Optical polyester release film and preparation method thereof
By adding modified nanosilicon dioxide and nucleation crystallizer to the polyester film and introducing modified nanosilicon dioxide ions into the release agent, the high haze and low light transmittance of the polyester release film are solved. Problem, achieving higher light transmittance and lower haze values, suitable for optical grade products.
Patent Information
- Application Number
- CN202310455814.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-25
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-04-25
AI Technical Summary
The existing polyester release films have problems with high haze value and low light transmittance in optical applications, which affects the quality of polarizers and other products.
By adding modified nanosilicon dioxide masterbatches and nucleation crystallizers to the polyester film, the polyester release film is improved by combining the mesh Si-O-Si structure of modified nanosilicon dioxide ions in the release agent. The light transmittance and reduce haze value, while the nanosilica is modified with a silane coupling agent to enhance its mechanical and optical properties.
It significantly improves the light transmittance and surface flatness of the polyester release film, reduces the haze value, enhances the toughness and transparency of the release film, and is suitable for optical-grade products.
Smart Images

Figure BDA0004199162280000091 
Figure BDA0004199162280000101
Abstract
Description
Technical Field
[0001] The present application relates to the field of release film technology, and in particular to an optical polyester release film and a preparation method thereof. Background Art
[0002] Release film is a film with a separable surface, which is composed of a substrate, a primer and a release agent. The substrate of polyester release film is mainly PET material, which has high film-forming properties, excellent mechanical properties and toughness, and is widely used in packaging, printing, reflective materials, sanitary paper, adhesive products and other industries.
[0003] Optical release film is formed by coating a special release agent on an optical-grade PET film. Optical release film is a special series of release film developed for applications such as optical adhesive coating, optical tape processing, and polarizing plates. Due to usage requirements, the optical release film needs to have good optical properties, a smooth surface, and no rainbow patterns.
[0004] Existing polyester release film products in the prior art generally have the disadvantages of high haze value and low transmittance, which makes it difficult to find defects on the surface of products such as polarizing plates, affecting the quality of flat panel displays. Therefore, there is an urgent need to improve the transmittance of optical polyester release films and reduce the haze value. Summary of the invention
[0005] In order to improve the light transmittance of an optical polyester film and reduce the haze value of the polyester film, the present application provides an optical polyester release film and a preparation method thereof.
[0006] The present application provides an optical polyester release film, which adopts the following technical solution:
[0007] An optical polyester release film and a preparation method thereof, wherein the optical polyester release film comprises a release agent layer and a modified polyester film layer from top to bottom; main raw materials of the release film comprise the following components: 240-280 parts of polyester chips, 1-3 parts of modified nano-silicon dioxide masterbatch, 1-2 parts of optical opening masterbatch, and 1-2 parts of nucleating crystallization agent masterbatch; the release agent raw materials comprise the following components: 3-10 parts of polyvinyl alcohol, 0.5-2.5 parts of modified nano-silicon dioxide, 0.3-0.7 parts of inhibitor, 0.6-2 parts of peeling regulator, 0.6-2 parts of silane coupling agent, and 50-80 parts of deionized water.
[0008] By adopting the above technical scheme, modified nano-silica masterbatch is added to the base polyester film, which can increase the light transmittance of the polyester release film. However, since the surface where the nano-silica is combined with the polyester film will produce light refraction or scattering, the haze of the polyester release film will increase. Therefore, by adding nucleating crystallization agent masterbatch to the polyester release film, the number of crystal nuclei can be increased, the spherulites can be refined and uniform, the degree of light scattering is weakened, the haze value is reduced, and the transparency of the material is increased, so the surface transmittance can be further increased and the haze value can be reduced; modified nano-silica ions are added to the release agent, a network Si-O-Si structure is introduced, the toughness of the release agent after film formation is enhanced, the residual rate of the release agent coating after peeling is reduced, and the transparency, brightness and whiteness of the release film are improved, while making the surface of the release film smooth and flat.
