A high-strength low-temperature impact-resistant alloy rod and preparation method thereof
By optimizing the elemental composition and process steps of alloy rods, the low-temperature impact resistance of alloy rods is improved, the problem of insufficient performance of alloy rods in low-temperature environments is solved, and high-strength and low-cost production effects are achieved.
Patent Information
- Application Number
- CN202310515280.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-09
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-05-09
AI Technical Summary
The impact resistance of alloy rods in low-temperature environments is insufficient, especially in cold northern regions, and it is difficult to meet the demand for use. Nickel, as a scarce resource, results in high production costs and limited performance improvement.
By optimizing the elemental composition of alloy rods, including the proportions of carbon, silicon, manganese, chromium, molybdenum, aluminum and vanadium, and using process steps such as converter smelting, LF refining, VD vacuum and bloom continuous casting, the element dosage and Process parameters are used to form high-strength low-temperature impact-resistant alloy rods, and combined with magnetic flux leakage and ultrasonic joint testing to ensure material quality.
It significantly improves the tensile strength, yield strength and -20°C impact energy KV2 value of the alloy rod, improves its low-temperature impact resistance, meets the use needs in cold northern regions, and reduces production costs.
Smart Images

Figure GDA0004993069950000051 
Figure GDA0004993069950000061 
Figure GDA0004993069950000071
Abstract
Description
Technical Field
[0001] The present application relates to the field of alloy rods, and more specifically, to a high-strength, low-temperature impact-resistant alloy rod and a preparation method thereof. Background Art
[0002] With the transformation of my country's automobile industry and machinery industry, the alloy bar industry has developed rapidly, its application fields have been continuously expanded, and its varieties have become increasingly complete and diversified, and it has entered a stage of high-quality development. At present, alloy bars are widely used in parts in the fields of automobiles and engineering machinery. They have the highest strength, but after overall quenching and tempering, there are problems such as insufficient low-temperature impact performance.
[0003] In the related art, by introducing nickel into the alloy bar raw material, the low-temperature impact resistance of the alloy bar after overall quenching and tempering is improved. However, since nickel is a relatively scarce resource, the production cost is relatively high. Moreover, when nickel is added, the low-temperature impact performance of the alloy bar is still relatively low, which makes it difficult to meet the use requirements in harsh low-temperature environments such as the colder northern regions. Summary of the invention
[0004] In order to improve the low-temperature impact resistance of alloy rods, the present application provides a high-strength low-temperature impact-resistant alloy rod and a preparation method thereof.
[0005] In the first aspect, the present application provides a high-strength, low-temperature impact-resistant alloy rod, which adopts the following technical solution: a high-strength, low-temperature impact-resistant alloy rod, which includes the following elements in weight percentage: a high-strength, low-temperature impact-resistant alloy rod, characterized in that it includes the following elemental components in weight percentage: carbon 0.34-0.38%, silicon 0.17-0.37%, manganese 0.80-1.00%, chromium 0.80-1.20%, molybdenum 0.15-0.25%, aluminum 0-0.002%, vanadium 0-0.04%, phosphorus ≤0.020%, sulfur ≤0.020%, and the remainder is iron and unavoidable impurities.
[0006] The raw materials of the alloy rod for high-pressure boiler tubes of the present application can be selected from carbon 0.34-0.38%, silicon 0.17-0.37%, manganese 0.80-1.00%, chromium 0.80-1.20%, molybdenum 0.15-0.25%, aluminum 0-0.002%, vanadium 0-0.04%, phosphorus ≤0.020%, sulfur ≤0.020%, and the balance is iron and inevitable impurities. Any value within the respective ranges can be selected, and the low-temperature impact resistance of the alloy rod can be improved. When the carbon is 0.36%, the silicon is 0.27%, the manganese is 0.90%, the chromium is 1.00%, the molybdenum is 0.20%, the phosphorus is 0.010%, and the sulfur is 0.015%, and the balance is iron 97.22% and 0.025% inevitable impurities, the effect is best.
