Light-controlled terahertz wave modulation chip based on tellurium nanowires and preparation method thereof

By using a 1D/2D mixed-dimensional homogeneous junction of tellurium nanowires and tellurium nanofilms in an optically controlled terahertz wave modulation chip, the unique optoelectronic properties of the tellurium material are used to solve the problem of slow modulation rate in the existing technology and achieve The combination of high modulation depth and fast modulation speed is suitable for industrial production.

CN116560115BActive Publication Date: 2024-10-18CAPITAL NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310207924.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-27
Publication Date
2024-10-18
Estimated Expiration
2043-02-27

AI Technical Summary

Technical Problem

The modulation rate of existing optically controlled terahertz wave modulation chips is relatively slow, which limits its development in optoelectronic devices.

Method used

Using a light-controlled terahertz wave modulation chip based on tellurium nanowires, a tellurium nanowire film is formed on an insulating substrate and combined with a tellurium nanofilm to achieve a 1D/2D mixed-dimensional homojunction. The unique optoelectronic properties of tellurium materials are used to improve Modulate depth and speed.

Benefits of technology

It achieves broadband modulation at lower pump laser power, with large modulation depth, high sensitivity, and fast modulation speed, which is suitable for large-scale industrial production. The modulation depth reaches 94% at 100mW, and the modulation speed remains at the picosecond level.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116560115B_ABST
    Figure CN116560115B_ABST
Patent Text Reader

Abstract

The present invention provides a light-controlled terahertz wave modulation chip based on tellurium nanowires, and a preparation method thereof. The light-controlled terahertz wave modulation chip based on tellurium nanowires comprises: an insulating substrate, which does not generate carriers after light excitation and is transparent to terahertz waves; a tellurium nanowire film formed on the insulating substrate. Compared with other light-controlled terahertz wave modulation films, such as MoTe2 films, the tellurium nanowire film of the present invention can achieve broadband modulation, large modulation depth and high sensitivity under lower pump laser power; at the same time, it has low preparation cost and high precision, and is more suitable for large-scale industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of optoelectronic technology, and in particular to a light-controlled terahertz wave modulation chip based on tellurium nanowires, and a preparation method thereof. Background Art

[0002] Terahertz (THz) waves have broadband, low photon energy and fingerprint characteristics, and are widely used in wireless communications, imaging, biomedicine and other fields. However, the lack of excellent optoelectronic devices has limited the development of THz wave technology to a certain extent. Two-dimensional (2D) materials have unique physical properties, such as tunable band structures, atomic film thickness, strong light-matter interaction, and fast carrier recombination, which provide an interesting platform for studying the interaction between light and matter in basic physics and important device concepts.

[0003] In the process of realizing the present invention, the applicant discovered that the optically controlled terahertz wave modulation chip of the prior art has a high modulation depth but a relatively slow modulation rate, which affects its development in optoelectronic devices. Summary of the invention

[0004] 1. Technical issues to be resolved

[0005] In view of this, the present invention is intended to at least partially solve one of the above technical problems.

[0006] (II) Technical solution

[0007] In a first aspect of the present invention, a light-controlled terahertz wave modulation chip based on tellurium nanowires is provided, comprising: an insulating substrate that does not generate carriers after light excitation and through which terahertz waves can pass; and a tellurium nanowire film formed on the insulating substrate.

[0008] In some embodiments of the present invention, the thickness of the tellurium nanowire film is between 1 nm and 200 nm, wherein the length of the tellurium nanowire is between 100 nm and 5000 nm.

[0009] In some embodiments of the present invention, the present invention further comprises: a tellurium nanofilm formed on an insulating substrate, with a thickness ranging from 1 nm to 1000 nm; wherein the tellurium nanowire film is formed on the tellurium nanofilm.

[0010] In some embodiments of the present invention, the tellurium nanofilm has a thickness between 1 nm and 200 nm.

[0011] In some embodiments of the present invention, the insulating substrate is a quartz substrate or a sapphire substrate.

[0012] In a second aspect of the present invention, a method for preparing the above optically controlled terahertz wave modulation chip is provided, comprising:

[0013] Step A, preparing an insulating substrate;

[0014] Step C, forming a tellurium nanowire thin film on an insulating substrate.