[0009] Preferably, the raw materials of the modified nano-silicon dioxide mainly include: 2-3 parts of nano-silicon dioxide, 24-30 parts of anhydrous ethanol, 10-15 parts of silane coupling agent, and 20-30 parts of deionized water.
[0010] By adopting the above technical scheme, nano-silica is modified by using a silane coupling agent, and hydrophobic groups are grafted on the surface of nano-silica to reduce the number of hydroxyl groups on its surface, so that it changes from hydrophilic to hydrophobic, thereby improving the compatibility between nano-silica and organic matter, reducing the agglomeration of nano-silica, thereby better exerting the mechanical properties and optical properties of nano-silica and improving the light transmittance of the polyester release film.
[0011] Preferably, the nucleating crystallization agent mainly includes calcium stearate and DBS nucleating agent, and the weight ratio is (0.4-0.8):1.
[0012] By adopting the above technical solution, the use of nucleating crystallization agent can increase the light transmittance of polyester release film and reduce the haze value. The addition of DBS nucleating agent can improve the crystallinity of polyester release film, make it uniform and fine, greatly improve the optical and mechanical properties, and improve the haze of polyester release film; and the addition of stearic acid can increase the light transmittance of polyester release film. Therefore, by compounding the two, the light transmittance of polyester release film can be further improved and the haze value can be reduced.
[0013] Preferably, the optical opening masterbatch mainly comprises barium sulfate.
[0014] By adopting the above technical solution and using barium sulfate as the optical opening masterbatch, it can effectively play a connecting role; and has little effect on the transmittance and haze of the polyester release film.
[0015] The present application also provides a method for preparing an optical polyester release film, which adopts the following technical solution:
[0016] The release agent is 80-100g / m 2 The amount of the coating agent is applied on the surface of the modified polyester film, followed by drying and cooling to room temperature to obtain an optical polyester release film.
[0017] By adopting the above technical solution, the release agent can improve the light transmittance of the release film and reduce the haze. At the same time, the modified polyester film also has a high light transmittance, and when the two are used in combination, the light transmittance is further enhanced.
[0018] Preferably, the method for preparing the modified polyester film comprises the following steps:
[0019] S1. 50-60 parts of polyester chips and 0.5-1.5 parts of modified nano-silica are mixed and ground, 0.3-0.5 parts of a dispersant are added, and granulated by twin-screw extrusion to obtain a modified nano-silica masterbatch;
[0020] S2. 50-60 parts of polyester chips and 1-1.8 parts of barium sulfate are mixed and ground, 0.3-0.5 parts of a dispersant are added, and granulated by twin-screw extrusion to obtain an optical opening masterbatch;
[0021] S3. 50-60 parts of polyester chips and 0.8-2 parts of nucleating crystallizing agent are mixed and ground, 0.3-0.5 parts of dispersant are added, and granulated by twin-screw extrusion to obtain a nucleating crystallizing agent masterbatch;
[0022] S4. Mix 1-3 parts of modified nano-silica masterbatch, 1-2 parts of optical opening masterbatch, 1-2 parts of nucleating crystallization agent masterbatch and 90-100 parts of polyester chips, feed them into an extruder, and obtain a modified polyester film by melt extrusion and biaxial stretching.
[0023] By adopting the above technical solution, the polyester chips are modified by using modified nano-silica masterbatch, optical opening masterbatch and nucleating crystallization agent masterbatch, so that the obtained polyester release film has stronger transmittance and lower haze value.
[0024] Preferably, the method for preparing the release agent comprises the following steps:
[0025] 3-10 parts of polyvinyl alcohol and 0.6-2 parts of silane coupling agent are added to 50-80 parts of deionized water and stirred evenly, and then 0.5-2.5 parts of modified nano-silicon dioxide, 0.3-0.7 parts of polymerization inhibitor and 0.6-2 parts of peeling regulator are added and stirred evenly to obtain a release agent.
[0026] By adopting the above technical scheme, modified nano-silica ions are added to the release agent, a network Si-O-Si structure is introduced, the toughness of the release agent after film formation is enhanced, the residual rate of the release agent coating after peeling is reduced, and the opacity, brightness and whiteness of the release film are improved, while making the surface of the release film smooth and flat.
