Cyclic olefin resin composition and molded article

By adding a specific amount of polyglycerol and fatty acid ester compound to the cyclic olefin resin composition, the cracks and pollution problems of the cyclic olefin-based copolymer in high temperature and high humidity environment are solved, and high humidity resistance and low humidity resistance are achieved Internal haze, suitable for applications such as optical lenses.

CN116507650BActive Publication Date: 2024-11-12MITSUI CHEMICALS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280007708.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-02-08
Filing Date
2022-02-03
Publication Date
2024-11-12
Estimated Expiration
2042-02-03

AI Technical Summary

Technical Problem

The cyclic olefin-based copolymer is prone to fine cracks and internal haze increase in high temperature and high humidity environments, and has poor compatibility with the mold, resulting in mold contamination and reduced optical characteristics.

Method used

By adding a specific amount of polyglycerol, fatty acid ester compound and polyglycerol to the cyclic olefin resin composition, the ratio thereof is controlled to inhibit the rise of internal haze and mold contamination, and ensure high humidity and heat resistance and optical properties.

Benefits of technology

A cyclic olefin-based resin composition with low internal haze and no mold contamination in high temperature and high humidity environment is realized. It is suitable for optical applications such as optical lenses, and maintains transparency and heat resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FDA0004907077430000011
    Figure FDA0004907077430000011
  • Figure FDA0004907077430000012
    Figure FDA0004907077430000012
  • Figure FDA0004907077430000021
    Figure FDA0004907077430000021
Patent Text Reader

Abstract

The present invention provides a cyclic olefin resin composition, which comprises a cyclic olefin copolymer (A), an ester compound (B) of polyglycerol and a fatty acid, and polyglycerol (C), wherein the amount of the compound (B) is 0.05 to 3 parts by mass relative to 100 parts by mass of the cyclic olefin copolymer (A), and the amount of the polyglycerol (C) is 0.001 to 0.04 parts by mass relative to 100 parts by mass of the cyclic olefin copolymer (A).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a cyclic olefin resin composition and a molded article. Background Art

[0002] Cyclic olefin copolymers are used in optical lenses such as camera lenses, fθ lenses, and pickup lenses. Cyclic olefin copolymers used in molded products such as optical lenses are required to have high transparency, excellent dimensional stability, excellent heat resistance, and excellent moisture resistance.

[0003] As a resin composition containing such a cyclic olefin copolymer, there is an invention described in Patent Document 1, for example. Patent Document 1 discloses a cyclic olefin resin composition containing a cyclic olefin polymer (A) and a triglycerol fatty acid ester.

[0004] In addition, Patent Document 2 discloses a resin composition, characterized in that it contains a polymer containing an alicyclic structure and a polyglycerol fatty acid ester-based additive, wherein the polyglycerol fatty acid ester-based additive is formed by one or more polyglycerol fatty acid ester compounds, the hydroxyl value of the polyglycerol fatty acid ester-based additive is 320 to 700 mgKOH / g, and the content of the polyglycerol fatty acid ester-based additive is 0.2 to 2.0 parts by weight relative to 100 parts by weight of the polymer containing an alicyclic structure.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2018-172665

[0008] Patent Document 2: International Publication No. 2017 / 033968 Summary of the invention

[0009] Problems to be solved by the invention

[0010] In recent years, durability under a harsh moisture and heat resistance test such as 80°C 90%RH, as disclosed in Patent Document 1, has been required for cyclic olefin copolymers. If the cyclic olefin copolymer does not contain a hydrophilic agent such as the additive disclosed in Patent Document 2, there is a problem that fine cracks are generated in the cyclic olefin resin under high temperature and high humidity, and the internal haze increases. On the other hand, there is also a problem that the compatibility with the cyclic olefin resin may be poor depending on the type of the hydrophilic agent.

[0011] In addition, when the cyclic olefin resin composition is used to mold a molded product such as a lens, there is a problem that the inside of the mold is contaminated. In particular, if the lens surface of the mold is contaminated, there is a problem that the optical properties of the lens as a molded product are degraded.

[0012] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a cyclic olefin resin composition having low internal haze and capable of suppressing contamination of the inside of a mold due to continuous molding.

[0013] Methods for solving problems

[0014] The present inventors have conducted intensive research to solve the above-mentioned problems. As a result, they have found that the mold is contaminated by the vaporization of the hydrophilic agent, and that the unreacted alcohol contained in the hydrophilic agent as an impurity contaminates the mold. Based on the above-mentioned findings, the present inventors have conducted further research and found for the first time that a cyclic olefin copolymer resin composition having low internal haze, suppressing the increase of internal haze even under high temperature and high humidity, and suppressing the contamination of the inside of the mold even in continuous molding by including a specific amount of polyglycerol can be obtained, thereby completing the present invention.

[0015] That is, according to the present invention, there are provided the cyclic olefin resin composition and the molded article shown below.

[0016] [1] A cyclic olefin resin composition comprising:

[0017] Cyclic olefin copolymer (A),

[0018] Ester compound of polyglycerol and fatty acid (B) and

[0019] Polyglycerol (C),

[0020] The amount of the ester compound (B) is 0.05 parts by mass or more and 3 parts by mass or less relative to 100 parts by mass of the cyclic olefin copolymer (A).

[0021] The amount of the polyglycerol (C) is 0.001 parts by mass or more and 0.04 parts by mass or less based on 100 parts by mass of the cyclic olefin copolymer (A). [2]

[0023] The cyclic olefin resin composition according to the above [1],

[0024] The cyclic olefin copolymer (A) comprises a structural unit (a) and a structural unit (b).

[0025] Structural unit (a): at least one structural unit derived from an olefin represented by the following general formula (I).

[0026] Structural unit (b): at least one structural unit derived from a cyclic olefin selected from the group consisting of a repeating unit (AA) represented by the following general formula (II), a repeating unit (AB) represented by the following general formula (III), and a repeating unit (AC) represented by the following general formula (IV).

[0027] [Chemistry 1]

[0028]

[0029] In the above general formula (I), R 300 It represents a hydrogen atom or a linear or branched hydrocarbon group having 1 to 29 carbon atoms.

[0030] [Chemistry 2]

[0031]

[0032] In the above general formula (II), u is 0 or 1, v is 0 or a positive integer, and w is 0 or 1. 61 ~R 78 and R a1 and R b1 R may be the same as or different from each other and is a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms, a halogenated alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 15 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms. 75 ~R 78 They may be bonded to each other to form a single ring or multiple rings.

