biomass-based epoxy resin with biodegradable and flame-retardant properties

By introducing biomass Schiff base intermediates into epoxy resin, using C=N bonds and benzene ring structures, the problems of epoxy resin's flammability and non-reprocessability are solved, and high flame retardancy and degradability are achieved. properties, enhances its mechanical properties and reduces environmental pollution.

CN116478065BActive Publication Date: 2024-10-15SOUTHWEAT UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310248990.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-15
Publication Date
2024-10-15
Estimated Expiration
2043-03-15

AI Technical Summary

Technical Problem

The flammability of epoxy resin limits its wider application, and irreversible covalent cross-linking makes it impossible to reprocess, resulting in environmental pollution and safety threats.

Method used

By using biomass vanillin and tyramine to synthesize Schiff base intermediates, and reacting with epichlorohydrin, an epoxy resin containing C=N bonds is formed, which combines dynamic covalent bonds and benzene ring rigid groups to improve resistance. flammable and degradable properties.

Benefits of technology

It significantly improves the flame retardant and mechanical properties of epoxy resin, while achieving the degradability of epoxy resin and reducing environmental pollution during combustion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116478065B_ABST
    Figure CN116478065B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a biomass Schiff base intermediate and the application of the biomass Schiff base intermediate in epoxy resin. The biomass Schiff base intermediate is prepared by condensation reaction of bio-based vanillin and tyramine by molecular design; epichlorohydrin and the biomass Schiff base intermediate are subjected to a series of reactions to obtain an epoxy resin containing a Schiff base structure (C=N), which is then mixed with a certain amount of curing agent and cured at a certain temperature to obtain a biomass epoxy resin with degradable and flame retardant properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer flame retardant materials, and specifically relates to the preparation and research of a biomass epoxy resin with degradable and flame retardant properties. Background Art

[0002] As a kind of thermosetting resin, epoxy resin has many excellent properties (excellent chemical resistance, electrical insulation and mechanical properties, etc.), and is widely used in coatings, adhesives and composite materials. However, since epoxy resins often contain a large amount of carbon and hydrogen elements, they are extremely flammable and can easily cause fires. When a fire occurs, a large amount of corrosive and toxic gases and thick smoke will be released, polluting people's living environment and threatening the safety of life and property, thus limiting the wider promotion and use of such materials. Therefore, improving the flame retardancy of epoxy resins through flame retardant modification has received widespread attention.

[0003] Nitrogen flame retardants are one of the hot research directions of halogen-free flame retardants. They mainly refer to polymer material systems containing compounds such as dicyandiamide, guanidine compounds, cyanuric acid, thiourea and its derivatives, melamine and its salts. Their main advantages are halogen-free, low smoke, low toxicity and environmentally friendly. When heated, nitrogen flame retardant systems will decompose to produce a series of non-flammable gases (such as N2, NH3, NO2, CO2, H2O), which can dilute the oxygen concentration in the air and reduce the concentration of combustible gases released by polymer decomposition. The nitrogen oxides produced can capture active free radicals, thereby inhibiting or interrupting the chain reaction of polymer combustion.

[0004] Due to irreversible covalent crosslinking, thermosetting epoxy resins cannot be reprocessed after molding. Researchers have endowed thermosetting epoxy resins with degradable properties by introducing dynamic covalent bonds such as ester bonds, Diels-Alder (DA) reactions, disulfide bonds, and Schiff bases. Among them, the Schiff base containing a C=N bond structure has the performance of breaking bonds at high temperatures and crosslinking at low temperatures, and has good carbon-forming properties, and can also give polymer compounds certain flame retardant properties. The present invention uses two bio-based materials, vanillin and tyramine, as raw materials to synthesize Schiff base compounds, and applies them to epoxy resins, which can give epoxy resins flame retardant properties and degradable properties. Summary of the invention

[0005] The invention discloses a biomass Schiff base intermediate, a preparation method thereof and application of the biomass Schiff base intermediate in epoxy resin, so as to achieve the effects of improving flame retardancy and reducing environmental pollution.

[0006] The purpose of the present invention is to provide a biomass Schiff base intermediate, which has flame retardant properties and can be widely used in the field of polymer material preparation.

[0007] Another object of the present invention is to provide a method for preparing the above intermediate.

[0008] Another object of the present invention is to provide the use of the intermediate in epoxy resin, wherein the epoxy resin containing the intermediate has good flame retardant properties and mechanical properties.

[0009] The biomass Schiff base intermediate provided by the present invention has a monomer structure as shown below:

[0010]

[0011] The biomass-based epoxy resin with biodegradable and flame-retardant properties provided by the present invention has a structural formula as shown below:

[0012]

[0013] A method for preparing a biomass Schiff base intermediate, characterized by comprising:

[0014] S1. reacting vanillin with tyramine in a solvent to prepare a biomass Schiff base intermediate;

[0015] The method for preparing the intermediate according to step S1 is characterized in that vanillin and tyramine are dissolved in a solvent, the reaction temperature is 0-120° C., the reaction time is 4-6 hours, and finally the biomass Schiff base intermediate is obtained through purification.