[0027] Preferably, the preparation method of the modified nano-silicon dioxide comprises the following steps:
[0028] S1. Add 2-3 parts of nano-silica to 24-30 parts of anhydrous ethanol and mix, stir until uniformly dispersed to obtain a dispersion of nano-silica; add 10-15 parts of a silane coupling agent to 20-30 parts of deionized water and stir for 1-2h to obtain an aqueous solution of a silane coupling agent;
[0029] S2. Add the nano-silica dispersion to the aqueous solution of the silane coupling agent, stir evenly, and reflux at 60-80°C for 2-4 hours; after the reaction, wash, filter, dry and grind the obtained product to obtain modified nano-silica powder.
[0030] By adopting the above technical scheme, nano-silica is modified by using a silane coupling agent, and hydrophobic groups are grafted on the surface of nano-silica to reduce the number of hydroxyl groups on its surface, thereby improving the compatibility between nano-silica and organic matter and reducing the agglomeration of nano-silica, thereby better exerting the mechanical and optical properties of nano-silica and improving the light transmittance of the polyester release film.
[0031] In summary, the present application includes at least one of the following beneficial technical effects:
[0032] 1. By adopting the above technical solution, modified nano-silica masterbatch is added to the polyester film as the substrate, which can increase the light transmittance of the polyester release film. However, since the surface where the nano-silica is combined with the polyester film will produce light refraction or scattering, the haze of the polyester release film will increase. Therefore, by adding nucleating crystallization agent masterbatch to the polyester release film, the number of crystal nuclei can be increased, the spherulites can be refined and uniform, the degree of light scattering is weakened, the haze value is reduced, and the transparency of the material is increased, so the light transmittance of the surface can be further increased, and the haze value can be reduced; modified nano-silica ions are added to the release agent, and a network Si-O-Si structure is introduced, which enhances the toughness of the release agent after film formation, reduces the residual rate of the release agent coating after peeling, and improves the opacity, brightness and whiteness of the release film, while making the surface of the release film smooth and flat;
[0033] 2. By adopting the above technical solution, the nano-silicon dioxide is modified by a silane coupling agent, and the number of hydroxyl groups on the surface of the nano-silicon dioxide is reduced by grafting hydrophobic groups on the surface of the nano-silicon dioxide, so that the hydrophilicity is changed to hydrophobicity, thereby improving the compatibility between the nano-silicon dioxide and organic matter, reducing the agglomeration of the nano-silicon dioxide, thereby better exerting the mechanical properties and optical properties of the nano-silicon dioxide, and improving the light transmittance of the polyester release film;
[0034] 3. By adopting the above technical solution, the use of nucleating crystallization agent can increase the light transmittance of the polyester release film and reduce the haze value. The addition of DBS nucleating agent can improve the crystallinity of the polyester release film, make it uniform and fine, greatly improve the optical and mechanical properties, and improve the haze of the polyester release film; and the addition of stearic acid can increase the light transmittance of the polyester release film. Therefore, by compounding the two, the light transmittance of the polyester release film can be further improved and the haze value can be reduced. DETAILED DESCRIPTION
[0035] The present application is further described in detail below with reference to the embodiments.
[0036] Preparation Example
[0037] Preparation Example 1
[0038] S1. 2 g of nano-silica was added to 24 g of anhydrous ethanol and mixed, and stirred at 200 rpm for 30 min to obtain a dispersion of nano-silica; 10 g of a silane coupling agent was added to 20 g of deionized water and stirred at 300 rpm for 1 h to obtain an aqueous solution of a silane coupling agent;
[0039] S2. Add the nano-silica dispersion to the aqueous solution of the silane coupling agent, stir magnetically at 600 rpm for 30 min, and then reflux at 60°C for 2 h. After the reaction, wash and filter the obtained product with anhydrous ethanol until the filtrate is clear, dry the product at 80°C for 2 h, and then grind the dried filter cake to obtain modified nano-silica powder. The silane coupling agent used in this preparation example is KH550.