[0033] [Chemistry 3]

[0034]

[0035] In the above general formula (III), x and d are each independently an integer of 0 or greater than 1. y and z are each independently an integer of 0 to 2. 81 ~R 99 R may be the same as or different from each other and is a hydrogen atom, a halogen atom, an aliphatic hydrocarbon group which is an alkyl group having 1 to 20 carbon atoms or a cycloalkyl group having 3 to 15 carbon atoms, an aromatic hydrocarbon group having 6 to 20 carbon atoms, or an alkoxy group. 89 and R 90 The carbon atom bound to R 93 The carbon atom or R 91 The carbon atom to which it is bonded may be bonded directly or through an alkylene group having 1 to 3 carbon atoms. 92 With R 99 or R 95 With R 99 They may be combined with each other to form a monocyclic or polycyclic aromatic ring.

[0036] [Chemistry 4]

[0037]

[0038] In the above general formula (IV), R 100 , R 101They may be the same as or different from each other and represent a hydrogen atom or a hydrocarbon group having 1 to 5 carbon atoms. f is 1≤f≤18. [3]

[0040] The cyclic olefin resin composition according to the above [2],

[0041] The cyclic olefin polymer (A) has:

[0042] The repeating unit (AA) represented by the above general formula (II) and the structural unit (D) derived from a cyclic olefin having an aromatic ring,

[0043] The above repeating unit (AA) does not contain an aromatic ring,

[0044] The cyclic olefin having an aromatic ring includes one or more selected from the group consisting of a compound represented by the following formula (D-1), a compound represented by the following formula (D-2), and a compound represented by the following formula (D-3).

[0045] [Chemistry 5]

[0046]

[0047] In the above (D-1), n ​​and q are each independently 0, 1 or 2. 1 ~R 17 are each independently a hydrogen atom, a halogen atom other than a fluorine atom, or a hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a halogen atom other than a fluorine atom, 10 ~R 17 In addition, when q = 0, R 10 With R 11 , R 11 With R 12 , R 12 With R 13 , R 13 With R 14 , R 14 With R 15 , R 15 With R 10 They can be combined with each other to form a single ring or multiple rings. In addition, when q=1 or 2, R 10 With R 11 , R 11 With R 17 , R 17 With R 17 , R 17 With R 12 , R 12 With R 13 , R 13 With R 14 , R 14 With R15 , R 15 With R 16 , R 16 With R 16 , R 16 With R 10 They may be bonded to each other to form a monocyclic ring or polycyclic rings, and the monocyclic ring or polycyclic rings may have a double bond, and the monocyclic ring or polycyclic rings may be aromatic rings.

[0048] [Chemistry 6]

[0049]

[0050] In the above formula (D-2), n and m are each independently 0, 1 or 2, and q is 1, 2 or 3. 18 ~R 31 Each is independently a hydrogen atom, a halogen atom other than a fluorine atom, or a hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a halogen atom other than a fluorine atom. 28 With R 29 , R 29 With R 30 , R 30 With R 31 They can be combined with each other to form a single ring or multiple rings. In addition, when q = 2 or 3, R 28 With R 28 , R 28 With R 29 , R 29 With R 30 , R 30 With R 31 , R 31 With R 31 They may be bonded to each other to form a monocyclic ring or polycyclic rings, the monocyclic ring or polycyclic rings may have a double bond, and the monocyclic ring or polycyclic rings may be aromatic rings.

[0051] [Chemistry 7]

[0052]

[0053] In the above formula (D-3), q is 1, 2 or 3, R 32 ~R 39 Each is independently a hydrogen atom, a halogen atom other than a fluorine atom, or a hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a halogen atom other than a fluorine atom. 36 With R 37 , R 37 With R 38 , R 38 With R 39 They can be combined with each other to form a monocyclic or polycyclic ring. In addition, when q=2 or 3, R36 With R 36 , R 36 With R 37 , R 37 With R 38 , R 38 With R 39 , R 39 With R 39 They may be bonded to each other to form a monocyclic ring or polycyclic rings, the monocyclic ring or polycyclic rings may have a double bond, and the monocyclic ring or polycyclic rings may be aromatic rings. [4]

[0055] The cyclic olefin resin composition according to any one of [1] to [3], wherein the glass transition temperature of the cyclic olefin copolymer (A) measured by a differential scanning calorimeter is 130° C. or more and 170° C. or less. [5]

[0057] A molded article comprising the cycloolefin resin composition according to any one of [1] to [4] above. [6]

[0059] The molded article according to the above [5], which is an optical member.

[0060] Effects of the Invention

[0061] If it is the cyclic olefin resin composition of the present invention, it is possible to form a molded body having high moisture and heat resistance compared to the conventional cyclic olefin copolymer. If it is such a molded body, the internal haze is low, and the increase of the internal haze before and after the moisture and heat resistance test can be suppressed. In addition, the contamination inside the mold caused by continuous molding can be suppressed, and in particular, the contamination of the lens surface of the mold can be suppressed. Therefore, it can be mainly suitable for optical applications and lenses. DETAILED DESCRIPTION

[0062] Hereinafter, the present invention will be described based on the embodiments. In the embodiments, "A to B" indicating a numerical range means A or more and B or less unless otherwise specified.

[0063] As described above, according to the knowledge of the inventors, conventional cyclic olefin copolymers and resins have problems such as internal haze, etc., if exposed to a high temperature and high humidity environment for a long time, and on the other hand, depending on the type of hydrophilic agent, sometimes the compatibility with the cyclic olefin resin is poor. In addition, there is a problem of contamination of the inside of the mold when the cyclic olefin resin composition is used to form a molded body such as a lens.

[0064] The present inventors have conducted intensive studies to solve the above problems. As a result, they have found that a molded body obtained from a cyclic olefin resin composition containing a specific amount of polyglycerol has higher moisture and heat resistance than a molded body obtained from a conventional cyclic olefin resin composition, and can suppress contamination of the inside of a mold caused by continuous molding, thereby completing the present invention.

[0065] That is, the cyclic olefin resin composition according to the present embodiment is as follows.

[0066] <Cyclic olefin resin composition>

[0067] The cyclic olefin resin composition according to the present embodiment includes:

[0068] Cyclic olefin copolymer (A),

[0069] Ester compound of polyglycerol and fatty acid (B) and

[0070] Polyglycerol (C),

[0071] The amount of the ester compound (B) is 0.05 parts by mass or more and 3 parts by mass or less relative to 100 parts by mass of the cyclic olefin copolymer (A).

