A method for preparing a self-healing polysiloxane dielectric elastomer composite material

By introducing dynamic chemical bonds into polysiloxane dielectric elastomer materials and using aromatic aldehydes to modify MXene with cross-linking agents and disulfide compounds, the self-healing problem of dielectric elastomer materials is solved and low-temperature rapid self-healing and High electrical drive strain performance improves the service life of the material.

CN116515302BActive Publication Date: 2024-10-18BEIJING UNIV OF CHEM TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310474997.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-10-18
Estimated Expiration
2043-04-27

AI Technical Summary

Technical Problem

Existing dielectric elastomer materials do not have self-healing properties. Once damaged or electrical breakdown occurs, they cannot be used again, resulting in a short service life of the dielectric elastomer driver and difficulty in achieving rapid self-healing at low temperatures.

Method used

By using aromatic aldehyde-modified two-dimensional transition metal carbonitride MXene as a dielectric filler, combined with a cross-linking agent and a disulfide compound to form dynamic imine bonds and disulfide bonds, a self-healing material capable of self-healing at room temperature was prepared. Polysiloxane dielectric elastomer composites.

Benefits of technology

The material achieves rapid self-healing after mechanical damage or electrical breakdown, improves high electrically driven strain performance under low electric fields, and has a simple preparation process and mild reaction conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116515302B_ABST
    Figure CN116515302B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a self-healing polysiloxane dielectric elastomer composite material, firstly, using aromatic aldehyde PA to modify a two-dimensional transition metal carbonitride MXene to obtain an aromatic aldehyde modified MXene; dissolving a cross-linking agent and a disulfide compound in tetrahydrofuran THF respectively, and mixing to obtain a mixed solution of a cross-linking agent and a disulfide compound; dissolving a lateral amino polysiloxane and PA-MXene in THF respectively, and obtaining a uniformly dispersed lateral amino polysiloxane solution and a PA-MXene suspension; adding the lateral amino polysiloxane solution and the PA-MXene suspension to the mixed solution, and then pouring the mixed solution into a polytetrafluoroethylene mold, volatilizing the solvent at room temperature, and obtaining a self-healing polysiloxane dielectric elastomer composite material. The above method has a simple operation process and mild reaction conditions, and the prepared material can quickly self-heal after mechanical damage or electrical breakdown.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of dielectric elastomers, and in particular to a method for preparing a self-healing polysiloxane dielectric elastomer composite material. Background Art

[0002] Dielectric elastomer is an electroactive polymer that can produce strain under the stimulation of an external electric field. The dielectric elastomer actuator, which consists of a dielectric elastomer film and flexible electrodes evenly coated on both sides of it, can convert electrical energy into mechanical energy and has broad application prospects in artificial muscles, actuators, generators and other fields.

[0003] However, the dielectric elastomer materials in the prior art do not have self-repairing properties. Once damaged or electrically broken down, they cannot be used again and can only be discarded, resulting in a very short service life of the dielectric elastomer drive, which is not conducive to the long-term stable use of the material. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a self-healing polysiloxane dielectric elastomer composite material. The method has a simple operation process and mild reaction conditions. The prepared material can quickly self-heal after mechanical damage or electrical breakdown, effectively solving the problem that the existing dielectric elastomer actuator cannot achieve low-temperature rapid self-healing, while taking into account high electric drive strain performance under low electric fields.

[0005] The objective of the present invention is achieved through the following technical solutions:

[0006] A method for preparing a self-healing polysiloxane dielectric elastomer composite material, the method comprising:

[0007] Step 1: First, the two-dimensional transition metal carbonitride MXene is modified by using an aromatic aldehyde PA to obtain a two-dimensional transition metal carbonitride modified by an aromatic aldehyde, which is recorded as PA-MXene, and the PA-MXene is used as a dielectric filler;

[0008] Step 2, dissolving the cross-linking agent and the disulfide compound in tetrahydrofuran (THF) respectively, and mixing them to obtain a mixed solution of the cross-linking agent and the disulfide compound;

[0009] Step 3, dissolving the lateral amino polysiloxane and PA-MXene in THF respectively to obtain a uniformly dispersed lateral amino polysiloxane solution and a PA-MXene suspension;

[0010] Step 4: Add the lateral amino polysiloxane solution and the PA-MXene suspension to the mixed solution obtained in step 2, pour the mixed solution into a polytetrafluoroethylene mold, evaporate the solvent at room temperature, and obtain a self-healing polysiloxane dielectric elastomer composite material.