[0007] By adopting the above technical solution, carbon can form precipitates with elements such as chromium and molybdenum. The precipitated carbides can improve the material's long-term creep performance through dispersion strengthening and other methods. Silicon is the main element for deoxidation, and silicon can also improve the strength of steel. Manganese plays a role in solid solution strengthening, which can improve the strength and toughness of steel and improve the processing performance of steel.
[0008] Chromium has high resistance to steam corrosion and hot corrosion. With the increase of chromium content, the steam corrosion resistance of steel increases significantly, and it can also improve the oxidation resistance and strength of alloy bars. Molybdenum can refine grains, improve hardenability and hot strength, and maintain sufficient strength and creep resistance at high temperatures.
[0009] Harmful elements phosphorus and sulfur will increase the segregation of steel at grain boundaries or subgrain boundaries, which can significantly reduce the high-temperature fatigue strength, stress corrosion resistance and thermal creep performance of alloy steel, increase its embrittlement tendency, and make the fracture performance of alloy steel under hydrogen corrosion conditions more obvious. Therefore, this application strictly reduces the phosphorus content and sulfur content in the alloy bar.
[0010] Preferably, the high-strength low-temperature impact-resistant alloy rod further comprises 0.001-0.002% aluminum.
[0011] By adopting the above technical solution, aluminum is also the main element for deoxidation, which can play a role in refining the grains. From the perspective of ensuring the deoxidation of molten steel and reducing the cleanliness of steel, the reinforcing effect of silicon is further improved.
[0012] In a second aspect, the present application provides a method for preparing a high-strength low-temperature impact-resistant alloy bar, which is specifically achieved through the following technical solutions:
[0013] A high-strength low-temperature impact-resistant alloy bar comprises the following steps:
[0014] Converter smelting: put molten iron and scrap steel into the converter, blow, add aluminum bars for strong deoxidation before tapping, further alloy in the ladle after deoxidation, and control the aluminum content at the station to 0.020-0.050%;
[0015] LF refining: using CaO-Al2O3-SiO2 slag system, binary basicity CaO / SiO2 controlled at 4-8, argon blowing in the ladle, slag treatment, heating, stop blowing argon, the slag basicity after refining is 5-10, white slag retention time ≥15min;
[0016] VD vacuum: deep vacuum degree ≤67Pa, vacuum maintenance time ≥15min, feed calcium-silicon wire, perform overall quenching and tempering, perform soft blowing, soft blowing time ≥15min, and stand for 20-35min;
[0017] Bloom continuous casting;
[0018] Billet heating: Heat the billet, the preheating section temperature is ≤850℃, the heating section temperature is 1200-1280℃, the soaking section temperature is 1210-1270℃, the rolling start temperature is 1150±30℃, and the total heating time is ≥300min;
[0019] Blooming rolling: 9 passes of reciprocating rolling, maximum reduction 80-90mm;
[0020] sawing and collecting;
[0021] Slow cooling after entering the pit: the temperature entering the pit is ≥500℃, the cooling rate is 6~8℃ / h, and the temperature leaving the pit is ≤100℃;
[0022] Combined flaw detection: using magnetic flux leakage and ultrasonic combined flaw detection method.
[0023] By adopting the above technical scheme, through converter smelting, that is, blowing, the carbon in the molten steel is reduced, and harmful impurities are removed, that is, dephosphorization, desulfurization and deoxidation are carried out to prevent the cold brittleness of steel caused by phosphorus and the hot brittleness of steel caused by sulfur. When the composition and temperature of the molten steel are adjusted to the specified value, the steel is tapped. Before tapping, aluminum bars are added to the furnace for deoxidation. The aluminum element has a greater affinity for oxygen than iron, thereby achieving a strong deoxidation effect. At the same time, converter smelting can also remove hydrogen, nitrogen gas and non-metallic inclusions such as oxides, sulfides, phosphides, and nitrides. Secondly, converter smelting adjusts the composition and temperature of the molten steel. Since there is a large amount of basic slag in the converter, it is difficult to completely deoxidize in the furnace, so the molten steel is poured into the ladle below the converter, and aluminum bars are added to the ladle for further deoxidation and alloying.