[0072] The amount of the polyglycerol (C) is 0.001 parts by mass or more and 0.04 parts by mass or less based on 100 parts by mass of the cyclic olefin copolymer (A).

[0073] According to the cyclic olefin resin composition of this embodiment, it is possible to suppress contamination of the inside of the mold caused by continuous molding, in particular, it is possible to suppress contamination of the lens surface of the mold. Furthermore, it is possible to suppress contamination not only inside the mold but also at the vent.

[0074] In addition, if it is a molded body of the cyclic olefin resin composition involved in this embodiment, the internal haze is low, and the increase of the internal haze before and after the moisture and heat resistance test can be reduced. Further, the molded body can maintain transparency before and after the moisture and heat resistance test, so it can also be suitable for use requiring transparency.

[0075] [Cyclic olefin copolymer (A)]

[0076] The cyclic olefin-based copolymer (A) according to the present embodiment is a copolymer including a structural unit derived from a cyclic olefin as an essential constituent unit.

[0077] Examples of the cyclic olefin-based copolymer (A) include copolymers (A1) of ethylene or an α-olefin and a cyclic olefin.

[0078] The cyclic olefin compound constituting the copolymer (A1) according to the present embodiment is not particularly limited, and examples thereof include the cyclic olefin monomers described in paragraphs 0037 to 0063 of International Publication No. 2006 / 0118261.

[0079] The cyclic olefin copolymer (A1) according to the present embodiment preferably has the structural unit (a) and the structural unit (b) from the viewpoint of further improving heat resistance while maintaining a good performance balance between transparency and refractive index of the obtained optical component, or improving moldability.

[0080] Structural unit (a): at least one structural unit derived from an olefin represented by the following general formula (I).

[0081] [Chemistry 8]

[0082]

[0083] In the above general formula (I), R 300 It represents a hydrogen atom or a linear or branched hydrocarbon group having 1 to 29 carbon atoms.

[0084] Structural unit (b): at least one structural unit derived from a cyclic olefin selected from the group consisting of a repeating unit (AA) represented by the following general formula (II), a repeating unit (AB) represented by the following general formula (III), and a repeating unit (AC) represented by the following general formula (IV).

[0085] [Chemistry 9]

[0086]

[0087] In the above general formula (II), u is 0 or 1, v is 0 or a positive integer, and w is 0 or 1. 61 ~R 78 and R a1 and R b1 R may be the same as or different from each other and is a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms, a halogenated alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 15 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms. 75 ~R 78 They may be bonded to each other to form a single ring or multiple rings.

[0088] [Chemistry 10]

[0089]

[0090] In the above general formula (III), x and d are each independently an integer of 0 or greater than 1. y and z are each independently an integer of 0 to 2. 81 ~R 99R may be the same as or different from each other and is a hydrogen atom, a halogen atom, an aliphatic hydrocarbon group which is an alkyl group having 1 to 20 carbon atoms or a cycloalkyl group having 3 to 15 carbon atoms, an aromatic hydrocarbon group having 6 to 20 carbon atoms, or an alkoxy group. 89 and R 90 The carbon atom bound to R 93 The carbon atom or R 91 The carbon atom to which it is bonded may be bonded directly or through an alkylene group having 1 to 3 carbon atoms. 92 With R 99 or R 95 With R 99 They may be combined with each other to form a monocyclic or polycyclic aromatic ring.

[0091] [Chemistry 11]

[0092]

[0093] In the above general formula (IV), R 100 , R 101 They may be the same as or different from each other and represent a hydrogen atom or a hydrocarbon group having 1 to 5 carbon atoms. f is 1≤f≤18.

[0094] The olefin monomer as one of the copolymerization raw materials of the copolymer (A1) according to the present embodiment is an olefin monomer which forms the structural unit represented by the above general formula (I) by addition polymerization. Specifically, an olefin monomer represented by the following general formula (Ia) corresponding to the above general formula (I) is used.

[0095] [Chemistry 12]

[0096]

[0097] In the above general formula (Ia), R 300 It represents a hydrogen atom or a linear or branched hydrocarbon group having 1 to 29 carbon atoms.

[0098] As the olefin monomer represented by the general formula (Ia), for example, ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene, 3-ethyl-1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene, etc. can be mentioned. From the viewpoint of obtaining an optical component with better heat resistance, mechanical properties and optical properties, among these, ethylene and propylene are preferred, and ethylene is particularly preferred. Two or more olefin monomers represented by the general formula (Ia) can be used.

[0099] When the total amount of the constituent units constituting the cyclic olefin-based copolymer involved in the present embodiment is set to 100 mol%, the proportion of the structural unit (a) derived from olefin is preferably from 5 mol% to 95 mol%, more preferably from 20 mol% to 90 mol%, further preferably from 40 mol% to 80 mol%, and particularly preferably from 50 mol% to 70 mol%.

[0100] In addition, the proportion of the structural unit (a) derived from olefin can be adjusted by 13 C-NMR determination.

[0101] The cyclic olefin monomer as one of the copolymerization raw materials of the copolymer (A1) involved in this embodiment is a cyclic olefin monomer that is formed by addition polymerization as a structural unit (b) derived from a cyclic olefin represented by the above-mentioned general formula (II), the above-mentioned general formula (III) or the above-mentioned general formula (IV). Specifically, the cyclic olefin monomers represented by the general formulas (IIa), (IIIa) and (IVa) corresponding to the above-mentioned general formulas (II), (III) and (IV), respectively, are used.

[0102] [Chemistry 13]

[0103]

[0104] In the above general formula (IIa), u is 0 or 1, v is 0 or a positive integer, preferably an integer of 0 or more and 2 or less, more preferably 0 or 1, w is 0 or 1, and R 61 ~R 78 and R a1 and R b1 They may be the same or different and are a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms, a haloalkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 15 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms. 75 ~R 78 They may be bonded to each other to form a single ring or multiple rings.

[0105] [Chemistry 14]

[0106]

[0107] In the above general formula (IIIa), x and d are each independently an integer of 0 or 1 or more, preferably an integer of 0 or more and 2 or less, more preferably 0 or 1, y and z are each independently 0, 1 or 2, R 81 ~R 99They may be the same or different and are a hydrogen atom, a halogen atom, an aliphatic hydrocarbon group which is an alkyl group having 1 to 20 carbon atoms or a cycloalkyl group having 3 to 15 carbon atoms, an aromatic hydrocarbon group having 6 to 20 carbon atoms, or an alkoxy group, R 89 and R 90 The carbon atom bound to R 93 The carbon atom or R 91 The carbon atom to which it is bonded may be bonded directly or through an alkylene group having 1 to 3 carbon atoms. When y=z=0, R 92 With R 99 or R 95 With R 99 They may be combined with each other to form a monocyclic or polycyclic aromatic ring.