[0011] It can be seen from the technical solution provided by the present invention that the above method has a simple operation process and mild reaction conditions. The prepared material can quickly self-heal after mechanical damage or electrical breakdown, effectively solving the problem that the existing dielectric elastomer actuator cannot achieve low-temperature rapid self-healing, while taking into account high electric drive strain performance under low electric fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0013] Figure 1 A schematic flow chart of a method for preparing a self-healing polysiloxane dielectric elastomer composite material provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0014] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments, which does not constitute a limitation of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0015] like Figure 1 The figure is a schematic flow chart of a method for preparing a self-healing polysiloxane dielectric elastomer composite material provided by an embodiment of the present invention, the method comprising:

[0016] Step 1: First, the two-dimensional transition metal carbonitride MXene is modified by using an aromatic aldehyde PA to obtain a two-dimensional transition metal carbonitride modified by an aromatic aldehyde, which is recorded as PA-MXene, and the PA-MXene is used as a dielectric filler;

[0017] In this step, specifically, 200 mg of MXene was dispersed in 60 mL of N,N-dimethylformamide to form a mixed solution;

[0018] Add 50-80 mg of aromatic aldehyde to the mixed solution, place it in a magnetic stirrer, set the stirring speed to 300-600 r / min, and stir for 1-6 hours at room temperature to form functionalized aldehyde groups on the surface of MXene to obtain a treated mixed solution;

[0019] The treated mixed solution was centrifuged and washed with ethanol, and then dried at 30°C for 24 h to obtain the aromatic aldehyde-modified MXene, which was recorded as PA-MXene.

[0020] Step 2, dissolving the cross-linking agent and the disulfide compound in tetrahydrofuran (THF) respectively, and mixing them to obtain a mixed solution of the cross-linking agent and the disulfide compound;

[0021] In this step, specifically, 0.03-0.15 g of the cross-linking agent is dissolved in 10 mL of THF and ultrasonically dispersed at 50 kHz for 30 min to form a uniformly dispersed cross-linking agent solution;

[0022] Dissolve 0.03-0.3 g of the disulfide compound in 10 mL of THF and disperse by ultrasound at 50 kHz for 30 min to form a uniformly dispersed disulfide compound solution;

[0023] The crosslinking agent solution and the disulfide compound solution are mixed, and stirred at 60° C. for 30-60 minutes to obtain a mixed solution of the crosslinking agent and the disulfide compound.

[0024] Step 3, dissolving the lateral amino polysiloxane and PA-MXene in THF respectively to obtain a uniformly dispersed lateral amino polysiloxane solution and a PA-MXene suspension;

[0025] In this step, 3 g of lateral amino polysiloxane is dissolved in 15 mL of THF, and ultrasonically dispersed at 50 kHz for 30 min to form a uniformly dispersed lateral amino polysiloxane solution;

[0026] 0.15-0.45 g of PA-MXene was dissolved in 60 mL of THF and ultrasonically dispersed at 50 kHz for 30 min to form a PA-MXene suspension.

[0027] Step 4: Add the lateral amino polysiloxane solution and the PA-MXene suspension to the mixed solution obtained in step 2, pour the mixed solution into a polytetrafluoroethylene mold, evaporate the solvent at room temperature, and obtain a self-healing polysiloxane dielectric elastomer composite material.

[0028] In this step, the side amino polysiloxane solution and the PA-MXene suspension are added to the mixed solution obtained in step 2, and the reaction is stirred at 60°C for 1-3 hours. The mixed solution is then poured into a polytetrafluoroethylene mold, and the solvent is evaporated at room temperature to obtain a self-healing polysiloxane dielectric elastomer composite material.

[0029] In a specific implementation, the side amino polysiloxane is a polysiloxane with an amino group on the side chain, with a viscosity of 300-1000 cP and an ammonia value of 0.6.

