Inserts and cutting tools
By rationally preparing cubic crystal and compressed boron nitride in the boron nitride sintered body blade, combined with the design of the matrix and joining materials, the problem of large wear of the boron nitride sintered body blade is solved, and high wear resistance and high temperature are achieved Hardness, extending blade life and reducing costs.
Patent Information
- Application Number
- CN202180082048.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-12-25
- Filing Date
- 2021-12-15
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-12-15
AI Technical Summary
Existing boron nitride sintered inserts suffer a large amount of wear during the cutting process, which affects their performance.
A boron nitride sintered blade containing cubic boron nitride and compressed boron nitride is used. By controlling the X-ray diffraction intensity ratio and orientation value, the wear resistance and hardness of the blade are improved. Combined with the design of the matrix and joining materials, Reduce the use of high-hardness materials.
Significantly improves the wear resistance and high temperature hardness of the blade, extends the service life of the blade, and reduces production costs.
Smart Images

Figure CN116568434B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to inserts and cutting tools. Background Art
[0002] Boron nitride sintered bodies have high hardness. Taking advantage of this property, boron nitride sintered bodies are used for crushing components and tool blades, etc.
[0003] Patent Document 1 describes a boron nitride sintered body containing cubic boron nitride. Patent Document 1 also describes a cubic boron nitride composite polycrystal containing wurtzite-type boron nitride and having an X-ray diffraction intensity I of the (220) plane of cubic boron nitride. (220) X-ray diffraction intensity I relative to the (111) plane of cubic boron nitride (111) Ratio I (220) / I (111) In other words, in the orientation plane of the cubic boron nitride composite polycrystal, I (111) isI (220) More than 10 times of that. That is, it can be said that in the orientation plane, the (111) plane is strongly oriented. This cubic boron nitride composite polycrystal can be obtained using pBN after orientation as a raw material. It is also described that, as a comparative example, when hexagonal boron nitride is included, even if the (111) plane of the cubic boron nitride is strongly oriented in the orientation plane, the wear amount is large and the performance as a cutting tool is poor.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent No. 5929655 Summary of the invention
[0007] A blade according to one embodiment of the present invention comprises a boron nitride sintered body having a first surface, a second surface, and a cutting edge located on at least a portion of the ridges of the first surface and the second surface. The boron nitride sintered body contains cubic boron nitride and compressed boron nitride. In transmission X-ray diffraction of a cross section of the boron nitride sintered body perpendicular to the first surface, the X-ray intensity at the top of the peak of the 111 diffraction of cubic boron nitride in the direction perpendicular to the first surface is denoted as IcBN(111)v, and the X-ray intensity at the top of the peak of the 002 diffraction of compressed boron nitride is denoted as IhBN(002)v, and the X-ray intensity at the top of the peak of the 111 diffraction of cubic boron nitride in the direction parallel to the first surface is denoted as IcBN(111)h, and the X-ray intensity at the top of the peak of the 002 diffraction of compressed boron nitride is denoted as IhBN(002)h. The compressed boron nitride content value represented by (IhBN(002)v+IhBN(002)h) / (IcBN(111)v+IcBN(111)h) is greater than 0.002 and less than 0.01. The cubic orientation value represented by IcBN(111)v / (IcBN(111)v+IcBN(111)h) is greater than 0.5. The compressed boron nitride orientation value represented by IhBN(002)v / (IhBNv(002)+IhBN(002)h) is greater than the cubic orientation value. In addition, the Vickers hardness in the direction perpendicular to the first surface of the boron nitride sintered body is 40.0 GPa or more at 1000°C.
[0008] A cutting tool according to one aspect of the present invention includes: a tool holder having a length extending from a first end to a second end and having a groove on the first end side; and the above-mentioned insert located in the groove. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 This is a perspective view showing an example of the blade of the present invention.
[0010] Figure 2 It is a perspective view showing another example of the blade of the present invention.
[0011] Figure 3 This is a diagram showing an example of the cutting tool of the present invention.