[0040] Preparation Example 2
[0041] S1. 2.5 g of nano-silica was added to 27 g of anhydrous ethanol and mixed, and stirred at 250 rpm for 40 min to obtain a dispersion of nano-silica; 12.5 g of a silane coupling agent was added to 25 g of deionized water and stirred at 350 rpm for 1.5 h to obtain an aqueous solution of a silane coupling agent;
[0042] S2. Add the nano-silica dispersion to the aqueous solution of the silane coupling agent, stir magnetically at 700 rpm for 35 min, and then reflux at 70°C for 3 h. After the reaction, wash and filter the obtained product with anhydrous ethanol until the filtrate is clear, dry the product at 90°C for 1.5 h, and then grind the dried filter cake to obtain modified nano-silica powder. The silane coupling agent used in this preparation example is KH550.
[0043] Preparation Example 3
[0044] S1. 3 g of nano-silica was added to 30 g of anhydrous ethanol and mixed, and stirred at 300 rpm for 50 min to obtain a dispersion of nano-silica; 15 g of a silane coupling agent was added to 30 g of deionized water and stirred at 400 rpm for 2 h to obtain an aqueous solution of a silane coupling agent;
[0045] S2. Add the nano-silica dispersion to the aqueous solution of the silane coupling agent, stir magnetically at 800 rpm for 40 min, and then reflux at 80°C for 4 h. After the reaction, wash and filter the obtained product with anhydrous ethanol until the filtrate is clear, dry the product at 100°C for 1 h, and then grind the dried filter cake to obtain modified nano-silica powder. The silane coupling agent used in this preparation example is KH550.
[0046] Example
[0047] Example 1
[0048] S1. 50 g of polyester chips were mixed with 0.5 g of the modified nano-silica obtained in Preparation Example 1, ground, 0.3 g of a dispersant was added, and granulated by twin-screw extrusion to obtain a modified nano-silica masterbatch;
[0049] S2. 50 g of polyester chips were mixed with 1 g of barium sulfate, ground, 0.3 g of dispersant was added, and granulated by twin-screw extrusion to obtain an optical opening masterbatch;
[0050] S3 50g polyester chips and 0.8g nucleating crystallizing agent mixed, ground, added 0.3g dispersant, twin-screw extrusion granulation, to obtain a nucleating crystallizing agent masterbatch;
[0051] S4. 1 g of modified nano-silica masterbatch, 1 g of optical opening masterbatch, 1 g of nucleating crystallization agent masterbatch and 90 g of polyester chips were mixed and fed into an extruder, melted and extruded, and the melt extruded from the die was attached to the surface of a cold drum and cooled to obtain a cast sheet. The cast sheet was stretched and shaped to obtain a modified polyester film having a thickness of 30 μm;
[0052] S5. 3 g of polyvinyl alcohol and 0.6 g of a silane coupling agent were added to 50 g of deionized water and stirred uniformly, followed by adding 0.5 g of the modified nano-silica obtained in Preparation Example 1, 0.3 g of an inhibitor, and 0.6 g of a release regulator, and stirred at 300 rpm for 1.5 h to obtain a release agent;
[0053] S6. Apply the release agent at 80g / m 2 The modified polyester film is coated with an amount of , and then dried at 100° C. for 2 h, and after cooling to room temperature, an optical polyester release film is obtained;
[0054] The dispersant used in this embodiment is hydroxymethyl cellulose; the nucleating crystallizing agents used include calcium stearate and DBS nucleating agent, with a weight ratio of 0.4:1; the silane coupling agent used is KH550; the inhibitor used is ammonium thiocyanate; and the release regulator used is methylsiloxane.