[0015] In some embodiments of the present invention, step C includes: sub-step C1, preparing a tellurium nanowire solution; sub-step C2, drop-coating the tellurium nanowire solution on an insulating substrate, and forming a tellurium nanowire thin film on the insulating substrate after the solvent of the tellurium nanowire solution evaporates.

[0016] In some embodiments of the present invention, in sub-step C1, a tellurium nanowire solution is prepared by electrodeposition, including: a solution containing TeO2 and KOH is prepared as an electrolyte, and a three-electrode system is used in an electrochemical workstation: the working electrode is a copper sheet, the counter electrode is a platinum sheet, and the reference electrode is a Hg / HgO electrode, and the deposition is performed under the conditions of an overpotential of -1.8V and a temperature of 85°C. After the reaction is complete, the solution is allowed to stand, an acidic solution is added to neutralize it, and then washed with deionized water to obtain a tellurium nanowire solution; or

[0017] In some embodiments of the present invention, in sub-step C1, the tellurium nanowire solution is prepared by using an Al foil replacement method, including: placing the Al foil in a solution containing TeO2 and KOH at room temperature to undergo a replacement reaction. After the reaction is complete, the solution is allowed to stand, an acid solution is added to neutralize the solution, and the solution is washed with deionized water to obtain a tellurium nanowire solution.

[0018] In some embodiments of the present invention, the method further includes: step B, forming a tellurium nanofilm on an insulating substrate; and step C includes: forming a tellurium nanowire film on the tellurium nanofilm.

[0019] In some embodiments of the present invention, in step B, magnetron sputtering or electron beam evaporation is used to form a tellurium nanofilm on an insulating substrate.

[0020] (III) Beneficial effects

[0021] It can be seen from the above technical solution that the present invention has at least one of the following beneficial effects compared with the prior art:

[0022] (1) Tellurium materials have a unique spiral chain structure that produces high carrier mobility at room temperature. They also have excellent properties such as narrow band gap, strong optical response, and environmental stability, resulting in strong light absorption and ultrafast charge carrier transport.

[0023] Therefore, compared with other optically controlled terahertz wave modulation films, such as MoTe 2Thin film, tellurium nanowire film can achieve broadband modulation, large modulation depth and high sensitivity under lower pump laser power; at the same time, the preparation cost is low and the precision is high, which is more suitable for large-scale industrial production.

[0024] (2) The hybrid dimensional optically controlled terahertz wave modulation chip includes: two tellurium films of different dimensions. Tellurium elements of different dimensions realize different functions. 1D tellurium nanowires have different sizes obtained by different preparation methods and can be prepared according to the requirements of use, which is highly flexible. 2D tellurium nanofilms achieve low-power excitation thresholds in the broadband terahertz band of 0.2THz-2.0THz and obtain high modulation at high power while still maintaining ultrafast characteristics, combining the advantages of fast modulation speed and large modulation depth.

[0025] Heterojunctions have some disadvantages that cannot be ignored, such as chemical mixing, grain boundaries, lattice mismatch, and discontinuous band arrangement, which lead to a large number of carrier scattering and capture centers at the heterojunction interface, thereby reducing the interface charge transfer efficiency and ultimately affecting the overall performance of the device. Experiments have shown that at 100mW, the modulation depth of the tellurium nanowire / tellurium nanofilm hybrid van der Waals homojunction optically controlled terahertz wave modulation chip is enhanced to 94%, indicating that there is a strong interlayer coupling between tellurium of different dimensions, and the lattice mismatch of the same element material is ignored, which further improves the performance of the optically controlled terahertz wave modulation chip.

[0026] (3) Experiments have shown that the hybrid-dimensional optically controlled terahertz wave modulation system of the present invention achieves an ultra-high modulation depth while maintaining a modulation speed in the picosecond range. In particular, the tellurium nanowire / tellurium nanofilm achieves an ultra-high modulation depth of 94% at a pump power of 100mW, while maintaining a modulation speed in the picosecond range, which is also the maximum modulation in the current terahertz hybrid-dimensional van der Waals homojunction all-optical modulation device. This means that the hybrid-dimensional homojunction of tellurium can effectively increase the modulation depth while maintaining a fast modulation speed, and achieve simultaneous optimization of multiple device parameters. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1A FIG. 4 is a cross-sectional schematic diagram of a first embodiment of the optically controlled terahertz wave modulation chip of the present invention.

[0028] Figure 1B The figure is a flow chart of a method for preparing the optically controlled terahertz wave modulation chip shown in FIG1 .