[0030] The cross-linking agent is one or both of terephthalaldehyde and isophthalaldehyde; the disulfide compound is one or both of 4,4'-diaminodiphenyl disulfide and 2,2'-dithiodibenzoic acid.

[0031] The aromatic aldehyde is one or more of benzaldehyde, 1-anthracenecarboxaldehyde and 1-pyrenecarboxaldehyde.

[0032] During the preparation process, the amino group in the side amino polysiloxane reacts with the aldehyde group in the cross-linker to form a dynamic imine bond. At the same time, the disulfide compound introduces a dynamic disulfide bond into the molecular chain, giving the polysiloxane excellent self-healing properties at room temperature. The aldehyde group in the aromatic aldehyde gives MXene good interfacial compatibility with the elastomer matrix, so that MXene can evenly and effectively form tiny capacitors in the above-mentioned self-healing elastomer, which not only improves the dielectric constant of the elastomer composite, but also maintains the self-healing properties and electrical breakdown strength of the matrix, and finally obtains a high-driving strain dielectric elastomer composite with excellent self-healing properties.

[0033] The self-healing polysiloxane dielectric elastomer composite material prepared by this method can complete self-healing at room temperature without any external auxiliary conditions, and the healing efficiency is as high as over 96% within 1 hour; the composite material has excellent electrical drive performance and mechanical properties, and the preparation process is simple, the reaction conditions are mild, and it is efficient and time-saving.

[0034] It is worth noting that the contents not described in detail in the embodiments of the present invention belong to the prior art known to professional and technical personnel in the field.

[0035] The following describes the preparation process, mechanical properties and electric drive performance of the composite material using a specific implementation case:

[0036] Implementation Case 1:

[0037] (1) 200 mg of MXene was dispersed in 60 mL of N,N-dimethylformamide to form solution 1;

[0038] (2) Add 50 mg of 1-pyrene formaldehyde to solution 1, place in a magnetic stirrer, set the speed to 600 r / min, and stir at room temperature for 2 h to obtain functionalized MXene to generate solution 2;

[0039] (3) Solution 2 was centrifuged and washed with ethanol, and then dried at 30 °C for 24 h to obtain PA-modified MXene, which was recorded as PA-MXene and used for later use;

[0040] (4) 3 g of aminopolysiloxane was dissolved in 15 mL of THF and ultrasonically dispersed at 50 kHz for 30 min to form a uniform solution 3;

[0041] (5) 0.3 g of PA-MXene was dissolved in 60 mL of THF and ultrasonically dispersed at 50 kHz for 30 min to form a uniform suspension 4;

[0042] (6) 0.1 g of terephthalaldehyde was dissolved in 10 mL of THF and ultrasonically dispersed at 50 kHz for 30 min to form a uniform solution 5;

[0043] (7) 0.2 g of 4,4'-diaminodiphenyl disulfide was dissolved in 10 mL of THF and ultrasonically dispersed at 50 kHz for 30 min to form a uniformly dispersed solution 6;

[0044] (8) Solution 5 and Solution 6 were mixed and stirred at 60° C. for 30 min to form Solution 7;

[0045] (9) Solution 3 and suspension 4 were added to solution 7, stirred at 60 °C for 3 h, poured into a polytetrafluoroethylene mold, and the solvent was evaporated at room temperature to obtain a self-healing polysiloxane dielectric elastomer composite material.

[0046] The dielectric elastomer composite material prepared in step (9) was subjected to a mechanical property test, and the tensile rate was set to 100 mm / min. The mechanical property self-healing test was performed by cutting the middle of the test specimen in a direction perpendicular to the tensile axis, then closely contacting the two fracture surfaces together, repairing at room temperature for 1 hour, and then conducting a mechanical property test again. The tensile test results are shown in Table 1 below.