[0012] Figure 4 It is a graph showing the high temperature hardness measurement results. DETAILED DESCRIPTION
[0013] Hereinafter, the mode (hereinafter, described as "embodiment") for implementing the blade and cutting tool of the present invention will be described in detail with reference to the accompanying drawings. Also, the present invention is not limited to this embodiment. In addition, each embodiment can be appropriately combined within the scope that does not conflict with the processing content. In addition, in each of the following embodiments, the same symbols are added to the same parts, and repeated descriptions are omitted.
[0014] In the embodiments shown below, expressions such as "certain", "orthogonal", "perpendicular" or "parallel" are sometimes used, but these expressions do not need to be "certain", "orthogonal", "perpendicular" or "parallel" in a strict sense. That is, the above expressions allow for deviations in manufacturing accuracy, setting accuracy, etc.
[0015] In addition, for the convenience of explanation, each figure referred to below only shows the necessary main parts in a simplified manner.
[0016] There are known inserts made of boron nitride sintered bodies, but such inserts have room for further improvement in terms of improving wear resistance.
[0017] <Blade>
[0018] Figure 1 An example of a blade 1 of the present invention is shown in FIG. Figure 1 In the example shown, the insert 1 is a polygonal boron nitride sintered body 3 . Figure 2 Another example of the blade 1 of the present invention is shown in FIG. Figure 2 3 shows an example in which a boron nitride sintered body 3 is bonded to a substrate 5, for example, made of cemented carbide. The substrate 5 and the boron nitride sintered body 3 together form a polygonal blade. With such a structure, the proportion of the relatively expensive boron nitride sintered body 3 in the blade 1 can be reduced. Figure 2 In the example shown, the boron nitride sintered body 3 is located at one of the multiple corners of the insert 1. The present invention is not limited thereto, and the boron nitride sintered body 3 may be located at two or more corners of the multiple corners of the insert 1.
[0019] A bonding material (not shown) containing, for example, Ti and Ag may be provided between the boron nitride sintered body 3 and the substrate 5. The boron nitride sintered body 3 and the substrate 5 can be integrated via the bonding material using a conventionally known bonding method.
[0020] The boron nitride sintered body 3 has a first surface 7 and a second surface 9. Figure 1 and Figure 2 In the example shown, the first surface 7 is the upper surface of the blade 1, and the second surface is the side surface of the blade 1. Figure 1 and Figure 2 In the example shown, the first surface 7 corresponds to the rake face, and the second surface 9 corresponds to the flank face. Hereinafter, the first surface 7 is sometimes referred to as the rake face 7. In addition, the second surface 9 is sometimes referred to as the flank face 9. The insert 1 has a cutting edge 13 at least in a portion of the ridges of the first surface 7 and the second surface 9.
[0021] The boron nitride sintered body 3 of the insert 1 of the present invention contains cubic boron nitride and compressed boron nitride.
[0022] In the transmission type X-ray diffraction with respect to the cross section perpendicular to the first surface 7 in the boron nitride sintered body 3, among the data obtained, the X-ray intensity of the 111 diffraction of the cubic boron nitride in the direction perpendicular to the first surface 7 is set to IcBN(111)v. In addition, the X-ray intensity of the 002 diffraction of the compression type boron nitride in the direction perpendicular to the first surface 7 is set to IhBN(002)v. In addition, in the transmission type X-ray diffraction with respect to the cross section perpendicular to the first surface 7 in the boron nitride sintered body 3, among the data obtained, the X-ray intensity of the 111 diffraction of the cubic boron nitride in the direction parallel to the first surface 7 is set to IcBN(111)h. In addition, the X-ray intensity of the 002 diffraction of the compression type boron nitride in the direction parallel to the first surface 7 is set to IhBN(002)h.
[0023] In addition, the above-mentioned special designations of each surface are based on JCPDS card No. 01-075-6381 for cubic boron nitride. In addition, for compressed boron nitride, it is based on JCPDS card No. 18-251. For hexagonal boron nitride, it is based on JCPDS card No. 00-045-0893. In addition, for wurtzite boron nitride described later, it is based on JCPDS card No. 00-049-1327.