[0029] Figure 2A and Figure 2B These are the SEM images of light-controlled terahertz chips made from tellurium nanowire solutions using electrodeposition and Al foil replacement methods, respectively.

[0030] Figure 3A and Figure 3BThe relative change of the terahertz peak transmittance of the light-controlled terahertz chip prepared by the tellurium nanowire solution prepared by the electrodeposition method and the Al foil replacement method as a function of the pump delay time between the pump pulse and the terahertz pulse.

[0031] Figure 4A FIG. 4 is a cross-sectional schematic diagram of a second embodiment of the optically controlled terahertz wave modulation chip of the present invention.

[0032] Figure 4B For preparation Figure 4A Flow chart of the method for optically controlling terahertz wave modulation chip.

[0033] Figure 5 for Figure 4A The relative change of the terahertz peak transmittance of the tellurium nanofilm in the optically controlled terahertz wave modulation chip at different powers with a pump wavelength of 800nm ​​is a function of the delay time between the pump and terahertz pulses.

[0034] Fig. 6A and Figure 6B They are Figure 4A The Raman spectrum and XRD pattern of the tellurium nanostructure in the optically controlled terahertz wave modulation chip are shown.

[0035] Figure 7 for Figure 4A The experimental curves of modulation depth of the optically controlled terahertz wave modulation chip shown in FIG. 1 are shown in FIG. 1 and FIG. 1 are shown in FIG. 1 .

[0036] Figure 8 for Figure 4A Schematic diagram of the modulation depth of the optically controlled terahertz wave modulation chip changing with pump power.

[0037] Fig. 9 FIG. 4 is a schematic diagram of an embodiment of a light-controlled terahertz wave modulation system according to the present invention. DETAILED DESCRIPTION

[0038] The present invention provides a light-controlled terahertz wave modulation chip based on tellurium nanowires, and on this basis provides a light-controlled terahertz wave modulation chip including a 1D / 2D mixed-dimensional homojunction of tellurium. Relying on the unique optoelectronic properties of tellurium materials, the present invention integrates the two advantages of high flexibility of 1D tellurium nanowires and fast modulation speed and large modulation depth of 2D tellurium nanofilms, and has greater advantages than other light-controlled terahertz wave modulation chips.

[0039] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in combination with specific embodiments and with reference to the accompanying drawings. However, it should be understood by those skilled in the art that no matter how the description order is, the technical contents of each part of the present invention are universal without conflict, and the technical features described in one embodiment can also be applied to other embodiments.

[0040] 1. Light-controlled terahertz wave modulation chip based on tellurium nanowires

[0041] The present invention firstly provides a light-controlled terahertz wave modulation chip based on tellurium nanowires. Figure 1A FIG. 1 is a cross-sectional schematic diagram of the first embodiment of the optically controlled terahertz wave modulation chip of the present invention. Figure 1A As shown, the optically controlled terahertz wave modulation chip of this embodiment includes: an insulating substrate 11, which does not generate carriers after optical excitation and is transparent to terahertz waves; and a tellurium nanowire film (TeNano-Wires, TeNW for short) 13, formed on the insulating substrate.

[0042] In this embodiment, the insulating substrate 11 is a double-sided polished quartz substrate. The use of quartz material as a wide bandgap insulating substrate is mainly based on the advantages that the carriers of quartz are not easily excited and the processing methods based on quartz materials are more mature. Its transmittance in the terahertz band is 60% to 70%. Those skilled in the art should understand that in addition to quartz substrates, other types of wide bandgap insulating substrates such as sapphire wafers can also be used, as long as no carriers are generated after light excitation and the terahertz wave is transparent.

[0043] In this embodiment, the thickness of the tellurium nanowire film 13 is between 1 nm and 200 nm, wherein the length of the tellurium nanowire is between 100 nm and 5000 nm.

[0044] Figure 1B The flowchart of the method for preparing the optically controlled terahertz wave modulation chip shown in FIG1 is shown in FIG1. Figure 1B As shown, the preparation method comprises:

[0045] Step A, preparing an insulating substrate 11;

[0046] In this embodiment, a double-sided polished quartz substrate is used.

[0047] Step C: prepare a tellurium nanowire solution, and drop-coat the tellurium nanowire solution on the insulating substrate. After the solvent of the tellurium nanowire solution evaporates, a tellurium nanowire thin film 13 is formed on the insulating substrate.