[0108] [Chemistry 15]

[0109]

[0110] In the above general formula (IVa), R 100 , R 101 They may be the same as or different from each other, and represent a hydrogen atom or a hydrocarbon group having 1 to 5 carbon atoms, and f is 1≤f≤18.

[0111] By using the olefin monomer represented by the above-mentioned general formula (Ia) or the cyclic olefin monomer represented by the general formula (IIa), (IIIa) or (IVa) as the copolymer component, the solubility of the cyclic olefin copolymer (A) in the solvent is further improved, thereby improving the moldability and improving the yield of the product.

[0112] As specific examples of the cyclic olefin monomer represented by the general formula (IIa), (IIIa) or (IVa), the compounds described in paragraphs 0037 to 0063 of International Publication No. 2006 / 0118261 can be used.

[0113] Specific examples include bicyclo-2-heptene derivatives (bicyclohept-2-ene derivatives), tricyclo-3-decene derivatives, tricyclo-3-undecene derivatives, tetracyclo-3-dodecene derivatives, pentacyclo-4-pentadecenes derivatives, pentacyclopentadiene derivatives, pentacyclo-3-pentadecenes derivatives, pentacyclo-4-hexadecene derivatives, pentacyclo-3-hexadecene derivatives, hexacyclo-4-heptadecenes derivatives, heptacyclo-5-eicosene derivatives. heptacyclic-4-eicosene derivatives, heptacyclic-5-heneicosene derivatives, octacyclic-5-hexadecene derivatives, nonacyclic-5-pentadecene derivatives, nonacyclic-6-hexadecene derivatives, cyclopentadiene-acenaphthylene adducts, 1,4-methylene-1,4,4a,9a-tetrahydrofluorene derivatives, 1,4-methylene-1,4,4a,5,10,10a-hexahydroanthracene derivatives, and cycloalkylene derivatives having 3 to 20 carbon atoms.

[0114] Among the cyclic olefin monomers (b) represented by the general formula (IIa), (IIIa) or (IVa), the cyclic olefin represented by the general formula (IIa) is preferred.

[0115] As the cyclic olefin monomer represented by the general formula (IIa), bicyclo[2.2.1]-2-heptene (also called norbornene), tetracyclo[4.4.0.1 2,5 .1 7,10 ]-3-dodecene (also called tetracyclododecene), preferably tetracyclo[4.4.0.1 2,5 .1 7,10 These cyclic olefins have a rigid ring structure and thus have the advantage of being easy to maintain the elastic modulus of the copolymer and the optical component.

[0116] When the total amount of the constituent units constituting the copolymer (A1) involved in the present embodiment is set to 100 mol%, the proportion of the constituent units (b) derived from the cyclic olefin monomer is preferably from 5 mol% to 95 mol%, more preferably from 10 mol% to 80 mol%, further preferably from 20 mol% to 60 mol%, and particularly preferably from 30 mol% to 50 mol%.

[0117] The copolymerization type of the copolymer (A1) involved in the present embodiment is not particularly limited, and for example, random copolymers, block copolymers, etc. can be cited. In the present embodiment, since optical components having excellent optical properties such as transparency, refractive index, and birefringence and high precision can be obtained, random copolymers are preferably used as the copolymer (A1) involved in the present embodiment.

[0118] The copolymer (A1) according to the present embodiment is preferably ethylene and tetracyclo[4.4.0.1 2,5 .17,10 ]-3-dodecene random copolymers and ethylene and bicyclo[2.2.1]-2-heptene random copolymers, more preferably ethylene and tetracyclo[4.4.0.1 2,5 .1 7,10 ]-random copolymer of 3-dodecene.

[0119] The copolymer (A1) according to the present embodiment may be used alone or in combination of two or more.

[0120] The copolymer (A1) according to the present embodiment can be produced by selecting appropriate conditions according to the methods of, for example, JP-A-60-168708, JP-A-61-120816, JP-A-61-115912, JP-A-61-115916, JP-A-61-271308, JP-A-61-272216, JP-A-62-252406, JP-A-62-252407, and the like.

[0121] In this embodiment, it is preferred that the cyclic olefin-based copolymer (A) has a repeating unit (AA) represented by the general formula (II) and a structural unit (D) derived from a cyclic olefin having an aromatic ring, wherein the repeating unit (AA) does not contain an aromatic ring, and the cyclic olefin having an aromatic ring comprises one or more selected from the group consisting of a compound represented by the following formula (D-1), a compound represented by the following formula (D-2), and a compound represented by the following formula (D-3).

[0122] [Chemistry 16]

[0123]

[0124] In the above (D-1), n ​​and q are each independently 0, 1 or 2. 1 ~R 17 are each independently a hydrogen atom, a halogen atom other than a fluorine atom, or a hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a halogen atom other than a fluorine atom, 10 ~R 17 In addition, when q = 0, R 10 With R 11 , R 11 With R 12 , R 12 With R 13 , R 13 With R 14 , R 14 With R 15 , R 15 With R 10They can be combined with each other to form a single ring or multiple rings. In addition, when q=1 or 2, R 10 With R 11 , R 11 With R 17 , R 17 With R 17 , R 17 With R 12 , R 12 With R 13 , R 13 With R 14 , R 14 With R 15 , R 15 With R 16 , R 16 With R 16 , R 16 With R 10 They may be bonded to each other to form a monocyclic ring or polycyclic rings, and the monocyclic ring or polycyclic rings may have a double bond, and the monocyclic ring or polycyclic rings may be aromatic rings.

[0125] [Chemistry 17]

[0126]

[0127] In the above formula (D-2), n and m are each independently 0, 1 or 2, and q is 1, 2 or 3. 18 ~R 31 Each is independently a hydrogen atom, a halogen atom other than a fluorine atom, or a hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a halogen atom other than a fluorine atom. 28 With R 29 , R 29 With R 30 , R 30 With R 31 They can be combined with each other to form a single ring or multiple rings. In addition, when q = 2 or 3, R 28 With R 28 , R 28 With R 29 , R 29 With R 30 , R 30 With R 31 , R 31 With R 31 They may be bonded to each other to form a monocyclic ring or polycyclic rings, the monocyclic ring or polycyclic rings may have a double bond, and the monocyclic ring or polycyclic rings may be aromatic rings.