[0024] Transmission X-ray diffraction can be performed, for example, using a curved IP X-ray diffraction apparatus RINTRAPID2 manufactured by Rigaku Corporation.
[0025] The (IhBN(002)v+IhBN(002)h) / (I(111)v+IcBN(111)h) obtained based on the above-mentioned X-ray intensities is called the compressed boron nitride content value. The compressed boron nitride content value is an indicator related to the amount of compressed boron nitride contained in the boron nitride sintered body 3. The larger the value, the greater the amount of compressed boron nitride contained in the boron nitride sintered body 3. The compressed boron nitride content value is not the content itself.
[0026] In the boron nitride sintered body 3 of the insert 1 of the present invention, the content of compressed boron nitride is greater than 0.002 and less than 0.01. That is, the boron nitride sintered body 3 of the insert 1 of the present invention contains compressed boron nitride to such an extent as to satisfy this condition.
[0027] In addition, IcBN(111)v / (IcBN(111)v+IcBN(111)h) obtained based on the above-mentioned X-ray intensities is called the cubic orientation value. If the cubic orientation value is 0.5, the 111 face of the cubic boron nitride is oriented in a random direction and is in a non-oriented state. The larger the cubic orientation value, the greater the degree to which the 111 face of the cubic boron nitride contained in the boron nitride sintered body 3 is oriented parallel to the first face 7.
[0028] In the boron nitride sintered body 3 of the blade 1 of the present invention, the cubic orientation value is greater than 0.5. In other words, the X-ray intensity at the top of the peak of the 111 diffraction of the cubic boron nitride in the vertical direction is greater than the X-ray intensity at the top of the peak of the 111 diffraction of the cubic boron nitride in the parallel direction. That is, it can also be said that the 111 face of the cubic boron nitride is oriented along the normal direction of the first face 7.
[0029] The IhBN(002)v / (IhBN(002)v+IhBN(002)h) obtained based on the above-mentioned X-ray intensities is called the compressed boron nitride orientation value. If the compressed boron nitride orientation value is 0.5, the 002 face of the compressed boron nitride is oriented in a random direction and is in a non-oriented state. The larger the compressed boron nitride orientation value, the greater the degree to which the 002 face of the compressed boron nitride contained in the boron nitride sintered body 3 is oriented parallel to the first face 7.
[0030] In the boron nitride sintered body 3 of the insert 1 of the present invention, the orientation value of the compressed boron nitride is greater than the orientation value of the cubic crystal. That is, the degree to which the 002 plane of the compressed boron nitride is oriented parallel to the first plane 7 is greater than the 111 plane of the cubic crystal boron nitride.
[0031] The insert 1 of the present invention has excellent wear resistance by having the above structure. This effect is presumed to be due to the fact that the insert 1 of the present invention contains a small amount of compressed boron nitride, and further, the 002 plane of the compressed boron nitride is oriented in large quantities on the first surface, so the workpiece bonded to the first surface is peeled off together with the compressed boron nitride.
[0032] The boron nitride sintered body 3 of the insert 1 of the present invention may have a compressed boron nitride content of 0.004 or more and 0.008 or less. With such a structure, the insert 1 has a high hardness.
[0033] In addition, the boron nitride sintered body 3 of the insert 1 of the present invention may have a cubic orientation value of 0.55 or more. With such a structure, the hardness of the first surface 7 is high.
[0034] In addition, the boron nitride sintered body 3 of the insert 1 of the present invention may have a compression type boron nitride orientation value of 0.8 or more. With such a structure, the insert 1 has a long life.
[0035] The boron nitride sintered body 3 of the blade 1 of the present invention may contain wurtzite-type boron nitride. The boron nitride sintered body 3 having such a structure has high hardness.
[0036] In addition, in the blade 1 of the present invention, the average particle size of the cubic boron nitride can be 200 nm or less. With such a structure, the blade 1 has high strength. In addition, the average particle size of the cubic boron nitride can be 100 nm or less.