[0016] The method for preparing the intermediate according to step S1 is characterized in that the solvent used in the reaction can be anhydrous ethanol, ether, ethyl acetate, etc. (all solvents that can obtain the intermediate are acceptable).

[0017] It should be understood that the amount of the solvent can be appropriately adjusted according to the solubility of the vanillin and tyramine, respectively, in combination with the prior art.

[0018] The purification treatment described in steps S1 and S2 may be filtration, washing, drying, etc. Any purification operation that can obtain the corresponding product falls within the protection scope of the present invention.

[0019] Application of a biomass Schiff base intermediate in epoxy resin.

[0020] Furthermore, the preparation method of the epoxy resin comprises the following steps:

[0021] A1. The biomass Schiff base (C=N) intermediate is reacted with epichlorohydrin to obtain an epoxy resin containing a Schiff base structure (C=N);

[0022] A2. Mix the epoxy resin containing Schiff base structure (C=N) with the curing agent in a certain proportion and cure it under certain temperature control conditions to obtain a biomass-based epoxy resin with biodegradable and flame-retardant properties.

[0023] The preparation method of the epoxy resin according to step A1 is characterized in that, under an inert atmosphere, the Schiff base compound reacts with epichlorohydrin under the action of a catalyst, the reaction temperature is 50-100° C., and the reaction time is 3-5 hours; then a certain concentration of sodium hydroxide solution is added, the reaction temperature is 30-60° C., the reaction time is 3-5 hours, and finally, the epoxy resin containing C=N is obtained after purification.

[0024] The curing method according to step A2 is characterized in that the curing agent is 4,4-diaminodiphenylmethane, the curing time is 0.5~0.8h (the curing agent can be completely dissolved), and the curing temperature is calculated according to the programmed temperature rise mode = 80℃ / 2h+110℃ / 2h+140℃ / 2h.

[0025] According to the solidification treatment described in step A2, any solidification operation that can obtain the corresponding solid belongs to the protection scope of the present invention.

[0026] The biomass Schiff base intermediate of the present invention contains C=N in its molecular structure, which increases the speed of releasing non-combustible gas when the epoxy resin material burns, so that the epoxy resin exhibits higher flame retardant performance when burning; at the same time, C=N in the molecular structure is a dynamic bond, which gives the epoxy resin a certain degradable property.

[0027] The biomass epoxy resin with degradable and flame-retardant properties of the present invention forms intermolecular hydrogen bonds during the curing process and contains rigid group benzene rings in the molecules, so that the epoxy resin has good mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The nuclear magnetic resonance hydrogen spectrum of the biomass Schiff base intermediate obtained by the present invention;

[0029] Figure 2 The infrared spectra of the raw materials and products used in the present invention;

[0030] Figure 3 The nuclear magnetic resonance hydrogen spectrum of the biomass-based epoxy resin having degradable and flame-retardant properties of the present invention;

[0031] Figure 4 The stress-strain curves of the epoxy resin containing Schiff base structure (C=N) and pure epoxy resin of the present invention;

[0032] Figure 5This is a bending performance diagram of the epoxy resin containing a Schiff base structure (C=N) of the present invention and a pure epoxy resin;

[0033] Figure 6 is the degradation performance curve of the epoxy resin containing Schiff base structure (C=N) in hydrochloric acid (c=0.1 mol / L);

[0034] Figure 7 This is the degradation performance curve of the epoxy resin containing a Schiff base structure (C=N) in hydrochloric acid (c=1 mol / L). Implementation

[0035] In order to facilitate the understanding of those skilled in the art, the present invention is further described below in conjunction with the examples and drawings, and the contents mentioned in the examples are not limitations of the present invention. It should be noted in advance that the following examples were completed in the laboratory, and those skilled in the art should understand that the amounts of the components given in the examples only represent the ratio relationship between the components, rather than specific limitations. Example

[0036] A method for preparing a biomass Schiff base intermediate comprises the following steps:

[0037] Vanillin (15.2 g, 0.1 mol) and tyramine (13.7 g, 0.1 mol) were dissolved in 150 mL of anhydrous ethanol and reacted at 60 °C for 4 h. After filtration and drying, a solid was obtained, which was a biomass Schiff base intermediate (NMR hydrogen spectrum as Figure 1 As shown, the infrared spectrum is Figure 2 shown);

[0038] Application examples:

[0039] S1. The above-mentioned biomass Schiff base intermediate (27.1 g, 0.1 mol) was dissolved in 80 mL of epichlorohydrin, tetrabutylammonium bromide (3.2 g, 0.01 mol) was added, and the mixture was condensed and refluxed at 80°C with stirring for 4 h to obtain solution I;

[0040] S2. Sodium hydroxide (16 g, 0.4 mol) was dissolved in 24 mL of water to obtain a 40 wt% sodium hydroxide solution (Solution II), Solution I was cooled to 50°C, Solution II was added dropwise and reacted for 4 h, and Solution III was obtained after filtration; Solution III was diluted nearly to one-fold with dichloromethane, washed and separated three times with distilled water, dichloromethane was removed by rotary evaporation, and epichlorohydrin was removed by vacuum distillation to obtain a biomass-based epoxy resin thick liquid with biodegradable and flame-retardant properties (wherein, the nuclear magnetic hydrogen spectrum is as follows Figure 3 As shown, the infrared spectrum is Figure 2 as shown).