[0128] [Chemistry 18]

[0129]

[0130] In the above formula (D-3), q is 1, 2 or 3, R 32 ~R 39 Each is independently a hydrogen atom, a halogen atom other than a fluorine atom, or a hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a halogen atom other than a fluorine atom. 36 With R 37 , R 37 With R 38 , R 38 With R 39 They can be combined with each other to form a monocyclic or polycyclic ring. In addition, when q=2 or 3, R 36 With R 36 , R 36 With R 37 , R 37 With R 38 , R 38 With R 39 , R 39 With R 39 They may be bonded to each other to form a monocyclic ring or polycyclic rings, the monocyclic ring or polycyclic rings may have a double bond, and the monocyclic ring or polycyclic rings may be aromatic rings.

[0131] In addition, as the hydrocarbon group having 1 to 20 carbon atoms of (D-1) to (D-3), for example, alkyl groups having 1 to 20 carbon atoms, cycloalkyl groups having 3 to 15 carbon atoms, and aromatic hydrocarbon groups can be mentioned independently. More specifically, as the alkyl group, methyl, ethyl, propyl, isopropyl, pentyl, hexyl, octyl, decyl, dodecyl, and octadecyl can be mentioned. As the cycloalkyl group, cyclohexyl can be mentioned. As the aromatic hydrocarbon group, aryl or aralkyl groups such as phenyl, tolyl, naphthyl, benzyl, and phenylethyl can be mentioned. These hydrocarbon groups may be substituted with halogen atoms other than fluorine atoms.

[0132] Such a cyclic olefin copolymer (A) can further suppress the generation of haze before and after the moist heat resistance test, and can further suppress the contamination of the inside of the mold due to continuous molding.

[0133] When all the structural units of the cyclic olefin-based copolymer (A) involved in the present embodiment are set to 100 mol%, the total content of the repeating unit (AA) represented by the general formula (II) and the structural unit (D) derived from the cyclic olefin having an aromatic ring is preferably 5 mol% to 95 mol%, more preferably 10 mol% to 90 mol%, further preferably 20 mol% to 80 mol%, further more preferably 30 mol% to 80 mol%, and further preferably 40 mol% to 78 mol%.

[0134] In this embodiment, the content of the repeating unit (AA) and the structural unit (D) can be adjusted by, for example1 H-NMR or 13 The measurement was performed by C-NMR.

[0135] The content of the cyclic olefin copolymer (A) according to the present embodiment is preferably 80% by mass to 99% by mass in the resin composition, more preferably 90% by mass to 99% by mass, and even more preferably 95% by mass to 99% by mass.

[0136] The glass transition temperature (Tg) of the cyclic olefin copolymer (A) according to the present embodiment is preferably in the range of 130° C. to 170° C. If the glass transition temperature (Tg) of the cyclic olefin copolymer (A) is in the above range, sufficient heat resistance can be obtained when used as an optical component requiring heat resistance, such as an in-vehicle camera lens or a camera lens for a portable device, and good moldability can be obtained.

[0137] The glass transition temperature (Tg) of the cyclic olefin copolymer (A) according to the present embodiment can be measured using a differential scanning calorimeter (DSC). For example, the glass transition temperature can be measured by using RDC220 manufactured by SII nanotechnology, in a nitrogen atmosphere, heating from room temperature to 200°C at a heating rate of 10°C / min, holding for 5 minutes, then cooling to 30°C at a cooling rate of 10°C / min, holding for 5 minutes, and then heating to 200°C at a heating rate of 10°C / min.

[0138] [Polyglycerol and fatty acid ester compound (B)]

[0139] The ester compound (B) according to the present embodiment is an ester compound of polyglycerol and fatty acid, and is an ester of polyglycerol in a dimer or higher state and a saturated or unsaturated fatty acid having 8 to 24 carbon atoms. The ester compound (B) is preferably an ester of triglycerol, which is a trimer, and a saturated or unsaturated fatty acid having 8 to 24 carbon atoms.

[0140] The cyclic olefin resin composition according to the present embodiment contains the ester compound (B), so that even under high temperature and high humidity, the cyclic olefin resin can suppress the generation of fine cracks and suppress the increase of internal haze.

[0141] Examples of the esters of such polyglycerol and saturated or unsaturated fatty acids include triglycerol oleate, tetraglycerol oleate, and polyglycerol oleate.

[0142] The content of the ester compound (B) in the cyclic olefin resin composition according to the present embodiment is generally 0.05 to 3 parts by mass, preferably 0.5 to 2 parts by mass, and more preferably 0.8 to 1.5 parts by mass, relative to 100 parts by mass of the cyclic olefin copolymer (A).

[0143] When the content of the ester compound (B) is at least the above lower limit, the change in internal haze before and after the moisture and heat resistance test can be suppressed. Further, when it is at most the above upper limit, the internal haze before the moisture and heat resistance test can be suppressed.

[0144] [Polyglycerol (C)]

[0145] The cyclic olefin resin composition according to the present embodiment contains a specific amount of polyglycerol (C). This can suppress mold contamination during continuous molding due to vaporization of alcohol contained as an impurity in the hydrophilic agent.

[0146] The polyglycerol (C) may be exemplified by diglycerol, triglycerol, tetraglycerol, etc., but is not limited thereto. The polyglycerol may be used alone or in combination of two or more.

[0147] The content of the polyglycerol (C) is 0.001 to 0.04 parts by mass, preferably 0.001 to 0.03 parts by mass, and more preferably 0.01 to 0.015 parts by mass, based on 100 parts by mass of the cyclic olefin copolymer (A).

[0148] If the polyglycerol (C) is within the above range, the change in internal haze can be reduced even before and after a more severe humidity and heat resistance test (e.g., 85°C 95% RH 1008 hours) than conventional humidity and heat resistance tests. In addition, contamination inside the mold can be suppressed during continuous molding of the molded body.

[0149] The content of the polyglycerol (C) can be adjusted by, for example, adding and adjusting the polyglycerol when preparing the cyclic olefin resin composition. As another example, when preparing the hydrophilic agent, a method of adjusting the content by adding polyglycerol in an amount that does not react with the ester compound (B) can also be exemplified. If the content of the polyglycerol (C) involved in the present embodiment is within the above range, the method for adjusting the content is not particularly limited.