[0048] Specifically, step C may further include:

[0049] Sub-step C1, preparing a tellurium nanowire solution;

[0050] In the present invention, two methods for preparing tellurium nanowire solutions are provided.

[0051] (1) Electrodeposition

[0052] The preparation contained 10 mM TeO 2 The solution of 1M KOH was used as the electrolyte, and a three-electrode system was used in the electrochemical workstation for preparation: the working electrode was a copper sheet, the counter electrode was a platinum sheet, and the reference electrode was a Hg / HgO electrode. The deposition was performed at an overpotential of -1.8V and a temperature of 85°C. After the reaction was complete, it was allowed to stand, HCl was added for neutralization, and then washed with deionized water to obtain a solution containing tellurium nanowires with a length of 500nm to 1000nm.

[0053] (2) Al foil replacement method

[0054] At room temperature, the Al foil was placed in a solution containing 10 mM TeO 2 After the reaction is complete, the solution is allowed to stand, and then HCl solution is added to neutralize the solution, and then washed with deionized water to obtain a solution containing tellurium nanowires with a length of 2000nm to 2500nm.

[0055] In actual production, those skilled in the art may choose one of the above two methods. Of course, other known methods in the field may also be used, which will not be described in detail here.

[0056] Sub-step C2, forming a tellurium nanowire thin film on a quartz substrate by a drop coating method;

[0057] The prepared tellurium nanowire solution was drop-coated on a quartz substrate and allowed to stand at room temperature for 40 minutes to form a black tellurium nanowire thin film layer with structural stability and ease of preparation.

[0058] Figure 2A and Figure 2B Scanning electron microscope (SEM) images of light-controlled terahertz chips made from tellurium nanowire solutions using electrodeposition and Al foil replacement methods, respectively. Figure 2A and Figure 2B It can be seen that tellurium nanowires are formed on the surface of the quartz substrate. The tellurium nanowires prepared by electrodeposition are denser but shorter, while the tellurium nanowires prepared by Al foil replacement are sparser but longer.

[0059] Figure 3A and Figure 3B The relative change of the terahertz peak transmittance of the light-controlled terahertz chip prepared by the tellurium nanowire solution prepared by the electrodeposition method and the Al foil replacement method as a function of the pump delay time between the pump pulse and the terahertz pulse.

[0060] Figure 3A and Figure 3B In the experiment, the pump laser wavelength is 800nm, and the functional relationship is defined as the transient time response, which consists of three stages with different time scales. First, the pump causes the peak transmittance of the terahertz wave to drop rapidly within a few picoseconds, which originates from the generation of hot electrons. After that, the rapid recovery process is about tens of picoseconds, that is, the charge carriers cool down. Subsequently, the slow recovery lasts for about a few hundred picoseconds and returns to the initial state. By comparison, it is found that the carrier lifetime of tellurium nanowires produced by the Al foil replacement method is shorter, which is more suitable for the production of ultrafast devices. Therefore, in the subsequent embodiments, the tellurium nanowire solution is prepared by the Al foil replacement method.

[0061] Those skilled in the art should understand that tellurium materials have a unique spiral chain structure, high carrier mobility at room temperature, and excellent properties such as narrow band gap, strong optical response, and environmental stability, which can produce strong light absorption and ultrafast charge carrier transport. Therefore, compared with other light-controlled terahertz wave modulation films, such as MoTe 2 Thin film, tellurium nanofilm can achieve broadband modulation, large modulation depth and high sensitivity under lower pump laser power; at the same time, the preparation cost is low and the precision is high, which is more suitable for large-scale industrial production.

[0062] 2. Hybrid-dimensional homojunction optically controlled terahertz wave modulation chip

[0063] On the basis of the above embodiments, the present invention further provides a hybrid-dimensional optically controlled terahertz wave modulation chip. Figure 4A FIG. 2 is a cross-sectional schematic diagram of a second embodiment of the optically controlled terahertz wave modulation chip of the present invention. Figure 4A As shown, the optically controlled terahertz wave modulation chip of this embodiment includes: an insulating substrate 11, which does not generate carriers after optical excitation and is transparent to terahertz waves; a tellurium nanofilm (Te Nano-Film, TeNF for short) 12, formed on the insulating substrate, with a thickness between 1nm and 1000nm; a tellurium nanowire film (Te Nano-Wires, TeNW for short) 13, formed on the tellurium nanofilm.

