A kind of infrared chalcogenide glass doped with high concentration of rare earth and preparation method thereof

By introducing Ga and La elements into chalcogenide glass, the solubility of rare earth ions and the number of active centers are increased, the problem of low rare earth doping concentration in the existing technology is solved, and efficient mid-infrared laser output characteristics are achieved, which is a new step for mid-infrared lasers. The development provides new research directions.

CN116573854BActive Publication Date: 2024-10-08NINGBO UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310453687.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-23
Publication Date
2024-10-08
Estimated Expiration
2043-04-23

AI Technical Summary

Technical Problem

It is difficult to achieve high concentration of rare earth doping in existing rare earth-doped chalcogenide glasses in mid-infrared lasers, resulting in low laser output efficiency and failure to achieve effective emission of mid-infrared lasers.

Method used

By introducing Ga and La elements into chalcogenide glass, a high-concentration rare earth-doped infrared chalcogenide glass is formed. The edge sharing structure of Ga and the similarity of La ions are used to increase the solubility of rare earth ions and the number of activation centers to optimize the chalcogenide glass. The composition and preparation process are used to achieve high concentration of rare earth doping.

Benefits of technology

The infrared chalcogenide glass doped with high concentration of rare earths has achieved stable physical and chemical properties and excellent mid-infrared transmittance and fluorescence emission characteristics, providing a new research approach for the development of mid-infrared lasers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116573854B_ABST
    Figure CN116573854B_ABST
Patent Text Reader

Abstract

The molar percentage composition of the high-concentration rare earth-doped infrared chalcogenide glass disclosed in the present invention is: GeS 2 :30~55%,Ga 2 S 3 :15~40%,La 2 S 3 :1~12%,LaCl 3 :1~9%,CsCl:5~20%,Rare earth sulfide RE 2 S 3 :0.1~35%, wherein the rare earth RE is at least one of Er, Tm, Pr, Ho, and Dy. The present invention introduces Ga and La elements into the chalcogenide glass by optimizing the composition and preparation process of the chalcogenide glass, thereby achieving high-concentration doping of multiple rare earth ions, increasing the number of activation centers, and thus improving the mid-infrared luminescence efficiency of the chalcogenide glass. The infrared chalcogenide glass doped with high concentrations of rare earths of the present invention has stable physicochemical properties, good glass-forming ability, excellent mid-infrared transmittance and fluorescence emission characteristics, and can be applied to mid-infrared lasers, opening up a new research path for the development of mid-infrared lasers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of chalcogenide glass and preparation thereof, and in particular to high-concentration rare earth-doped infrared chalcogenide glass and a preparation method thereof. Background Art

[0002] Mid-infrared lasers have very important applications in advanced manufacturing, medical treatment, sensing, national security and other fields. In order to obtain efficient mid-infrared laser output, activation ions and matrix materials are two factors that must be considered. Among the many activation ions, rare earth ions (such as Er, Pr, Tm, Ho, Dy, etc.) have rich emission energy levels in the mid-infrared band and become the most potential emission center for achieving mid-infrared laser output. For mid-infrared lasers, the energy interval between the upper and lower energy levels of rare earth ions is small, and multi-phonon non-radiative relaxation is very likely to occur in the matrix with high phonon energy, resulting in fluorescence quenching, which is not conducive to laser output. Therefore, the use of matrix materials with low phonon energy is a necessary condition for producing mid-infrared laser output.

[0003] Chalcogenide glass refers to a type of inorganic non-oxide glass that is based on the periodic table's Group VI A elements sulfur (S), selenium (Se), and tellurium (Te) and introduces a certain amount of other elements with weak electronegativity, such as arsenic (As), antimony (Sb), and germanium (Ge). It has the following notable characteristics: (1) It has a wide infrared transmission range (~20μm); (2) It has very low phonon energy (~350cm -1 ), so the probability of non-radiative transition caused by multi-phonon relaxation is low, the excited state lifetime is long, and the quantum efficiency is high; (3) It has a large refractive index (>2.0), which makes the strong local electric field around the rare earth ions in the chalcogenide glass induce a large stimulated radiation cross section, which is conducive to laser output. Therefore, rare earth-doped chalcogenide glass is considered to be a very promising gain material for obtaining mid-infrared laser output.