[0055] Example 2
[0056] S1. 55 g of polyester chips were mixed with 0.5 g of the modified nano-silica obtained in Preparation Example 1, ground, 0.4 g of a dispersant was added, and granulated by twin-screw extrusion to obtain a modified nano-silica masterbatch;
[0057] S2. 55g of polyester chips were mixed with 1.0g of barium sulfate, ground, 0.4g of dispersant was added, and granulated by twin-screw extrusion to obtain an optical opening masterbatch;
[0058] S3 55g of polyester chips and 0.8g of nucleating crystallizing agent were mixed and ground, 0.4g of dispersant was added, and granulated by twin-screw extrusion to obtain a nucleating crystallizing agent masterbatch;
[0059] S4. 2 g of modified nano-silica masterbatch, 1.5 g of optical opening masterbatch, 1.5 g of nucleating crystallization agent masterbatch and 95 g of polyester chips were mixed and fed into an extruder, melted and extruded, and the melt extruded from the die was attached to the surface of a cold drum and cooled to obtain a cast sheet. The cast sheet was stretched and shaped to obtain a modified polyester film having a thickness of 30 μm;
[0060] S5. 6.5 g of polyvinyl alcohol and 1.3 g of a silane coupling agent were added to 65 g of deionized water and stirred uniformly, followed by adding 0.5 g of the modified nano-silica obtained in Preparation Example 1, 0.5 g of an inhibitor, and 1.3 g of a release regulator, and stirred at 350 rpm for 2 h to obtain a release agent;
[0061] S6. Apply the release agent at 80g / m 2 The amount of the modified polyester film was coated on the surface of the modified polyester film, and then dried at 110° C. for 2.5 hours, and after cooling to room temperature, an optical polyester release film was obtained;
[0062] The dispersant used in this embodiment is hydroxymethyl cellulose; the nucleating crystallizing agents used include calcium stearate and DBS nucleating agent, with a weight ratio of 0.4:1; the silane coupling agent used is KH550; the inhibitor used is ammonium thiocyanate; and the release regulator used is methylsiloxane.
[0063] Example 3
[0064] S1. 60 g of polyester chips were mixed with 0.5 g of the modified nano-silica obtained in Preparation Example 1, ground, 0.5 g of a dispersant was added, and granulated by twin-screw extrusion to obtain a modified nano-silica masterbatch;
[0065] S2. 60 g of polyester chips were mixed with 1 g of barium sulfate, ground, 0.5 g of dispersant was added, and granulated by twin-screw extrusion to obtain an optical opening masterbatch;
[0066] S3 60g polyester chips and 0.8g nucleating crystallizing agent mixed, ground, added 0.5g dispersant, by twin-screw extrusion granulation, to obtain a nucleating crystallizing agent masterbatch;
[0067] S4. 3g of modified nano-silica masterbatch, 2g of optical opening masterbatch, 2g of nucleating crystallization agent masterbatch and 100g of polyester chips were mixed and fed into an extruder, melted and extruded, and the melt extruded from the die was attached to the surface of a cold drum and cooled to obtain a cast sheet. The cast sheet was stretched and shaped to obtain a modified polyester film having a thickness of 30μm;
[0068] S5. 10 g of polyvinyl alcohol and 2 g of silane coupling agent were added to 80 g of deionized water and stirred uniformly, followed by adding 0.5 g of the modified nano-silica obtained in Preparation Example 1, 0.7 g of an inhibitor, and 2 g of a release regulator, and stirred at 400 rpm for 2.5 h to obtain a release agent;
[0069] S6. Apply the release agent at 80g / m 2 The amount of the modified polyester film is coated on the surface of the modified polyester film, and then dried at 120° C. for 1.5 h, and after cooling to room temperature, an optical polyester release film is obtained;
[0070] The dispersant used in this embodiment is hydroxymethyl cellulose; the nucleating crystallizing agents used include calcium stearate and DBS nucleating agent, with a weight ratio of 0.4:1; the silane coupling agent used is KH550; the inhibitor used is ammonium thiocyanate; and the release regulator used is methylsiloxane.
[0071] Example 4
[0072] The difference between Example 4 and Example 1 is that the modified nano-silica used in S1 and S5 in Example 4 comes from Preparation Example 2.
[0073] Example 5
[0074] The difference between Example 5 and Example 1 is that the modified nano-silica used in S1 and S5 in Example 5 comes from Preparation Example 3.