[0064] In this embodiment, the insulating substrate 11 is a double-sided polished quartz substrate. The use of quartz material as a wide bandgap insulating substrate is mainly based on the advantages that the carriers of quartz are not easily excited and the processing methods based on quartz materials are more mature. Its transmittance in the terahertz band is 60% to 70%. Those skilled in the art should understand that in addition to quartz substrates, other types of wide bandgap insulating substrates such as sapphire wafers can also be used, as long as no carriers are generated after light excitation and the terahertz wave is transparent.

[0065] In this embodiment, the thickness of the tellurium nanowire film 13 is between 1 nm and 200 nm, wherein the length of the tellurium nanowire is between 100 nm and 5000 nm.

[0066] In this embodiment, the tellurium nanofilm 12 has a thickness of 100 nm and is formed by electron beam evaporation.

[0067] Figure 4B For preparation Figure 4A The flowchart of the method for optically controlling terahertz wave modulation chip is shown in FIG. Figure 4B As shown, the preparation method comprises:

[0068] Step A, preparing an insulating substrate 11;

[0069] Step B, forming a tellurium nanofilm 12 on an insulating substrate;

[0070] For step B, in this embodiment, the tellurium nanofilm is formed on a double-polished quartz substrate by electron beam evaporation. During the electron beam evaporation process, the evaporation chamber is evacuated to a vacuum of more than 10 -4 After Pa, electron beam evaporation is performed, and the evaporation deposition rate is not higher than 0.1nm / s. After the tellurium thin film is deposited, the evaporation chamber is maintained in vacuum and annealed at 100°C for half an hour in situ.

[0071] In addition, the applicant also uses magnetron sputtering to prepare tellurium nanofilm 12. When magnetron sputtering is used, the vacuum in the sputtering chamber is higher than 10 -4 After the argon gas with a purity of 99.999% was introduced for magnetron sputtering, and the sputtering speed was not higher than 0.1 nm / s.

[0072] The test results show that the optically controlled terahertz wave modulation chips prepared by electron beam evaporation and magnetron sputtering can meet the requirements of practical applications, and the performance of the chips prepared by electron beam evaporation is better.

[0073] Step C: prepare a tellurium nanowire solution, and drop-coat the tellurium nanowire solution on the tellurium nanofilm. After the solvent of the tellurium nanowire solution evaporates completely, a tellurium nanowire film 13 is formed on the tellurium nanofilm.

[0074] It has been demonstrated in the previous embodiment that the tellurium nanowires prepared by the Al foil replacement method have better modulation performance for terahertz waves than those prepared by the electrodeposition method. Therefore, in this embodiment, the Al foil replacement method is used to prepare the tellurium nanowire solution.

[0075] Specifically, step C1 may further include:

[0076] Sub-step C1, preparing a tellurium nanowire solution by using an Al foil replacement method;

[0077] At room temperature, the Al foil was placed in a solution containing 10 mM TeO 2 A replacement reaction occurs in a solution of 1M KOH; after the reaction is complete, the solution is allowed to stand, an HCl solution is added to neutralize the solution, and the solution is washed with deionized water to obtain a solution containing tellurium nanowires with a length of 2000nm to 2500nm.

[0078] Sub-step C2, forming a tellurium nanowire film 13 on the tellurium nanofilm 12 by using a drop coating method

[0079] 15 μL of the tellurium nanowire solution was directly dropped onto the prepared tellurium nanofilm with a thickness of 100 nm to form a uniform black film, which was then placed on a horizontal surface to dry naturally to form a tellurium nanowire film 13 .

[0080] Of course, those skilled in the art can adjust the experimental parameters according to actual needs.

[0081] In the present invention, the mixed-dimensional homojunction optically controlled terahertz wave modulation chip includes: two tellurium films of different dimensions. Te elements of different dimensions realize different functions. 1D tellurium nanowires have different sizes under different preparation methods and can be prepared according to the use requirements, which is highly flexible. 2D tellurium nanofilm (TeNF) achieves a low-power excitation threshold in the broadband terahertz band with an operating frequency of 0.2THz-2.0THz and obtains high modulation at high power while still maintaining ultrafast characteristics, combining the two advantages of fast modulation speed and large modulation depth.