[0047] The dielectric elastomer composite material prepared in step (9) is subjected to an electric drive performance test. The specific test method is: a circular flexible electrode with a diameter of 14 mm is sprayed on both sides of the dielectric elastomer film using a spray gun, and cured in a 60°C oven to form a dielectric elastomer actuator. A DC voltage is applied to the electrode, and a camera is used to record the change process of the electrode area under electric field stimulation in real time. The planar electric drive strain of the dielectric elastomer is calculated by the formula S = (A-A0) / A0×100%, where A0 is the area of ​​the electrode area when no electric field is applied, and A is the area under a certain electric field strength. The electric drive self-healing performance test is performed after the dielectric elastomer actuator is electrically broken down, repaired at room temperature for 1 hour, and the electric drive performance test is performed again. The results of the electric drive performance test are shown in Table 1 below.

[0048] Implementation Case 2: The preparation method is the same as that of Implementation Case 1, except that the amount of terephthalaldehyde added in step (6) is 0.03 g. The mechanical properties and electrodeformability tests of the prepared dielectric elastomer composite material were carried out before and after self-healing. The test results are shown in Table 1.

[0049] Implementation case 3: The preparation method is the same as that of implementation case 1, except that the amount of terephthalaldehyde added in step (6) is 0.15 g. The mechanical properties and electrodeformability tests of the prepared dielectric elastomer composite material are carried out before and after self-healing. The test results are shown in Table 1.

[0050] Implementation case 4. The preparation method is the same as that of implementation case 1, except that the amount of PA-MXene added in step (5) is 0.15 g. The mechanical properties and electrodeformability tests of the prepared dielectric elastomer composite material were carried out before and after self-healing. The test results are shown in Table 1.

[0051] Implementation case 5. The preparation method is the same as that of implementation case 1, except that the amount of PA-MXene added in step (5) is 0.45 g. The mechanical properties and electrodeformability tests of the prepared dielectric elastomer composite material were carried out before and after self-healing. The test results are shown in Table 1.

[0052] Implementation case 6. The preparation method is the same as that of implementation case 1, except that the amount of 4,4'-diaminodiphenyl disulfide added in step (7) is 0.03 g. The mechanical properties and electrodeformability tests of the prepared dielectric elastomer composite material were carried out before and after self-healing. The test results are shown in Table 1.

[0053] Implementation case 7. The preparation method is the same as that of implementation case 1, except that the amount of 4,4'-diaminodiphenyl disulfide added in step (7) is 0.3 g. The mechanical properties and electrodeformability tests of the prepared dielectric elastomer composite material were carried out before and after self-healing. The test results are shown in Table 1.

[0054] Example 8: The preparation method is the same as Example 1, except that the amount of 1-pyrene carboxaldehyde added in step (2) is 80 mg. The mechanical properties and electric drive performance of the prepared dielectric elastomer composite material were tested before and after self-healing. The test results are shown in Table 1.

[0055] Example 9: The preparation method is the same as Example 1, except that the crosslinking agent added in step (6) is 0.1 g of isophthalic acid. The mechanical properties and electric drive performance of the prepared dielectric elastomer composite material were tested before and after self-healing. The test results are shown in Table 1.

[0056] Example 10: The preparation method is the same as Example 1, except that the crosslinking agent added in step (7) is 0.2 g of 2,2'-dithiodibenzoic acid. The mechanical properties and electrodeformability tests of the prepared dielectric elastomer composite material were performed before and after self-healing. The test results are shown in Table 1.

[0057] Comparative Example 11: The preparation method is the same as that of Example 1, except that no PA-modified MXene is added. The mechanical properties and electrodeformability tests of the pure lateral amino polysiloxane elastomer were performed before and after self-healing, and the comparison results are shown in Table 1.

[0058] Table 1 Comparison of the performance of the composite materials prepared in the implementation case and the comparative case

[0059]

[0060] From the data in Table 1, it can be seen that when the PA-modified MXene is filled to 10wt%, the electro-induced deformation can reach 38.81% at 11.34kV / mm, and the self-healing efficiency reaches more than 96%. The self-healing dielectric elastomer composite prepared by this method has excellent self-healing properties, which produces a large electrically driven deformation at a lower electric field strength while maintaining the electrical breakdown strength of the matrix.

[0061] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the technical scope disclosed in the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims. The information disclosed in the background technology section of this article is only intended to deepen the understanding of the overall background technology of the present invention, and should not be regarded as an admission or in any form that the information constitutes prior art known to those skilled in the art.