[0037] Furthermore, the insert 1 of the present invention may have a hard coating (not shown) on the surface of the boron nitride sintered body 3 .
[0038] <Vickers hardness>
[0039] In the insert 1 of the present invention, the Vickers hardness in the direction perpendicular to the first surface 7 of the boron nitride sintered body 3 is 40.0 GPa or more at 1000°C.
[0040] Furthermore, the Vickers hardness in the direction perpendicular to the first surface 7 of the boron nitride sintered body 3 is greater than 45.0 GPa at 700°C.
[0041] Furthermore, the Vickers hardness in the direction perpendicular to the first surface 7 of the boron nitride sintered body 3 is greater than 47.0 GPa at 400°C.
[0042] As described above, since the insert 1 of the present invention has high hardness at high temperatures, it is excellent in wear resistance during high-temperature cutting.
[0043] <Cutting tools>
[0044] Next, refer to Figure 3 The cutting tool of the present invention will be described. Figure 3 This is a diagram showing an example of the cutting tool of the present invention.
[0045] The cutting tool 101 of the present invention, such as Figure 3 As shown, for example, from the first end ( Figure 3 ) toward the second end ( Figure 3 A rod-shaped body extending from the lower end of the rod.
[0046] Cutting tool 101, such as Figure 3 As shown, the cutting tool 101 comprises: a tool holder 105 having a length extending from a first end (front end) to a second end and having a slot 103 located at the first end side; and the blade 1 located at the slot 103. Since the cutting tool 101 comprises the blade 1, stable cutting processing can be performed for a long time.
[0047] The slot 103 is a portion where the blade 1 is mounted, and has a support surface parallel to the lower surface of the handle 105 and a limiting side surface perpendicular or inclined to the support surface.
[0048] The blade 1 is located in the slot 103. At this time, the lower surface of the blade 1 can be directly in contact with the slot 103, and a spacer (not shown) can also be sandwiched between the blade 1 and the slot 103.
[0049] The blade 1 is mounted on the handle 105 in such a manner that at least a portion of the portion of the ridge where the rake face 7 and the flank face 9 intersect, which is used as the cutting edge 13, protrudes outward from the handle 105. In the present embodiment, the blade 1 is mounted on the handle 105 by a fixing bolt 107. That is, the fixing bolt 107 is inserted into the through hole 55 of the blade 1, and the front end of the fixing bolt 107 is inserted into a screw hole (not shown) formed in the slot 103, and the threaded portions are tightened, thereby mounting the blade 1 on the handle 105.
[0050] Steel, cast iron, etc. can be used as the material of the handle 105. Among these members, steel with high toughness can be used.
[0051] In this embodiment, the cutting tool for so-called turning is illustrated. As turning, for example, inner diameter processing, outer diameter processing and slotting processing can be listed. In addition, as a cutting tool, it is not limited to turning. For example, the cutting tool for milling can also use the blade 1 of the above embodiment.
[0052] <Manufacturing method>
[0053] The following is a description of a method for manufacturing a sintered boron nitride body of a blade of the present invention. First, prepare a flat hexagonal boron nitride powder as a raw material powder. Use a commercially available raw material with an average particle size of 0.7 μm or more and an oxygen impurity content of less than 0.5% by mass. The so-called average particle size of the hexagonal boron nitride powder means the average value of the length of the long axis direction of the boron nitride powder measured by an electron microscope. The hexagonal boron nitride powder can have an average particle size of 0.2 μm or more and 30 μm or less. The hexagonal boron nitride powder can also be a high-purity powder with a purity of more than 99%. In addition, it can also contain a catalyst component used when manufacturing cubic boron nitride powder. In addition, a raw material powder with a purity of less than 99% can also be used.