[0082] Heterojunctions have some disadvantages that cannot be ignored, such as chemical mixing, grain boundaries, lattice mismatch, and discontinuous band arrangement, which leads to a large number of carrier scattering and capture centers at the heterojunction interface, thereby reducing the efficiency of interface charge transfer and ultimately affecting the overall performance of the device. However, homojunctions have great prospects in new electronic and optoelectronic devices due to their unique structure and properties, such as homogeneous composition, perfect lattice matching, and efficient interface charge transfer. Since tellurium constitutes a 1D / 2D mixed-dimensional van der Waals homojunction, it can accelerate the transfer of free charges and promote the separation and migration of photogenerated carriers, thus bringing great advantages to terahertz wave modulation. At the same time, experiments have also proved that there is a strong interlayer coupling between tellurium of different dimensions, which further improves the performance of the light-controlled terahertz wave modulation chip, which will be explained in more detail below.

[0083] Figure 5 for Figure 4A The relative change of the terahertz peak transmittance of the tellurium nanofilm in the optically controlled terahertz wave modulation chip at different powers with a pump wavelength of 800nm ​​is a function of the delay time between the pump and terahertz pulses. Figure 5 In the figure, tellurium nanofilm is represented by TeNF.

[0084] Depend on Figure 5 It can be seen that the functional relationship still consists of three stages with different time scales. First, the pump light causes the terahertz amplitude to drop rapidly within a few picoseconds, which originates from the generation of hot electrons. After that, the fast recovery process is about 2 picoseconds, which is when the charge carriers begin to cool. Subsequently, the slow recovery lasts for about 8 picoseconds and returns to the initial state. In particular, the relaxation times of both the fast and slow components show independence of the pump injection amount, indicating that the synergy between defect capture and the Auger effect dominates the photocarrier dynamics in tellurium films, which is conducive to the realization of ultrafast devices. The modulation speed is not deteriorated by the increase of pump power and is not affected by external conditions.

[0085] Fig. 6A and Figure 6B They are Figure 4A The Raman spectrum and XRD pattern of the tellurium nanostructure in the optically controlled terahertz wave modulation chip are shown. In the figure, the tellurium nanowire prepared by electrodeposition is represented by TeNW (85°C), the tellurium nanowire prepared by Al foil replacement is represented by TeNW (Al), and TeNF represents the tellurium nanofilm.

[0086] It is well known that the optical properties of homojunctions are closely related to the material composition and its interface. Homojunctions in a single material can effectively improve the separation and transfer capabilities of carriers. Tellurium has excellent properties such as carrier mobility in single-element materials. Fig. 6A The Raman properties of different tellurium nanostructures were compared. The three characteristic Raman peaks of tellurium nanowires (TeNW(Al)) prepared by Al foil replacement method are closer to those of tellurium nanofilms (TeNF). Figure 6B X-ray diffraction (XRD) patterns of different tellurium nanostructures and standard PDF cards are shown. The typical peaks of tellurium nanowires (TeNW(Al)) and tellurium nanofilms (TeNF) prepared by Al foil replacement method are (100) and (101) planes, which can achieve perfect crystal plane matching.

[0087] Figure 7 for Figure 4A The experimental curves of modulation depth of the optically controlled terahertz wave modulation chip under different modulation powers are shown. The optically controlled terahertz wave modulation chip includes both tellurium nanofilm and tellurium nanowire film, which are expressed as TeNW(Al) / TeNF. Figure 7 As shown in the figure, the modulation depth increases rapidly with the increase of pump power, and the modulation depth reaches 94% at 100mW, achieving an ultra-high modulation depth. Compared with tellurium nanowires, the hybrid van der Waals homojunction significantly improves the modulation depth and significantly accelerates the modulation speed. This is due to the natural matching of its chemical and electronic structures, which contributes to efficient interface charge transfer within the interface.

[0088] In this embodiment, the modulation depth is defined as the maximum value of the transient time response. Figure 8 for Figure 4A Schematic diagram showing the modulation depth of the optically controlled terahertz wave modulation chip changing with pump power. Figure 8 As shown in the figure, the modulation depth of tellurium nanowire (TeNW(Al)) / tellurium nanofilm (TeNF) can reach 80% at a pump power of 50mW, and a modulation depth of 94% can be obtained at 100mW, which is almost fully modulated. This is attributed to the homogeneous composition, perfect lattice matching and strong interlayer coupling between tellurium nanowire (TeNW(Al)) and tellurium nanofilm (TeNF).