[0024] LF slag in LF refining is the oxides formed by the oxidation of various elements, the sand and rust brought in by scrap steel, the corroded lining refractory materials and various slag-making materials added. The slag is alkaline slag, and the basicity of the slag is 5-10, which can achieve the purpose of dephosphorization, desulfurization and deoxidation. The white slag retention time is controlled at ≥15min, which can reduce the content of oxygen, sulfur and inclusions in the alloy bar.
[0025] VD vacuum control deep vacuum degree ≤67Pa, vacuum maintenance time ≥15min, soft blowing time ≥15min, remove larger particle inclusions in molten steel, let it stand for 20-35min after soft blowing, which can promote the floating of small particle inclusions and improve the purity of steel.
[0026] The use of large square billet continuous casting can reduce non-metallic inclusions in the billet, prevent internal looseness, and increase the casting speed. The preheating section temperature of the billet heating is controlled at ≤850℃, the heating section temperature is controlled at 1200-1280℃, the soaking section temperature is controlled at 1210-1270℃, and the rolling temperature is controlled at 1150±30℃, which can prevent defects such as overheating, overburning and decarburization.
[0027] The slab rolling adopts 1100 slab rolling machine, which is rolled back and forth for 9 times with a maximum reduction of 90mm. The large reduction is used to improve the grain size crushing ability, refine the grain size of the organization, and improve the impact performance of the raw materials. Slow cooling after entering the pit helps to release the internal stress of the rolled material and prevent cracks in the rolled material. The temperature entering the pit is controlled at ≥500℃, which can avoid cracking inside the alloy bar and improve the qualified rate of subsequent flaw detection. The cooling rate is 6-8℃ / h, which reduces the organizational stress and thermal stress generated during the cooling process, avoids the surface and internal cracks of the ingot, and maximizes the production rhythm.
[0028] Combined flaw detection uses magnetic flux leakage and ultrasonic combined flaw detection to ensure the surface and internal quality of the bar. Magnetic flux leakage flaw detection is when the alloy bar is magnetized, a leakage magnetic field is formed on its surface due to defects on the surface or near the surface of the test piece. People can find defects by detecting changes in the leakage magnetic field. Ultrasonic flaw detection is when ultrasonic waves enter an object and encounter defects, part of the sound waves will be reflected, and the receiver can analyze the reflected waves, which can accurately measure the defects in the alloy bar and display the location and size of the internal defects. The combined flaw detection of the two can accurately measure the internal and external defects of the alloy bar.
[0029] Preferably, 0.03-0.04% vanadium is added during steel tapping in the converter smelting step.
[0030] By adopting the above technical solution and adding the microalloying element vanadium, the grain size of the structure can be refined, the strength and toughness of the alloy rod can be improved, and thus the low-temperature impact resistance of the alloy rod can be improved.
[0031] Preferably, the LF refining step adopts narrow composition control technology, with carbon controlled at ±0.01%, and manganese and chromium controlled at ±0.02%.
[0032] By adopting the above technical solution, LF refining uses narrow composition control technology to accurately control the composition of various alloy elements in the alloy bar, reduce fluctuations, control carbon to ±0.01%, and control manganese and chromium to ±0.02%, thereby improving the stability of raw material performance.
[0033] Preferably, in the VD vacuum step, after the vacuum treatment, the molten steel is soft-blown at an argon flow rate of 40 to 80 Nl / min.
[0034] By adopting the above technical solution, the argon flow rate is controlled at 40-80Nl / min, which can improve the effect of removing inclusions, increase the purity of the alloy rod, and thus improve the strength and low-temperature impact resistance of the alloy rod.
[0035] Preferably, in the large square billet continuous casting step, the superheat of the molten steel in the tundish is controlled at 20-35°C, and the billet drawing speed is 0.80-1.0 m / min.