[0054] The raw material powder is formed by uniaxial pressing. By controlling the pressure during forming, the cubic orientation value and the orientation value of the compressed boron nitride after firing can be controlled. During uniaxial pressing, the flat hexagonal boron nitride powder is oriented, and the 002 plane of the hexagonal boron nitride powder is oriented in a manner perpendicular to the pressing axis direction of the pressing. During uniaxial pressing, if the same molded body is repeatedly pressed, the orientation of the hexagonal boron nitride powder of the molded body is high.
[0055] Next, the formed body produced by the above method is fired at a temperature of 1800 to 2200 degrees and a pressure of 8 to 10 GPa to obtain the boron nitride sintered body of the present invention. The proportion of compressed boron nitride contained in the boron nitride sintered body can be controlled by the temperature and pressure during firing.
[0056] As mentioned above, the boron nitride sintered body, the insert, and the cutting tool of the present invention have been described, but the present invention is not limited to the above-mentioned embodiments, and various improvements and changes can be made without departing from the scope of the present invention.
[0057] Example
[0058] Flat hexagonal boron nitride powders having an average particle size of 0.3 μm, 6 μm, and 16 μm and an oxygen impurity content of 0.3 mass% were molded by uniaxial pressing to obtain molded bodies. In addition, the same hexagonal boron nitride powders were subjected to isostatic pressing to produce molded bodies. These molded bodies were sintered under the conditions shown in Table 1.
[0059] Next, the obtained sintered body was cut along the direction perpendicular to the first surface of the sintered body to prepare a test piece with a thickness of about 0.5 mm having a surface intersecting at right angles with respect to the first surface. Based on the cross section of the test piece perpendicular to the first surface, the content value of compressed boron nitride, the cubic crystal orientation value, and the orientation value of compressed boron nitride were obtained using the curved IPX-ray diffraction device RINT RAPID2 manufactured by Rigaku Co., Ltd. The obtained values are shown in Table 1.
[0060] [Table 1]
[0061]
[0062] In addition, a portion of the obtained sintered body was cut to make a blade. A cutting test was performed using the first surface of the blade as the rake face. The conditions of the cutting test are shown below.
[0063] <Cutting test conditions>
[0064] Cutting material: Ti alloy (Ti-6Al-4V)
[0065] Cutting conditions: Vc = 100m / min, f = 0.1mm / rev, ap = 0.4mm, Wet
[0066] Tool used: CNGA120408
[0067] Samples No. 1 to 3, 7, 11, and 15 obtained from isostatically pressed molded bodies do not have the structure of the boron nitride sintered body in the blade of the present invention. In addition, even when a uniaxially pressed molded body is used, samples No. 8 to 10, which are fired at a temperature of 2100°C and a pressure of 11 GPa, do not contain compressed boron nitride. Sample No. 16, which is a uniaxially pressed molded body with a firing temperature of 2300°C and a firing pressure of 7.7 GPa, contains compressed boron nitride, but the orientation value of the compressed boron nitride is less than the cubic orientation value.
[0068] On the other hand, among the samples formed by uniaxial pressing, the compressed boron nitride content of samples No. 4 to 6 and 12 to 14 is less than 0.005, the cubic orientation value is greater than 0.5, and the compressed boron nitride orientation value is greater than the cubic orientation value, and the life is long. In addition, the average particle size of the cubic boron nitride of samples No. 4 to 6 and 12 to 14 is less than 200nm. In particular, the average particle size of samples No. 4 and No. 12 using raw material powders with small average particle sizes is less than 100nm.
[0069] Samples No. 5, 6, 12, 13, and 14 with a cubic orientation value of 0.55 or more have a longer life than sample No. 4 with a cubic orientation value of less than 0.55. Samples No. 13 and 14 with a compressed boron nitride orientation value of 0.8 or more have a longer life than sample No. 12 with a compressed boron nitride orientation value of less than 0.8.
[0070] The life of the samples that did not satisfy the constituent requirements of the blade of the present invention was shorter than that of samples No. 4 to 6 and 12 to 14 that were the blade of the present invention.