[0150] (Other ingredients)

[0151] The cyclic olefin resin involved in the present embodiment can be combined with a weather stabilizer, a heat stabilizer, an antioxidant, a metal deactivator, a hydrochloric acid absorber, an antistatic agent, a flame retardant, a slip agent, an anti-blocking agent, an anti-fogging agent, a lubricant, a natural oil, a synthetic oil, a wax, an organic or inorganic filler, etc. as needed within a range that does not impair the purpose of the present embodiment, and the mixing ratio is an appropriate amount.

[0152] The cyclic olefin resin composition involved in the present embodiment can preferably be made into a molded body. As a method for molding the cyclic olefin resin composition to obtain a molded body, there is no particular limitation, and a known method can be used. Although it also depends on its use and shape, for example, extrusion molding, injection molding, inflation molding, blow molding, extrusion blow molding, injection blow molding, compression molding, vacuum molding, powder slush molding, calendering molding, foam molding, etc. can be applied. Among these, from the viewpoint of moldability and productivity, injection molding is preferably used. In addition, molding conditions can be appropriately selected according to the purpose of use or the molding method. For example, the resin temperature in injection molding is usually 150°C to 400°C, preferably 200°C to 350°C, and more preferably 230°C to 330°C.

[0153] The cyclic olefin resin composition involved in the present embodiment can be obtained, for example, by the following methods: a method of melt-kneading the cyclic olefin copolymer (A) and other components added as needed using a known kneading device such as an extruder and a Banbury mixer; a method of dissolving the cyclic olefin copolymer (A) and other components added as needed in a common solvent and then evaporating the solvent; a method of adding a solution of the cyclic olefin copolymer (A) and other components added as needed in a poor solvent to precipitate them, etc.

[0154] Next, the obtained molded body is annealed for 2 to 8 hours, for example, in the range of (glass transition temperature (Tg) of cyclic olefin copolymer (A) - 40) ° C to (glass transition temperature (Tg) of cyclic olefin copolymer (A) - 5) ° C, thereby obtaining an optical component. By performing the above-mentioned annealing treatment, the molecules of the cyclic olefin copolymer (A) in the molded body are relaxed and the free volume is reduced. Therefore, even if a heat treatment is performed, a change in specific gravity (change in volume) is not likely to occur.

[0155] Here, if the annealing conditions are made severe, the molded body will deform and cannot be restored, so it is preferably performed under the above conditions and within a range in which the molded body does not deform. That is, it is preferably performed at a temperature and time such that the molded body does not deform.

[0156] The optical component obtained by the above operation has excellent resistance to moisture and heat. Therefore, the increase of the internal haze before and after the moisture and heat resistance test can be suppressed, and it is mainly suitable for optical applications and lenses. In addition, since transparency can be maintained before and after the moisture and heat resistance test, it is also suitable for the purposes requiring transparency.

[0157] As mentioned above, although embodiment of this invention was described, these are illustrations of this invention, and various structures other than the above-mentioned can also be adopted.

[0158] In addition, the present invention is not limited to the above-mentioned embodiment, and modifications, improvements, etc. within the scope that can achieve the purpose of the present invention are also included in the present invention.

[0159] Example

[0160] Hereinafter, the present embodiment will be described in detail with reference to Examples etc. In addition, the present embodiment is not limited at all by the description of these Examples.

[0161] (Example 1)

[0162] <Polymerization of cyclic olefin copolymer (A)>

[0163] (Preparation of Catalyst)

[0164] VO(OC 2 H 5 )Cl 2 The solution was diluted with cyclohexane to prepare a vanadium catalyst cyclohexane solution having a vanadium concentration of 6.7 mmol / L. 2 H 5 ) 1.5 Cl 1.5 ) was diluted with cyclohexane to prepare a cyclohexane solution of an organic aluminum compound catalyst with an aluminum concentration of 107 mmol / L.

[0165] (polymerization)

[0166] Using a stirred polymerizer (inner diameter 500 mm, reaction volume 100 L), ethylene and tetracyclo[4.4.0.1 2,5 .1 7,10 ]-3-dodecene copolymerization reaction. Cyclohexane was used as the polymerization solvent. When the copolymerization reaction was carried out, the cyclohexane solution of the vanadium catalyst prepared by the above method was supplied to the polymerization vessel in such a manner that the concentration of the vanadium catalyst relative to cyclohexane in the polymerization vessel became 0.6 mmol / L.

[0167] Furthermore, ethylaluminum sesquichloride as an organic aluminum compound was supplied to the polymerization reactor so that the mass ratio of aluminum to vanadium (Al / V) was 18.0. The polymerization temperature was 8° C. and the polymerization pressure was 1.8 kg / cm 2 G, and then copolymerization was carried out continuously to obtain ethylene and tetracyclo[4.4.0.1 2,5 .1 7,10 ]-3-dodecene copolymer (ethylene-tetracyclo[4.4.0.1 2, 5 .1 7,10 ]-3-dodecene copolymer).

[0168] (deashing)

[0169] In the ethylene-tetracyclic [4.4.0.1 2,5 .1 7,10 ]-3-dodecene copolymer solution, water and a 25 mass % NaOH solution as a pH adjuster were added to stop the polymerization reaction. 2,5 .1 7,10 The catalyst residues present in the 3-dodecene copolymer were removed (deashing) to obtain a polymer solution A.

[0170] After the above deashing treatment, ethylene-tetracycline [4.4.0.1 2,5 .1 7,10 ]-3-dodecene copolymer cyclohexane solution (polymer solution A, polymer concentration 7.7 mass %), pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] as a stabilizer was added in an amount of 0.4 mass parts relative to 100 mass parts of the above copolymer, and then the effective volume of 1.0 cm was temporarily used. 3 Mix in a stirred tank for 1 hour.

[0171] (Desolventization)

[0172] When using 20kg / cm as a heat source 2 A cyclohexane solution of the copolymer having a concentration of 5 mass % was supplied at 150 kg / H to a double tube heater (outer tube diameter 2B, inner tube diameter 3 / 4B, length 21 m) with water vapor at G and heated to 180°C.