[0036] By adopting the above technical solution, the superheat of the water tundish and the casting speed of the billet are controlled, so that cracks in the billet can be prevented during the continuous casting of the billet, thereby improving the effect of the continuous casting of the billet.
[0037] As a preference: in the step of slowly cooling in the pit, when the rolled material enters the pit for slow cooling, a cushion plate is laid at the bottom and a cover plate is laid on the top.
[0038] By adopting the above technical scheme, the rolled material is slowly cooled in the pit, a pad is laid underneath and a cover is placed on top, which can reduce the influence of the formed "hot zone" and "cold zone" on the process accuracy and performance uniformity and reliability of the rolled material, and improve the hardness of the alloy bar.
[0039] In summary, the present application includes at least one of the following beneficial technical effects:
[0040] (1) The present application controls the type and dosage of each element component so that the tensile strength and yield strength of the alloy bar after overall quenching and tempering are 750MPa and 550MPa respectively, which has high strength, and the impact energy KV2 at -20℃ can reach 30J, thereby improving the low-temperature impact resistance of the alloy bar.
[0041] (2) The present application adds aluminum to the alloy bar so that the -20°C impact energy KV2 of the overall quenched and tempered alloy bar reaches 34-37J, thereby further improving the low-temperature impact resistance of the alloy bar.
[0042] (3) The present application adds 0.03%-0.04% vanadium element during steel tapping in the converter smelting step, so that the -20°C impact energy KV2 of the overall quenched and tempered alloy rod reaches 41-43J, further improving the low-temperature impact resistance of the alloy rod.
[0043] (4) The present application adopts narrow composition control technology in LF refining to accurately control the composition of various alloy elements in the alloy rod and reduce fluctuations. The carbon is controlled at ±0.01%, and the manganese and chromium are controlled at ±0.02%. The -20°C impact energy KV2 of the overall quenched and tempered alloy rod reaches 45J, thereby improving the low-temperature impact resistance of the alloy rod.
[0044] (5) In the present application, in the VD vacuum step, after vacuum treatment, soft blowing of molten steel is maintained under the condition of an argon gas flow rate of 60 Nl / min, so that the -20°C impact energy KV2 of the overall tempered alloy rod reaches 46J, thereby further improving the low-temperature impact resistance of the alloy rod.
[0045] (6) In the process of continuous casting of large square billets, the present application controls the superheat of the molten steel in the tundish to 30°C and the billet drawing speed to 0.9 m / min, so that the -20°C impact energy KV2 of the overall tempered alloy bar reaches 48J, thereby further improving the low-temperature impact resistance of the alloy bar.
[0046] (7) In the present application, during the slow cooling step, the rolled material is put into the pit, a pad is laid underneath, and a cover is placed on top, so that the -20°C impact energy KV2 of the overall tempered alloy bar reaches 52J, thereby further improving the low-temperature impact resistance of the alloy bar.
[0047] (8) In the present application, the maximum reduction is controlled to 90 mm through 9 reciprocating rolling during the billet rolling process. The impact energy KV2 of the alloy bar after overall quenching and tempering at -20°C is higher than that of the alloy bar after the maximum reduction is controlled to 80 mm and 40 mm. It can be seen that the maximum reduction is controlled to 90 mm through 9 reciprocating rolling during the billet rolling process, which improves the low-temperature impact resistance of the alloy bar. DETAILED DESCRIPTION
[0048] The present application is further described in detail below in conjunction with specific embodiments.
[0049] The following raw materials in this application are all commercially available products, and are intended to fully disclose the raw materials in this application, and should not be understood as limiting the sources of the raw materials. Specifically: silicon carbon, SiC65; silicon manganese, FeMn68Si18; ferrochrome, FeCr65C0.10; ferromolybdenum, FeMo60; ferroaluminum, AlFe20; ferrovanadium, FeV60.