[0041] S3. Weigh 80 parts of epoxy resin containing Schiff base structure and 20 parts of curing agent, stir them with vacuum magnetic stirring at 80℃ for 30 minutes, then pour them into a mold, and carry out curing reaction through a programmed temperature rise process of 80℃ / 2h+110℃ / 2h+140℃ / 2h. The obtained solid is a biomass-based epoxy resin with biodegradable and flame-retardant properties.

[0042] Comparative Example:

[0043] Weigh 80 parts of epoxy resin (bisphenol A type) and 20 parts of curing agent, stir them magnetically under vacuum at 80°C for 30 minutes, then pour them into a mold, and carry out a curing reaction through a programmed temperature rise process of 80°C / 2h+110°C / 2h+140°C / 2h to obtain a solid, which is a pure epoxy resin thermosetting material.

[0044] Experimental results

[0045] In order to verify the fireproof effect of the biomass epoxy resin material with degradable and flame retardant properties of the present invention, an experiment was conducted. The data are shown in the following table:

[0046] product LOI (%) UL-94 Comparative Example 24.7 NR Application Examples 28.4 V-1

[0047] It can be seen from the above table that compared with the comparative example, the LOI and flame retardancy level of the application example are significantly improved, indicating that the epoxy resin prepared from the biomass Schiff base intermediate of the present invention has good flame retardancy.

[0048] In order to verify the mechanical properties of the biomass epoxy resin material with degradable and flame retardant properties of the present invention, an experiment was conducted. The data are shown in the following table:

[0049] product Tensile strength (MPa) Elongation at break (%) Bending strength (MPa) Comparative Example 72 4.9 60 Application Examples 110 5.0 70

[0050] It can be seen from the above table that compared with the comparative example, the tensile strength and flexural strength of the application example are improved, indicating that the epoxy resin prepared from the biomass Schiff base intermediate of the present invention has good mechanical properties.

[0051] In order to verify the degradation performance of the biomass-based epoxy resin material with degradable and flame-retardant properties of the present invention, an experiment was conducted. The data are shown in the following table:

[0052] HCl:THF 1:9 2:8 3:7 4:6 5:5 Degradation rate (%) 2 25 24 39 31

[0053] Note: c(HCl)=0.1mol / L, t=12h

[0054] HCl:THF 1:9 2:8 3:7 4:6 5:5 Degradation rate (%) 1 5 4 12 10

[0055] Note: c(HCl)=1mol / L, t=12h

[0056] It can be seen from the above table that when the ratio of 0.1 mol / L HCl to THF is 4:6, a degradation rate of 39% can be achieved after 12 hours, indicating that the epoxy resin prepared from the biomass Schiff base intermediate of the present invention has good degradation performance.

[0057] In summary, the biomass Schiff base intermediate of the present invention improves the flame retardancy and degradation properties of epoxy resin and enhances its mechanical properties.

[0058] The above is only a preferred embodiment of the present invention. It should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art shall not deviate from the spirit and scope of the present invention, and shall be within the scope of protection of the claims attached to the present invention.

Claims

1. A biomass-based epoxy resin with biodegradable and flame-retardant properties, the structural formula of which is as follows: 。 2. A method for preparing the biomass-based epoxy resin having degradable and flame-retardant properties as claimed in claim 1, It is characterized in that The method comprises the following steps: reacting a biomass Schiff base intermediate with epichlorohydrin to prepare an epoxy resin containing a Schiff base structure; The chemical structural formula of the biomass Schiff base intermediate is as follows: 。 3. The method for preparing the biomass-based epoxy resin having degradable and flame-retardant properties according to claim 2, It is characterized in that Under an inert atmosphere, biomass Schiff base intermediates react with epichlorohydrin in the presence of a catalyst, the reaction temperature is 50-100°C, and the reaction time is 3-5h; subsequently, a certain concentration of sodium hydroxide solution is added, the reaction temperature is 30-60°C, and the reaction time is 3-5h. Finally, after purification, an epoxy resin containing a Schiff base structure is obtained.

4. The method for preparing the biomass-based epoxy resin having degradable and flame-retardant properties according to claim 2, It is characterized in that The method for preparing the biomass Schiff base intermediate comprises reacting vanillin with tyramine in a solvent to prepare the biomass Schiff base intermediate.

5. The method for preparing the biomass-based epoxy resin having degradable and flame-retardant properties according to claim 4, It is characterized in that Vanillin and tyramine are dissolved in a solvent, the reaction temperature is 0-120° C., the reaction time is 4-6 hours, and finally a biomass Schiff base intermediate is obtained through purification.

6. The method for preparing the biomass-based epoxy resin having degradable and flame-retardant properties according to claim 4, It is characterized in that The solvents used in the reaction are anhydrous ethanol, ether and ethyl acetate.