[0173] As a heat source, 25 kg / cm 2A double tubular flash dryer (outer diameter 2B, inner diameter 3 / 4B, length 27m) and a flash hopper (volume 200L) containing water vapor of 1000 g were used to remove most of the unreacted monomers from the cyclohexane solution of the copolymer that had undergone the above heating step together with cyclohexane as a polymerization solvent, thereby obtaining a cyclic olefin random copolymer in a molten state after flash drying (cyclic olefin copolymer (A-1)). The glass transition temperature (Tg) of the cyclic olefin copolymer (A-1) measured by a differential scanning calorimeter was 161°C.

[0174] <Ester compound of polyglycerol and fatty acid (B)>

[0175] As the ester compound (B) of polyglycerol and fatty acid, triglycerol oleate was used.

[0176] <Polyglycerol (C)>

[0177] Polyglycerol (C-1): A mixture of triglycerol and tetraglycerol.

[0178] Triglycerol:Tetraglycerol = 6:1

[0179] Polyglycerol (C-2): A mixture of diglycerol, triglycerol and tetraglycerol.

[0180] Diglycerol: triglycerol: tetraglycerol = 5:60:9

[0181] (Extrusion)

[0182] Using a twin-screw kneading extruder equipped with a vent, the molten cyclic olefin copolymer (A-1) was charged from the resin charging part of the extruder, and then, while suction was performed from the vent part through a trap by a vacuum pump for the purpose of removing volatiles, 0.90 parts by mass of triglycerol oleate relative to 100 parts by mass of the cyclic olefin copolymer (A-1) and 0.0072 parts by mass of polyglycerol (C-1) relative to the cyclic olefin copolymer (A-1) were added to the barrel part on the downstream side of the vent part, and kneading was performed on the downstream side of the extruder than the vent part. At this time, the conditions of the extruder were adjusted so that the difference between the maximum and minimum values ​​of the resin temperature in the manifold part of the extruder was within 3°C.

[0183] Next, the kneaded product was pelletized by an underwater pelletizer installed at the outlet of the extruder, and the obtained pellets were dried with hot air at a temperature of 100° C. for 4 hours.

[0184] Furthermore, for washing, a resin of about 3 to 5 times the amount of resin calculated from the average residence time in the polymerization vessel was allowed to flow, and then a sample was collected to obtain a resin composition containing a cyclic olefin copolymer (A-1). In order to suppress the mixing of iron atoms (Fe), stainless steel piping and polymerization devices were used in the polymer production equipment.

[0185] (Example 2)

[0186] A resin composition was produced in the same manner as in Example 1 except that the amount of triglycerol oleate added was 0.80 parts by mass and the amount of polyglycerol (C-1) added was 0.0064 parts by mass relative to 100 parts by mass of the cyclic olefin copolymer (A-1).

[0187] (Example 3)

[0188] A resin composition was produced in the same manner as in Example 1 except that the amount of triglycerol oleate added was 1.5 parts by mass based on 100 parts by mass of the cyclic olefin copolymer (A-1) and the amount of polyglycerol (C-1) added was 0.012 parts by mass based on 100 parts by mass of the cyclic olefin copolymer (A-1).

[0189] (Example 4)

[0190] TOPAS (registered trademark) COC 5013L-10 (manufactured by Polyplastics Co., Ltd., an addition copolymer of norbornene and ethylene, hereinafter referred to as cyclic olefin copolymer (A-2)) as a cyclic olefin copolymer (A) was introduced into a twin-screw extruder (manufactured by The Japan Steel Works, Ltd.: TEX44SS-30BW-3V). Furthermore, 0.90 parts by mass of triglycerol oleate and 0.0072 parts by mass of polyglycerol (C-1) were added to 100 parts by mass of the cyclic olefin copolymer (A-2), respectively, and melt-kneaded and pelletized to obtain a pelletized resin composition.

[0191] (Example 5)

[0192] A resin composition was produced in the same manner as in Example 4 except that the amount of triglycerol oleate added was 1.5 parts by mass based on 100 parts by mass of the cyclic olefin copolymer (A-2) and the amount of polyglycerol (C-1) added was 0.012 parts by mass based on 100 parts by mass of the cyclic olefin copolymer (A-2).

[0193] (Example 6)

[0194] A resin composition was produced in the same manner as in Example 1, except that the amount of triglycerol oleate added was 0.85 parts by mass relative to 100 parts by mass of the cyclic olefin copolymer (A-1), and that polyglycerol (C-2) was used as the polyglycerol (C) instead of polyglycerol (C-1) in an amount of 0.063 parts by mass relative to 100 parts by mass of the cyclic olefin copolymer (A-1).

[0195] (Example 7)

[0196] A resin composition was produced in the same manner as in Example 1 except that the amount of triglycerol oleate added was 4.0 parts by mass based on 100 parts by mass of the cyclic olefin copolymer (A-1) and the amount of polyglycerol (C-1) added was 0.032 parts by mass based on 100 parts by mass of the cyclic olefin copolymer (A-1).

[0197] <Evaluation>

[0198] [Internal haze]

[0199] The obtained resin composition was injection molded using an injection molding machine (ROBOSHOT S2000i-30α manufactured by FANUC) at a cylinder temperature of 275° C. and a mold temperature of 120° C. to form a test piece having an optical surface and measuring 35 mm×65 mm×3 mm thick.

[0200] The internal haze of the test piece was measured using benzyl alcohol in accordance with JIS K-7105.

[0201] [Wet and heat resistance test]

[0202] The test piece prepared for the internal haze measurement was left in an atmosphere of 85°C and 95% relative humidity for 1008 hours, then taken out to an atmosphere of 23°C and 50% relative humidity, and the internal haze was measured 48 hours later.

[0203] The amount of change (hereinafter, referred to as Δ internal haze) obtained by subtracting the internal haze before the moisture and heat resistance test from the internal haze after the moisture and heat resistance test was measured.

[0204] [Contamination of mold lens surface]

[0205] The obtained resin composition was injection molded using a mold for forming a flat lens having a lens portion having a diameter of 6.0 mm and a thickness of 0.5 mm and an injection molding machine (ROBOSHOT S2000i-30α manufactured by FANUC) at a barrel temperature of 285° C. and a mold temperature of 105° C., and a total of 4500 times of molding were performed. Every 900 times, the contamination of the lens surface of the mold was observed using a digital microscope VHX-5000 (manufactured by KEYENCE).

[0206] The number of moldings at which contamination of the lens surface was observed is recorded in Table 1. The case where no contamination occurred even after 4500 moldings was marked as “none”.

[0207] The results of Examples 1 to 7 are shown in Table 1. "-" means that no evaluation was performed.