[0089] 3. Optically controlled terahertz wave modulation system

[0090] Based on the above optically controlled terahertz wave modulation chip, the present invention also provides an optically controlled terahertz wave modulator and an optically controlled terahertz wave modulation system. Fig. 9 Schematic diagram of an embodiment of the optically controlled terahertz wave modulation system according to the present invention. Fig. 9 , the modulator and modulation system are introduced together.

[0091] Please refer to Fig. 9 The optically controlled terahertz wave modulator of the present invention comprises:

[0092] The optically controlled terahertz wave modulation chip as described in the above embodiment, wherein a tellurium nanofilm 12 and a tellurium nanowire film 13 are sequentially deposited on a quartz substrate 11;

[0093] An optical pump source 20, used to generate a pump laser A to irradiate the terahertz wave modulation chip;

[0094] The terahertz wave source 31 and the terahertz wave detector 32 are arranged opposite to each other, wherein the terahertz wave source 31 is located on the film side of the optically controlled terahertz wave modulation chip; and the terahertz wave detector 32 is located on the substrate side of the optically controlled terahertz wave modulation chip.

[0095] The optically controlled terahertz wave modulation chip 10 in this embodiment may be the optically controlled terahertz wave modulation chip in the first embodiment or the optically controlled terahertz wave modulation chip in the second embodiment of the present invention, both of which can implement the present invention.

[0096] Preferably, the second embodiment of the optically controlled terahertz wave modulation chip, i.e., the optically controlled terahertz wave modulation chip, is used in this embodiment, comprising: an insulating substrate 11, which does not generate carriers after optical excitation and is transparent to terahertz waves; a tellurium nanofilm 12, formed on the insulating substrate, with a thickness between 1nm and 1000nm; a tellurium nanowire film 13, formed on the tellurium nanofilm, with a thickness between 1nm and 200nm, wherein the length of the tellurium nanowire is between 100nm and 5000nm. The tellurium nanofilm 12 is a film formed by magnetron sputtering or electron beam evaporation; the tellurium nanowire film 13 is a film formed by a tellurium nanowire solution by drop coating.

[0097] The terahertz wave source 31 is a generating circuit in the optical pump-terahertz detection (OPTP) system, which emits a terahertz wave B. The terahertz detector 32 is used to receive the terahertz signal of the terahertz wave source 31 through the mixed vanadium-telluride material. The terahertz wave B emitted by the terahertz wave source 31 passes through the optically controlled terahertz wave modulation chip and is detected by the terahertz wave detector 32, and the pump laser A generated by the optical pump source 20 is used to modulate the terahertz wave passing through the optically controlled terahertz wave modulation chip 10.

[0098] Working principle: When an optical pump source with a wavelength of 800nm ​​acts on the hybrid tellurium material on the quartz substrate, including tellurium nanofilm and tellurium nanowire layer, the terahertz wave is actively regulated due to the high mobility and strong light absorption of the material and the ultrafast charge transfer characteristics inside.

[0099] Experiments have shown that the hybrid-dimensional optically controlled terahertz wave modulation system of this embodiment achieves ultra-high modulation depth, while the modulation speed is kept in the picosecond level. In particular, the tellurium nanowire / tellurium nanofilm achieves an ultra-high modulation depth of 94% at a pump power of 100mW, while the modulation speed is in the picosecond level, which is also the maximum modulation in the current terahertz hybrid-dimensional van der Waals homojunction all-optical modulation device. This means that the hybrid-dimensional homojunction of tellurium can effectively increase the modulation depth while maintaining a fast modulation speed, and realize the simultaneous optimization of multiple parameters of the device.

[0100] So far, the various embodiments of the present invention have been introduced.

[0101] In summary, the optically controlled terahertz wave chip and system of the present invention rely on the unique optoelectronic properties of tellurium materials, and integrate the two advantages of high flexibility of one-dimensional tellurium nanowires and fast modulation speed and large modulation depth of two-dimensional tellurium nanofilms. Compared with other optically controlled terahertz wave modulation chips, it has greater advantages and good application prospects.

[0102] It should be noted that for certain implementations, if they are not the key content of the present invention and are well known to ordinary technicians in the relevant technical field, they are not described in detail in the drawings or the body of the specification. In this case, they can be understood by referring to the relevant prior art. The above part has described the embodiments of the present invention in as much detail as possible in combination with the drawings. Based on the above description, those skilled in the art should have a clear understanding of the present invention.