[0050] Example 1
[0051] A high-strength low-temperature impact-resistant alloy bar is prepared by the following steps:
[0052] Converter smelting: according to the dosage in Table 1, the raw materials are loaded into the converter, blown, and aluminum bars are added for strong deoxidation before tapping. After deoxidation, further alloying is performed in the ladle (i.e., silicon manganese, ferrochrome, and ferromolybdenum are added), and the aluminum leaving the station is controlled to be 0.030%;
[0053] LF refining: CaO-Al2O3-SiO2 slag system is used, the binary basicity CaO / SiO2 is controlled at 6, argon is blown into the ladle, the slag is treated, heated, and argon blowing is stopped. The basicity of the slag after refining is about 7, and the white slag is kept for 15 minutes;
[0054] VD vacuum: deep vacuum degree 67Pa, vacuum maintenance time 15min, feed calcium-silicon wire and aluminum wire, perform overall quenching and tempering, soft blowing under the condition of argon flow rate 50Nl / min, soft blowing time 15min, stand for 30min;
[0055] Continuous casting of large square billets; the superheat of the molten steel in the tundish is 40°C, and the billet drawing speed is 1m / min;
[0056] Ingot heating: Ingot is heated, the preheating section temperature is 850℃, the heating section temperature is 1240℃, the soaking section temperature is 1250℃, the rolling start temperature is 1150℃, and the total heating time is 300min;
[0057] Billet rolling: 9 passes of reciprocating rolling, maximum reduction 90mm;
[0058] sawing and collecting;
[0059] Slow cooling after entering the pit: the temperature of entering the pit is 500℃, the cooling rate is 7℃ / h, and the temperature of exiting the pit is 100℃;
[0060] Combined flaw detection: using magnetic flux leakage and ultrasonic combined flaw detection method.
[0061] Embodiment 2-6
[0062] The preparation methods of the high-strength low-temperature impact-resistant alloy bars of Examples 2-6 are the same, except that the alloy bars also include aluminum elements, that is, aluminum iron is further added during ladle alloying after deoxidation, and the specific addition amounts are shown in Table 1.
[0063] Table 1 Content of each raw material component of high strength low temperature impact resistant alloy rods of Examples 1-6 (unit: %)
[0064]
[0065]
[0066] The balance is Fe and inevitable impurities, and the inevitable impurities are ≤ 0.03%.
[0067] Embodiment 7-11
[0068] The high-strength, low-temperature impact-resistant alloy rods of Examples 7-11 have the same elemental composition as that of Example 1, except that ferrovanadium is added during steelmaking in the converter smelting step, so that the vanadium content is 0.02%, 0.03%, 0.035%, 0.04% and 0.045%, and the iron content is 97.1985%, 97.1835%, 97.1785% and 97.1735%. The types and amounts of other elements are the same as those in Example 4.
[0069] Example 12
[0070] The high-strength low-temperature impact-resistant alloy rod of Example 12 has the same elemental composition as that of Example 9, except that the narrow composition control technology is adopted in the LF refining step, carbon is controlled at ±0.01%, manganese and chromium are controlled at ±0.02%, and the remaining operations are the same as those of Example 9.
[0071] Embodiment 13
[0072] The high-strength, low-temperature impact-resistant alloy rod of Example 13 has the same elemental composition as that of Example 12, with the difference being that in the VD vacuum step, after the vacuum treatment, the molten steel is soft-blown under the condition of an argon flow rate of 60 Nl / min, and the rest of the operations are the same as those of Example 12.
[0073] Embodiment 14
[0074] The high-strength, low-temperature impact-resistant alloy rod of Example 14 has the same elemental composition as that of Example 13, with the difference that in the large square billet continuous casting step, the superheat of the molten steel in the tundish is controlled at 30°C, the billet drawing speed is 0.9m / min, and the rest of the operations are the same as those of Example 13.
[0075] Embodiment 15
[0076] The high-strength low-temperature impact-resistant alloy rod of Example 15 has the same elemental composition as that of Example 14, the difference being that in the pit slow cooling step, the rolled material is put into the pit, a pad is laid underneath, and a cover plate is placed on top, and the rest of the operations are the same as those of Example 14.