[0208] [Table 1]

[0209]

[0210] In Examples 1 to 5 containing the ester compound (B) of polyglycerol and fatty acid and a specific amount of polyglycerol (C), the internal haze is low and the generation of internal haze before and after the wet heat resistance test can be suppressed. In addition, the contamination of the inside of the mold caused by continuous molding can be suppressed, especially the contamination of the lens surface of the mold can be suppressed.

[0211] On the other hand, in Example 6 containing a specific amount or more of polyglycerol, mold lens surface contamination could not be suppressed and occurred after molding 900 times. In Example 7, the pellets were cloudy, so mold lens surface contamination was not evaluated.

[0212] This application claims priority based on Japanese patent application No. 2021-018162, filed on February 8, 2021, the disclosure of which is incorporated herein in its entirety.

Claims

1. A cyclic olefin resin composition comprising: Cyclic olefin copolymer (A), Ester compound of polyglycerol and fatty acid (B) and Polyglycerol (C), The amount of the ester compound (B) is 0.05 parts by mass or more and 3 parts by mass or less relative to 100 parts by mass of the cyclic olefin copolymer (A). The amount of the polyglycerol (C) is 0.001 parts by mass or more and 0.04 parts by mass or less relative to 100 parts by mass of the cyclic olefin copolymer (A). The polyglycerol (C) comprises a mixture of triglycerol and tetraglycerol, The cyclic olefin copolymer (A) comprises a structural unit (a) and a structural unit (b), Structural unit (a): at least one structural unit derived from an olefin represented by the following general formula (I), Structural unit (b): at least one structural unit derived from a cyclic olefin selected from the group consisting of a repeating unit (AA) represented by the following general formula (II), a repeating unit (AB) represented by the following general formula (III), and a repeating unit (AC) represented by the following general formula (IV), [Chemistry 1] In the general formula (I), R 300 represents a hydrogen atom, or a linear or branched hydrocarbon group having 1 to 29 carbon atoms, [Chemistry 2] In the general formula (II), u is 0 or 1, v is 0 or a positive integer, w is 0 or 1, R 61 ~R 78 and R a1 and R b1 They may be the same or different and are a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms, a haloalkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 15 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms. 75 ~R 78 can be combined with each other to form a single ring or multiple rings, [Chemistry 3] In the general formula (III), x and d are each independently an integer of 0 or 1 or more, y and z are each independently an integer of 0 to 2, and R 81 ~R 99They may be the same or different and are a hydrogen atom, a halogen atom, an aliphatic hydrocarbon group which is an alkyl group having 1 to 20 carbon atoms or a cycloalkyl group having 3 to 15 carbon atoms, an aromatic hydrocarbon group having 6 to 20 carbon atoms, or an alkoxy group, R 89 and R 90 The carbon atom bound to R 93 The carbon atom or R 91 The carbon atom to which it is bonded may be bonded directly or through an alkylene group having 1 to 3 carbon atoms. In addition, when y=z=0, R 92 With R 99 or R 95 With R 99 may be combined with each other to form a monocyclic or polycyclic aromatic ring, [Chemistry 4] In the general formula (IV), R 100 , R 101 They may be the same as or different from each other, and represent a hydrogen atom or a hydrocarbon group having 1 to 5 carbon atoms, and f is 1≤f≤18.

2. The cyclic olefin resin composition according to claim 1, The cyclic olefin copolymer (A) has: The repeating unit (AA) represented by the general formula (II) and the structural unit (D) derived from a cyclic olefin having an aromatic ring, The repeating unit (AA) does not contain an aromatic ring, The cyclic olefin having an aromatic ring includes one or more selected from the group consisting of a compound represented by the following formula (D-1), a compound represented by the following formula (D-2), and a compound represented by the following formula (D-3), [Chemistry 5] In the above (D-1), n ​​and q are each independently 0, 1 or 2, R 1 ~R 17 are each independently a hydrogen atom, a halogen atom other than a fluorine atom, or a hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a halogen atom other than a fluorine atom, 10 ~R 17 One of them is a bonding bond. In addition, when q=0, R 10 With R 11 , R 11 With R 12 , R 12 With R 13 , R 13 With R 14 , R 14 With R 15 , R15 With R 10 can be combined with each other to form a monocyclic or polycyclic ring. In addition, when q=1 or 2, R 10 With R 11 , R 11 With R 17 , R 17 With R 17 , R 17 With R 12 , R 12 With R 13 , R 13 With R 14 , R 14 With R 15 , R 15 With R 16 , R 16 With R 16 , R 16 With R 10 may be combined with each other to form a monocyclic or polycyclic ring, and the monocyclic or polycyclic ring may have a double bond, and the monocyclic or polycyclic ring may be an aromatic ring, [Chemistry 6] In the formula (D-2), n and m are each independently 0, 1 or 2, q is 1, 2 or 3, and R 18 ~R 31 are each independently a hydrogen atom, a halogen atom other than a fluorine atom, or a hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a halogen atom other than a fluorine atom. When q=1, R 28 With R 29 , R 29 With R 30 , R 30 With R 31 They can be combined with each other to form a single ring or multiple rings. In addition, when q=2 or 3, R 28 With R 28 , R 28 With R 29 , R 29 With R 30 , R 30 With R 31 , R 31 With R 31 may be combined with each other to form a monocyclic or polycyclic ring, the monocyclic ring or the polycyclic ring may have a double bond, and the monocyclic ring or the polycyclic ring may be an aromatic ring, [Chemistry 7] In the formula (D-3), q is 1, 2 or 3, R 32 ~R 39are each independently a hydrogen atom, a halogen atom other than a fluorine atom, or a hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a halogen atom other than a fluorine atom. When q=1, R 36 With R 37 , R 37 With R 38 , R 38 With R 39 can be combined with each other to form a monocyclic or polycyclic ring. In addition, when q=2 or 3, R 36 With R 36 , R 36 With R 37 , R 37 With R 38 , R 38 With R 39 , R 39 With R 39 They may be combined with each other to form a monocyclic ring or polycyclic rings, the monocyclic ring or the polycyclic rings may have a double bond, and furthermore the monocyclic ring or the polycyclic rings may be an aromatic ring. 3 . The cyclic olefin resin composition according to claim 1 , wherein the glass transition temperature of the cyclic olefin copolymer (A) measured by a differential scanning calorimeter is 130° C. or higher and 170° C. or lower. 4 . A molded article comprising the cyclic olefin resin composition according to claim 1 . The molded article according to claim 4 , which is an optical member.