[0075] Example 6
[0076] The difference between Example 6 and Example 1 is that the mass of the modified nano-silicon dioxide used in S1 in Example 6 is 1 g.
[0077] Example 7
[0078] The difference between Example 7 and Example 1 is that the mass of the modified nano-silicon dioxide used in S1 in Example 7 is 1.5 g.
[0079] Example 8
[0080] The difference between Example 8 and Example 1 is that the mass of the modified nano-silicon dioxide used in S5 in Example 8 is 1.5 g.
[0081] Example 9
[0082] The difference between Example 9 and Example 1 is that the mass of the modified nano-silicon dioxide used in S5 in Example 9 is 2.5 g.
[0083] Example 10
[0084] The difference between Example 10 and Example 1 is that the mass of barium sulfate used in Example 10 is 1.4 g.
[0085] Embodiment 11
[0086] The difference between Example 11 and Example 1 is that the mass of barium sulfate used in Example 11 is 1.8 g.
[0087] Example 12
[0088] The difference between Example 12 and Example 1 is that the mass of the nucleating crystallization agent used in Example 12 is 1.4 g.
[0089] Embodiment 13
[0090] The difference between Example 13 and Example 1 is that the mass of the nucleating crystallization agent used in Example 13 is 1.8 g.
[0091] Embodiment 14
[0092] The difference between Example 14 and Example 1 is that the weight ratio of the nucleating crystallizing agent calcium stearate and the DBS nucleating agent used in Example 14 is 0.6:1.
[0093] Embodiment 15
[0094] The difference between Example 15 and Example 1 is that the weight ratio of the nucleating crystallizing agent calcium stearate and the DBS nucleating agent used in Example 15 is 0.8:1.
[0095] Example 16
[0096] The difference between Example 16 and Example 1 is that the coating amount of the release agent used in Example 16 is 90 g / m 2 .
[0097] Embodiment 17
[0098] The difference between Example 17 and Example 1 is that the coating amount of the release agent used in Example 17 is 100 g / m 2 .
[0099] Comparative Example
[0100] Comparative Example 1
[0101] The difference between Comparative Example 1 and Example 1 is that the nano-silicon dioxide used in S1 and S5 in Comparative Example 4 is unmodified common nano-silicon dioxide.
[0102] Comparative Example 2
[0103] The difference between Comparative Example 2 and Example 1 is that the mass of the modified nano-silicon dioxide used in S1 in Comparative Example 2 is 0.1 g.
[0104] Comparative Example 3
[0105] The difference between Comparative Example 3 and Example 1 is that the mass of the modified nano-silicon dioxide used in S1 in Comparative Example 3 is 2.0 g.
[0106] Comparative Example 4
[0107] The difference between Comparative Example 4 and Example 1 is that the mass of the modified nano-silicon dioxide used in S5 in Comparative Example 4 is 0.1 g.
[0108] Comparative Example 5
[0109] The difference between Comparative Example 5 and Example 1 is that the mass of the modified nano-silicon dioxide used in S5 in Comparative Example 5 is 3.0 g.
[0110] Comparative Example 6
[0111] The difference between Comparative Example 6 and Example 1 is that the mass of barium sulfate used in Comparative Example 6 is 0.6 g.
[0112] Comparative Example 7
[0113] The difference between Comparative Example 7 and Example 1 is that the mass of barium sulfate used in Comparative Example 7 is 2.2 g.
[0114] Comparative Example 8
[0115] The difference between Comparative Example 8 and Example 1 is that the mass of the nucleating crystallization agent used in Comparative Example 8 is 0.2 g.
[0116] Comparative Example 9
[0117] The difference between Comparative Example 9 and Example 1 is that the mass of the nucleating crystallization agent used in Comparative Example 9 is 2.6 g.
[0118] Comparative Example 10
[0119] The difference between Comparative Example 10 and Example 1 is that the weight ratio of the nucleating crystallization agent calcium stearate and the DBS nucleating agent used in Comparative Example 10 is 0.2:1.