[0071] <High temperature hardness measurement>
[0072] Flat hexagonal boron nitride powders with average particle sizes of 0.3 μm, 6 μm, and 16 μm and oxygen impurity content of 0.3 mass% were formed by uniaxial pressing to obtain a compact. The compact was sintered at a sintering temperature of 2100 to 2200° C. and a pressure of 9 GPa.
[0073] Then, the Vickers hardness of the obtained sintered body was measured at 25°C, 400°C, 700°C and 1000°C respectively. The Vickers hardness was evaluated by a known test method, in which a diamond pyramid-shaped (quadrangular pyramid-shaped) indenter was pressed into the first face (front face) of the sintered body, and the indentation left after the load was released was measured. The measurement conditions were as follows.
[0074] <Measurement conditions>
[0075] Current example device: High temperature hardness tester QM type manufactured by Nikon Corporation
[0076] Indenter load: 4.9N
[0077] Pressing time of the pressure head: 15sec
[0078] Measuring atmosphere: vacuum
[0079] Figure 4 is a graph showing the results of high temperature hardness measurement. Figure 4As shown, the Vickers hardness in the direction perpendicular to the first surface of the obtained sintered body is about 42.0 GPa at 1000°C, about 46.0 GPa at 700°C, and about 48.0 GPa at 400°C.
[0080] The embodiments disclosed herein should be considered to be illustrative in all respects and not restrictive. In fact, the above embodiments can be embodied in various ways. In addition, the above embodiments can be omitted, replaced, and changed in various ways without departing from the scope of the attached claims and their purpose.
[0081] Explanation of symbols
[0082] 1…Blade
[0083] 3… Boron nitride sintered body
[0084] 5…Matrix
[0085] 7… Rake face
[0086] 9…flank face
[0087] 13…Cutting edge
[0088] 101…Cutting tools
[0089] 103…Card slot
[0090] 105…Handle
Claims
1. A blade comprising a boron nitride sintered body having a first surface, a second surface, and a cutting edge located on at least a portion of an edge portion between the first surface and the second surface, in, The boron nitride sintered body contains cubic boron nitride and compressed boron nitride. In transmission X-ray diffraction of a cross section of the boron nitride sintered body perpendicular to the first surface, Assume that the X-ray intensity at the top of the peak of the 111 diffraction of the cubic boron nitride in the direction perpendicular to the first surface is IcBN(111)v, and the X-ray intensity at the top of the peak of the 002 diffraction of the compressed boron nitride is IhBN(002)v, Assuming that the X-ray intensity at the top of the peak of the 111 diffraction of the cubic boron nitride in the direction parallel to the first surface is IcBN(111)h, and the X-ray intensity at the top of the peak of the 002 diffraction of the compressed boron nitride is IhBN(002)h, The compressed boron nitride content expressed by (IhBN(002)v+IhBN(002)h) / (IcBN(111)v+IcBN(111)h) is greater than 0.002 and less than 0.01, The cubic orientation value represented by IcBN(111)v / (IcBN(111)v+IcBN(111)h) is greater than 0.5, The compression type boron nitride orientation value represented by IhBN(002)v / (IhBN(002)v+IhBN(002)h) is greater than the cubic orientation value, The Vickers hardness of the boron nitride sintered body in a direction perpendicular to the first surface is 40.0 GPa or more at 1000°C.
2. The blade according to claim 1, in, The cubic crystal orientation value is greater than 0.
55.
3. The blade according to claim 1 or 2, in, The compressed boron nitride has an orientation value of 0.8 or more.
4. The blade according to claim 1 or 2, in, The boron nitride sintered body contains wurtzite-type boron nitride.
5. The blade according to claim 1 or 2, in, An average grain size of the cubic boron nitride in the cross section is 200 nm or less.
6. The blade according to claim 1 or 2, in, The Vickers hardness is greater than 45.0 GPa at 700°C.
7. The blade according to claim 1 or 2, in, The Vickers hardness is greater than 47.0 GPa at 400°C.
8. A cutting tool, comprising: a tool holder having a length extending from a first end to a second end and having a groove on the first end side; The blade according to any one of claims 1 to 7 located in the slot.