[0077] Example 16
[0078] The high-strength, low-temperature impact-resistant alloy rod of Example 16 has the same elemental composition as that of Example 15, except that the billet rolling is performed through 9 reciprocating rolling passes with a maximum reduction of 80 mm, and the remaining operations are the same as those of Example 14.
[0079] Embodiment 17
[0080] The preparation method of the high-strength low-temperature impact-resistant alloy rod in Example 17 is exactly the same as that in Example 15, except that: billet rolling: 9 passes of reciprocating rolling, the maximum reduction is 40 mm, and the other raw materials and admixtures are the same as those in Example 15.
[0081] Embodiment 18
[0082] The preparation method of the high-strength low-temperature impact-resistant alloy rod in Example 18 is exactly the same as that in Example 15, with the difference that the pit entry temperature is 450°C, the cooling rate is 9°C / h, the pit exit temperature is 100°C, and the other raw materials and admixtures are the same as those in Example 15.
[0083] Comparative Example 1
[0084] The preparation method of the high-strength low-temperature impact-resistant alloy rod of Comparative Example 1 is exactly the same as that of Example 1, except that an equal amount of chromium in the alloy rod is replaced by iron, and the remaining raw materials and admixtures are the same as those of Example 1.
[0085] Comparative Example 2
[0086] The preparation method of the high-strength low-temperature impact-resistant alloy rod of Comparative Example 2 is exactly the same as that of Example 1, except that an equal amount of silicon in the alloy rod is replaced by iron, and the remaining raw materials and admixtures are the same as those of Example 1.
[0087] Comparative Example 3
[0088] The preparation method of the high-strength low-temperature impact-resistant alloy rod of Comparative Example 3 is exactly the same as that of Example 1, except that an equal amount of the molybdenum element in the alloy rod is replaced by iron, and the remaining raw materials and admixtures are the same as those of Example 1.
[0089] Performance test (I)
[0090] The following testing standards or methods were used to test the basic properties of the alloy bars obtained in different Examples 1-18 and Comparative Examples 1-3. The test results are shown in Table 2.
[0091] Tensile strength: The tensile strength of alloy bars is tested in accordance with GB / T 228.1-2010 "Room Temperature Tensile Test Method for Metallic Materials".
[0092] Yield strength: The yield strength of alloy bars is tested in accordance with GB / T 228.1-2010 "Room Temperature Tensile Test Method for Metallic Materials".
[0093] -20℃ impact energy KV2: Test the -20℃ impact energy KV2 of alloy bars in accordance with GB / T 229-2007 "Charpy pendulum impact test method for metallic materials".
[0094] Table 2 Performance test results of different alloy bars
[0095]
[0096]
[0097] The test results in Table 2 show that the alloy bar obtained in the present application has a maximum tensile strength and a yield strength of 790 MPa and 585 MPa respectively after overall quenching and tempering, has high strength, and the -20°C impact energy KV2 can reach up to 52 J, which improves the low-temperature impact resistance of the alloy bar and can meet the low-temperature impact toughness required in the northern cold regions.
[0098] Combined with the performance test data of the alloy bar in Example 1, it is found that the tensile strength and yield strength of the alloy bar obtained in Example 1 after overall quenching and tempering are 750MPa and 550MPa respectively, which has high strength, and the -20°C impact energy KV2 can reach 30J, which improves the low-temperature impact resistance of the alloy bar. It shows that the element composition and dosage of the alloy bar in Example 1 of the present application and the preparation method of the alloy bar in the example can improve the low-temperature resistance of the alloy bar.
[0099] In Examples 2-6, the alloy bars obtained in Examples 3-5 have a tensile strength and a yield strength of 760-765 MPa and 555-560 MPa respectively after overall quenching and tempering, and have relatively high strength, and the -20°C impact energy KV2 can reach 34-37 J, indicating that adding 0.001-0.002% aluminum to the alloy bars can improve the low-temperature impact resistance of the alloy bars, which may be related to the fact that aluminum is also the main element for deoxidation and can play a role in refining the grains.