[0120] Comparative Example 11
[0121] The difference between Comparative Example 11 and Example 1 is that the weight ratio of the nucleating crystallizing agent calcium stearate and the DBS nucleating agent used in Comparative Example 11 is 1:1.
[0122] Comparative Example 12
[0123] The difference between Comparative Example 12 and Example 1 is that the coating amount of the release agent used in Comparative Example 12 is 60 g / m 2 .
[0124] Comparative Example 13
[0125] The difference between Comparative Example 13 and Example 1 is that the coating amount of the release agent used in Comparative Example 13 is 120 g / m 2 .
[0126] Performance testing
[0127] 1. The light transmittance and haze of the optical polyester release films obtained in Examples 1-17 and Comparative Examples 1-13 were tested using GB / T 2410-2008 “Determination of light transmittance and haze of transparent plastics”. The results are shown in Table 1.
[0128] The specific test results are as follows:
[0129] Table 1 Performance test results
[0130]
[0131]
[0132]
[0133] It can be seen from the data in Table 1 that the optical polyester release film provided in the present application has a transmittance of up to 91.5-92.8% and a haze value of 1.4-2.4%, indicating that the polyester release film obtained in the present application has a high transmittance and a low haze value, and the surface of the release film is smooth and has no rainbow patterns, and is suitable for optical-grade products.
[0134] It can be seen from the test results of Examples 1-3 that the process parameters for preparing optical polyester release films provided in the present application are all conducive to obtaining release films with higher transmittance and lower haze, and that changes within the parameter range have little impact on changes in the transmittance and haze values of the release films.
[0135] It can be seen from the test results of Examples 1, 4, 5 and Comparative Example 1 that the process parameters for preparing modified nano-silica provided in the present application are all beneficial to improving the transmittance of the release film and reducing the haze, and when changing within the parameter range, the effect on the changes in the transmittance and haze values of the release film is relatively low; however, when unmodified nano-silica is used, the transmittance of the release film is significantly reduced, the haze value is significantly increased, and slight ripples appear on the surface.
[0136] It can be seen from the test results of Examples 1, 6, 7 and Comparative Examples 2, 3 that when the mass of the modified nano-silicon dioxide used in S1 of the present application increases, the transmittance of the obtained polyester release film gradually increases, and the haze value also gradually increases; but when the mass of the modified nano-silicon dioxide is greater than 1.5g, the haze value of the obtained polyester release film becomes significantly larger; when the mass of the modified nano-silicon dioxide is less than 0.5g, the transmittance of the obtained polyester release film is significantly smaller, and the haze value is high.
[0137] It can be seen from the test results of Examples 1, 8, 9 and Comparative Examples 4, 5 that when the mass of the modified nano-silicon dioxide used in S5 of the present application increases, the transmittance of the obtained polyester release film gradually increases, and the haze value also gradually increases; but when the mass of the modified nano-silicon dioxide is greater than 2.5g, the haze value of the obtained polyester release film becomes significantly larger; when the mass of the modified nano-silicon dioxide is less than 0.5g, the transmittance of the obtained polyester release film is significantly smaller, and the haze value is high.
[0138] It can be seen from the test results of Examples 1, 10, 11 and Comparative Examples 6 and 7 that when the mass of barium sulfate for preparing the polyester release film provided in the present application increases, the light transmittance and haze of the polyester film are less affected, the light transmittance of the polyester film decreases slightly, and the haze value also decreases slightly; when the mass of barium sulfate reaches 1.8 g, the haze value no longer decreases.
[0139] It can be seen from the test results of Examples 1, 12, 13 and Comparative Examples 8, 9 that when the mass of the nucleating crystallization agent for preparing the polyester release film provided in the present application increases, the transmittance of the obtained polyester film gradually increases and the haze value also slightly decreases; but when the mass of the nucleating crystallization agent is greater than 2g, the transmittance of the obtained polyester film becomes smaller and the haze value becomes larger.