[0103] Unless expressly indicated to the contrary, the numerical parameters in the specification and claims of the present invention may be approximate values ​​and can be changed according to the content of the present invention. Specifically, all the numbers recorded in the specification and claims indicating the content of the composition, reaction conditions, etc., should be understood to be modified by the term "about" in all cases, and the meaning of the expression is to include the change of ±10% in some embodiments, ±5% in some embodiments, ±1% in some embodiments, and ±0.5% in some embodiments by the specific number.

[0104] It is to be understood that the present invention can be implemented in many different forms and should not be construed as being limited to the embodiments described herein. In addition, the above definitions of each element and method are not limited to the various specific structures, shapes or modes mentioned in the embodiments, and those of ordinary skill in the art may simply modify or replace them.

[0105] Similarly, it should be understood that the various features of the present invention are sometimes grouped together into a single embodiment, figure, or description thereof. However, the method of the invention should not be interpreted as reflecting the following intention: the claimed invention requires more features than those explicitly stated in each claim. More specifically, as reflected in the claims, each inventive aspect consists in less than all the features of the previous single embodiment. Moreover, the embodiments can be mixed and matched with each other or with other embodiments based on design and reliability considerations, that is, the technical features in different embodiments can be freely combined to form more embodiments. Therefore, the claims following the specific embodiment are hereby explicitly incorporated into the specific embodiment, wherein each claim itself serves as a separate embodiment of the present invention.

[0106] The above specific embodiments provide a detailed description of the objectives, technical means and beneficial effects of the present invention. It should be understood that the purpose of the detailed description is to enable those skilled in the art to understand the present invention more clearly, and it is not used to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A light-controlled terahertz wave modulation chip based on tellurium nanowires, characterized in that: include: an insulating substrate, which does not generate carriers after photoexcitation and through which the terahertz wave is transparent; A tellurium nanofilm is formed on the insulating substrate, and has a thickness between 1 nm and 1000 nm; A tellurium nanowire film is formed on the tellurium nanofilm.

2. The optically controlled terahertz wave modulation chip according to claim 1, characterized in that: The thickness of the tellurium nanowire film is between 1 nm and 200 nm, wherein the length of the tellurium nanowire is between 100 nm and 5000 nm.

3. The optically controlled terahertz wave modulation chip according to claim 1, characterized in that: The tellurium nanofilm has a thickness between 1 nm and 200 nm.

4. The optically controlled terahertz wave modulation chip according to claim 1, characterized in that: The insulating substrate is a quartz substrate or a sapphire substrate.

5. A method for preparing the optically controlled terahertz wave modulation chip according to any one of claims 1 to 4, characterized in that: include: Step A, preparing an insulating substrate; Step B, forming a tellurium nanofilm on the insulating substrate; Step C, forming a tellurium nanowire thin film on the tellurium nanofilm.

6. The preparation method according to claim 5, characterized in that: The step C comprises: Sub-step C1, preparing a tellurium nanowire solution; Sub-step C2, drop-coating the tellurium nanowire solution on the insulating substrate, and after the solvent of the tellurium nanowire solution is completely evaporated, a tellurium nanowire thin film is formed on the insulating substrate.

7. The preparation method according to claim 6, characterized in that: In the sub-step C1, Prepare a tellurium nanowire solution by electrodeposition, including: prepare a solution containing TeO2 and KOH as an electrolyte, use a three-electrode system in an electrochemical workstation for preparation: the working electrode is a copper sheet, the counter electrode is a platinum sheet, and the reference electrode is a Hg / HgO electrode, deposit at an overpotential of -1.8V and a temperature of 85°C, and after the reaction is complete, let it stand, add an acidic solution for neutralization, and then wash with deionized water to obtain a tellurium nanowire solution; or The Al foil replacement method is used to prepare a tellurium nanowire solution, which includes: placing the Al foil in a solution containing TeO2 and KOH at room temperature to undergo a replacement reaction, standing the foil after the reaction is complete, adding an acid solution to neutralize the foil, and then washing the foil with deionized water to obtain a tellurium nanowire solution.

8. The preparation method according to claim 5, characterized in that: In the step B, magnetron sputtering or electron beam evaporation is used to form a tellurium nanofilm on the insulating substrate.