[0100] In Examples 7-11, the alloy bars obtained in Examples 8-10 have a tensile strength and a yield strength of 770-775 MPa and 568-572 MPa respectively after overall tempering, have relatively high strength, and the impact energy KV2 at -20°C can reach 41-43 J, indicating that the addition of 0.03%-0.04% vanadium during steelmaking in the converter smelting step can improve the low-temperature impact resistance of the alloy bars, which may be related to the fact that the addition of the microalloying element vanadium can refine the grain size of the structure, improve the strength and toughness of the alloy bars, and thus improve the low-temperature impact resistance of the alloy bars.
[0101] Combining the performance test data of the alloy bars of Example 9 and Example 12, it is found that the tensile strength and yield strength of the alloy bar obtained in Example 12 after overall quenching and tempering are 780MPa and 575MPa respectively, which has high strength, and the -20°C impact energy KV2 can reach 45J, indicating that the narrow component control technology is adopted in the LF refining step, carbon is controlled at ±0.01%, manganese and chromium are controlled at ±0.02%, and the low-temperature impact resistance of the alloy bar can be improved. It may be related to the narrow component control technology adopted in LF refining, the precise control of the composition of various alloy elements in the alloy bar, the reduction of fluctuations, the control of carbon at ±0.01%, the control of manganese and chromium at ±0.02%, and the improvement of the stability of raw material performance.
[0102] Combining the performance test data of the alloy bars of Example 12 and Example 13, it is found that the alloy bar obtained in Example 13 has a tensile strength and a yield strength of 783MPa and 578MPa respectively after overall quenching and tempering, which has a relatively high strength, and the impact energy KV2 at -20°C can reach 46J, indicating that in the VD vacuum step, after vacuum treatment, soft blowing of molten steel under the condition of argon flow rate of 60Nl / min can improve the low-temperature impact resistance of the alloy bar. This may be related to the fact that soft blowing of molten steel can promote the floating of small particle inclusions and improve the purity of steel.
[0103] Combining the performance test data of the alloy bars of Example 13 and Example 14, it is found that the tensile strength and yield strength of the alloy bar obtained in Example 14 after overall quenching and tempering are 786MPa and 581MPa respectively, which has high strength, and the impact energy KV2 at -20℃ can reach 48J, indicating that in the large square billet continuous casting step, controlling the superheat of the molten steel tundish at 30℃ and the billet casting speed at 0.9m / min can improve the low-temperature impact resistance of the alloy bar. It may be related to controlling the argon flow rate at 40-80Nl / min, which can improve the effect of removing inclusions, improve the purity of the alloy bar, and thus improve the strength and low-temperature impact resistance of the alloy bar.
[0104] Combining the performance test data of the alloy bars of Example 14 and Example 15, it is found that the tensile strength and yield strength of the alloy bar obtained in Example 15 after overall quenching and tempering are 790MPa and 585MPa respectively, which has high strength, and the -20℃ impact energy KV2 can reach 52J, indicating that the low-temperature impact resistance of the alloy bar can be improved by putting the rolled material into the pit, laying the pad below, and covering the cover plate on the top in the pit slow cooling step. It may be related to the fact that the rolled material is put into the pit for slow cooling, laying the pad below, and covering the cover plate on the top, which can reduce the influence of the formed "hot zone" and "cold zone" on the process accuracy and performance uniformity and reliability of the rolled material, and improve the hardness of the alloy bar.
[0105] Combining the performance test data of the alloy bars of Example 15 and Example 16-17, it is found that the tensile strength and yield strength of the alloy bars obtained in Example 16-17 after overall quenching and tempering are lower than those in Example 15, and the -20°C impact energy KV2 is also lower than that in Example 15, indicating that during billet rolling, 9 reciprocating rolling passes with a maximum reduction of 90 mm can improve the low-temperature impact resistance of the alloy bars. This may be related to the use of large reduction to improve the grain size crushing ability, refine the grain size of the organization, and improve the impact performance of the raw materials.