[0140] It can be seen from the test results of Examples 1, 14, 15 and Comparative Examples 10 and 11 that when the weight ratio of the nucleating crystallizing agent calcium stearate and the DBS nucleating agent for preparing the polyester release film provided in the present application varies within the range of (0.4-0.8): 1, it is beneficial to improve the transmittance of the polyester release film and reduce the haze value; but when it is lower than or higher than this range, the transmittance of the polyester release film will decrease and the haze value will increase.
[0141] It can be seen from the test results of Examples 1, 16, 17 and Comparative Examples 12 and 13 that when the coating amount of the release agent for preparing the polyester release film provided by the present application increases, the light transmittance of the obtained polyester film gradually increases and the haze value also decreases slightly; however, when the amount is greater than 100 g / m 2 When the light transmittance of the obtained polyester film becomes smaller, the haze value becomes larger.
[0142] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. An optical polyester release film, characterized in that: The optical polyester release film comprises a release agent layer and a modified polyester film layer from top to bottom; the raw materials for preparing the release agent comprise the following components: 3-10 parts of polyvinyl alcohol, 0.5-2.5 parts of modified nano-silicon dioxide, 0.3-0.7 parts of polymerization inhibitor, 0.6-2 parts of peeling regulator, 0.6-2 parts of silane coupling agent, and 50-80 parts of deionized water; The preparation method of the modified polyester film comprises the following steps: S1. 50-60 parts of polyester chips and 0.5-1.5 parts of modified nano-silica are mixed and ground, 0.3-0.5 parts of a dispersant are added, and granulated by twin-screw extrusion to obtain a modified nano-silica masterbatch; S2. 50-60 parts of polyester chips and 1-1.8 parts of barium sulfate are mixed and ground, 0.3-0.5 parts of a dispersant are added, and granulated by twin-screw extrusion to obtain an optical opening masterbatch; S3. 50-60 parts of polyester chips and 0.8-2 parts of nucleating crystallizing agent are mixed and ground, 0.3-0.5 parts of dispersant are added, and granulated by twin-screw extrusion to obtain a nucleating crystallizing agent masterbatch; S4. 1-3 parts of modified nano-silica masterbatch, 1-2 parts of optical opening masterbatch, 1-2 parts of nucleating crystallization agent masterbatch and 90-100 parts of polyester chips are mixed and fed into an extruder, and a modified polyester film is obtained by melt extrusion and biaxial stretching; The raw materials for preparing the modified nano-silicon dioxide include: 2-3 parts of nano-silicon dioxide, 24-30 parts of anhydrous ethanol, 10-15 parts of silane coupling agent, and 20-30 parts of deionized water; The nucleating crystallizing agent mainly includes calcium stearate and DBS nucleating agent, and the weight ratio is (0.4-0.8):
1.
2. A method for preparing the optical polyester release film according to claim 1, characterized in that: The following steps are involved: The release agent is 80-100g / m 2 The amount of the coating agent is applied on the surface of the modified polyester film, followed by drying and cooling to room temperature to obtain an optical polyester release film.
3. The method for preparing an optical polyester release film according to claim 2, characterized in that: The preparation method of the release agent comprises the following steps: 3-10 parts of polyvinyl alcohol and 0.6-2 parts of silane coupling agent are added to 50-80 parts of deionized water and stirred evenly, and then 0.5-2.5 parts of modified nano-silicon dioxide, 0.3-0.7 parts of polymerization inhibitor and 0.6-2 parts of peeling regulator are added and stirred evenly to obtain a release agent.
4. The method for preparing an optical polyester release film according to claim 2, characterized in that: The preparation method of the modified nano silicon dioxide comprises the following steps: S1. Add 2-3 parts of nano-silica to 24-30 parts of anhydrous ethanol and mix, stir until uniformly dispersed to obtain a dispersion of nano-silica; add 10-15 parts of a silane coupling agent to 20-30 parts of deionized water and stir for 1-2h to obtain an aqueous solution of a silane coupling agent; S2. Add the nano-silica dispersion to the aqueous solution of the silane coupling agent, stir evenly, and reflux at 60-80°C for 2-4 hours; after the reaction, wash, filter, dry and grind the obtained product to obtain modified nano-silica powder.