Claims

1. A method for preparing a self-healing polysiloxane dielectric elastomer composite material, characterized in that: The method comprises: Step 1: First, the two-dimensional transition metal carbonitride MXene is modified by using an aromatic aldehyde PA to obtain a two-dimensional transition metal carbonitride modified by an aromatic aldehyde, which is recorded as PA-MXene, and the PA-MXene is used as a dielectric filler; Step 2, dissolving the cross-linking agent and the disulfide compound in tetrahydrofuran (THF) respectively, and mixing them to obtain a mixed solution of the cross-linking agent and the disulfide compound; Step 3, dissolving the lateral amino polysiloxane and PA-MXene in THF respectively to obtain a uniformly dispersed lateral amino polysiloxane solution and a PA-MXene suspension; Step 4, adding the amino-side polysiloxane solution and the PA-MXene suspension to the mixed solution obtained in step 2, pouring the mixed solution into a polytetrafluoroethylene mold, and volatilizing the solvent at room temperature to obtain a self-healing polysiloxane dielectric elastomer composite material; Wherein, the side amino polysiloxane is a polysiloxane with an amino group in the side chain, with a viscosity of 300-1000 cP and an ammonia value of 0.6; The cross-linking agent is one or both of terephthalaldehyde and isophthalaldehyde; The disulfide compound is one or both of 4,4'-diaminodiphenyl disulfide and 2,2'-dithiodibenzoic acid; The aromatic aldehyde is one or more of benzaldehyde, 1-anthracenecarboxaldehyde and 1-pyrenecarboxaldehyde.

2. The method for preparing the self-healing polysiloxane dielectric elastomer composite material according to claim 1, characterized in that: The process of step 1 is specifically as follows: 200 mg of MXene was dispersed in 60 mL of N,N-dimethylformamide to form a mixed solution; Add 50-80 mg of aromatic aldehyde to the mixed solution, place it in a magnetic stirrer, set the stirring speed to 300-600 r / min, and stir for 1-6 hours at room temperature to form functionalized aldehyde groups on the surface of MXene to obtain a treated mixed solution; The treated mixed solution was centrifuged and washed with ethanol, and then dried at 30°C for 24 h to obtain the aromatic aldehyde-modified MXene, which was recorded as PA-MXene.

3. The method for preparing the self-healing polysiloxane dielectric elastomer composite material according to claim 1, characterized in that: The process of step 2 is specifically as follows: 0.03-0.15 g of the cross-linking agent was dissolved in 10 mL of THF and ultrasonically dispersed at 50 kHz for 30 min to form a uniformly dispersed cross-linking agent solution; Dissolve 0.03-0.3 g of the disulfide compound in 10 mL of THF and disperse by ultrasound at 50 kHz for 30 min to form a uniformly dispersed disulfide compound solution; The crosslinking agent solution and the disulfide compound solution are mixed, and stirred at 60° C. for 30-60 minutes to obtain a mixed solution of the crosslinking agent and the disulfide compound.

4. The method for preparing the self-healing polysiloxane dielectric elastomer composite material according to claim 1, characterized in that: The process of step 3 is specifically as follows: 3 g of amino-side polysiloxane was dissolved in 15 mL of THF and ultrasonically dispersed at 50 kHz for 30 min to form a uniformly dispersed amino-side polysiloxane solution; 0.15-0.45 g of PA-MXene was dissolved in 60 mL of THF and ultrasonically dispersed at 50 kHz for 30 min to form a PA-MXene suspension.

5. The method for preparing the self-healing polysiloxane dielectric elastomer composite material according to claim 1, characterized in that: The process of step 4 is specifically as follows: Add the side amino polysiloxane solution and the PA-MXene suspension to the mixed solution obtained in step 2, stir and react at 60°C for 1-3 hours, pour the mixed solution into a polytetrafluoroethylene mold, evaporate the solvent at room temperature, and obtain a self-healing polysiloxane dielectric elastomer composite material.

Citation Information

Patent Citations

  • MXene doped polymer solid electrolyte membrane and application thereof

    CN110739489A

  • Bionic MXene aerogel-based sensing material as well as preparation method and application thereof

    CN112834088A