[0106] Combining the performance test data of the alloy bars of Example 15 and Example 18, it is found that the tensile strength and yield strength of the alloy bar obtained in Example 18 after overall quenching and tempering are lower than those of Example 15, and the -20°C impact energy KV2 is also lower than that of Example 15, indicating that the pit entry temperature of 500°C and the cooling rate of 7°C / h can improve the low-temperature impact resistance of the alloy bar. This may be related to the fact that the pit entry temperature is controlled at ≥500°C, which can avoid internal cracking of the alloy bar and improve the qualified rate of subsequent flaw detection, and the cooling rate is 6-8°C / h, which reduces the organizational stress and thermal stress generated during the cooling process and avoids the generation of surface and internal cracks on the ingot.
[0107] Combining the performance test data of the alloy bars of Comparative Examples 1-3 with that of Example 1, it is found that adding chromium, silicon and molybdenum elements to the alloy bars can improve the low-temperature impact resistance of the alloy bars.
[0108] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A high-strength low-temperature impact-resistant alloy bar, characterized in that: The alloy rod is composed of the following elemental components in percentage by weight: carbon 0.34-0.38%, silicon 0.17-0.37%, manganese 0.80-1.00%, chromium 0.80-1.20%, molybdenum 0.15-0.25%, aluminum 0-0.002%, vanadium 0-0.04%, phosphorus ≤0.020%, sulfur ≤0.020%, and the balance is iron and unavoidable impurities; and the preparation method of the alloy rod comprises the following steps: Converter smelting: put molten iron and scrap steel into the converter, blow, add aluminum bars for strong deoxidation before tapping, alloy in the ladle after deoxidation, control the aluminum content at the station to 0.020-0.050%; add 0.03-0.04% vanadium when tapping; LF refining: CaO-Al2O3-SiO2 slag system is used, the binary basicity CaO / SiO2 is controlled at 4-8, the ladle is argon-blown, the slag is treated, heated, and the argon blowing is stopped. The basicity of the slag after refining is 5-10, and the white slag retention time is ≥15min; the narrow composition control technology is used in this step, carbon is controlled at ±0.01%, and manganese and chromium are controlled at ±0.02%; VD vacuum: deep vacuum degree ≤67Pa, vacuum maintenance time ≥15min, feed calcium-silicon wire, perform overall quenching and tempering, perform soft blowing, soft blowing time ≥15min, stand for 20-35min; after vacuum treatment, maintain soft blowing of molten steel under the condition of argon flow rate of 40-80Nl / min; Bloom continuous casting: control the superheat of molten steel in the tundish at 20-35°C and the billet drawing speed at 0.80-1.0m / min; Billet heating: Heat the billet, the preheating section temperature is ≤850℃, the heating section temperature is 1200-1280℃, the soaking section temperature is 1210-1270℃, the rolling start temperature is 1150±30℃, and the total heating time is ≥300min; Billet rolling: 9 passes of reciprocating rolling, maximum reduction 80-90mm; sawing and collecting; Slow cooling after entering the pit: the rolled material enters the pit, with a pad underneath and a cover plate on top. The pit entry temperature is ≥500℃, the cooling rate is 6~8℃ / h, and the pit exit temperature is ≤100℃; Combined flaw detection: using magnetic flux leakage and ultrasonic combined flaw detection method.
Citation Information
Patent Citations
Manufacturing method of ultralow-temperature-impact resistant steel for high-intensity bolt of wind turbine generator set
CN107299278A
DEEP DRAWABLE STEEL PLATE WITH TENSILE STRENGTH 1100 MPa FOR APPLICATION AT LOW TEMPERATURE AND HIGH PRESSURE VESSEL, AND MANUFACTURING METHOD THEREOF
KR1020030055537A