[0004] Rare earth doped chalcogenide glass has experienced rapid development, but so far only near-infrared laser output has been achieved, and the mid-infrared band is mainly focused on fluorescence emission, and no mid-infrared laser research has been reported. This is mainly due to the fact that chalcogenide glass has the characteristics of strong covalent bonds and weak ionic bonds, resulting in low solubility of rare earth ions. The rare earth ion solubility of the more mature As2S3 glass is only 10 -4 In order to improve the rare earth solubility of chalcogenide glass, many researchers have systematically studied the effect of glass composition on rare earth doping concentration, but the achievable rare earth doping concentration is generally lower than 1 mol%, far from the ideal gain doping concentration. Therefore, the development of a new type of chalcogenide glass material with high rare earth solubility has important scientific significance for the development of mid-infrared lasers. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a high-concentration rare earth-doped infrared chalcogenide glass which can be applied to mid-infrared lasers and has stable physicochemical properties, good glass-forming ability, excellent mid-infrared transmittance and fluorescence emission characteristics, and a preparation method thereof in view of the shortcomings of the prior art.

[0006] The technical solution adopted by the present invention to solve the above technical problems is: a high-concentration rare earth-doped infrared chalcogenide glass, the molar percentage composition of the infrared chalcogenide glass is: GeS2: 30-55%, Ga2S3: 15-40%, La2S3: 1-12%, LaCl3: 1-9%, CsCl: 5-20%, rare earth sulfide RE2S3: 0.1-35%, wherein the rare earth RE is at least one of Er, Tm, Pr, Ho, and Dy.

[0007] The present invention achieves the purpose of improving the solubility of rare earth ions in chalcogenide glass by introducing Ga and La elements into chalcogenide glass, thereby realizing high concentration rare earth doping. The main reasons are: (1) the present invention adds Ga as a modifier into the chalcogenide glass network, which can significantly improve the solubility of rare earth ions due to the existence of edge-sharing [GaS4] tetrahedral structure; (2) rare earth ions and La 3+ With similar ionic radius and valence, rare earth ions can directly replace La 3+ position, thereby achieving high concentration of rare earth doping.

[0008] The present invention can achieve high-concentration doping of multiple rare earth ions by optimizing the composition of chalcogenide glass, increase the number of activation centers, and thus improve the mid-infrared luminescence efficiency of chalcogenide glass. The infrared chalcogenide glass doped with high concentrations of rare earths in the present invention has stable physical and chemical properties, good glass-forming ability, excellent mid-infrared transmittance and fluorescence emission characteristics, and can be applied to mid-infrared lasers, opening up a new research path for the development of mid-infrared lasers.

[0009] Preferably, in the infrared chalcogenide glass, the sum of the molar percentages of Ga and La is greater than 45%, and the molar percentage of the rare earth sulfide RE2S3 is 1 to 35%. When the sum of the molar percentages of Ga and La is greater than 45%, the rare earth doping concentration in the infrared chalcogenide glass of the present invention can be ensured to be 1 to 35 mol%.

[0010] The method for preparing the above-mentioned high-concentration rare earth-doped infrared chalcogenide glass comprises the following steps:

[0011] (1) Prepare the raw materials GeS2, Ga2S3, La2S3, LaCl3, CsCl and rare earth sulfide RE2S3 in the required proportions and weigh them in an inert gas-filled and dry environment;

[0012] (2) After the prepared raw materials are fully mixed, they are placed in a quartz ampoule, and the quartz ampoule is evacuated to a vacuum degree of less than 10 -3 Pa, then seal the quartz ampoule with hydrogen-oxygen flame or oxyacetylene flame;

[0013] (3) The sealed quartz ampoule is placed in a rocking furnace and slowly heated to 850-1000°C in a multi-stage heating manner. It is then kept at 850-1000°C for 12-24 hours while rocking. After standing upright for 1-3 hours, it is taken out of the furnace for quenching. It is then quickly placed in a precision annealing furnace and kept at 350-420°C for 2-6 hours. After cooling to room temperature with the furnace, a high-concentration rare earth-doped infrared chalcogenide glass is obtained.

[0014] Preferably, in step (1), the purity of the raw materials GeS2, Ga2S3, La2S3, LaCl3, CsCl and rare earth sulfide RE2S3 is above 4N.

[0015] Preferably, in step (1), the inert gas is nitrogen or argon.

[0016] Preferably, in step (3), the process of the multi-stage heating method is as follows: first, slowly heat the temperature to 300-450°C at a heating rate of 1-3°C / min, and keep it at this temperature for 1-3 hours; then slowly heat the temperature to 650-750°C at a heating rate of 1-4°C / min, and keep it at this temperature for 1-3 hours; finally, slowly heat the temperature to 850-1000°C at a heating rate of 1-2°C / min.

[0017] Preferably, in step (3), the swinging rate is 5 to 15 r / min, and the swinging angle is 30 to 180°.

[0018] Compared with mid-infrared laser gain materials, the present invention has the following advantages:

[0019] 1. The present invention optimizes the composition of chalcogenide glass and introduces Ga and La elements into the chalcogenide glass, thereby achieving high-concentration doping of multiple rare earth ions, increasing the number of activation centers, and thus improving the mid-infrared luminescence efficiency of the chalcogenide glass. The infrared chalcogenide glass doped with high concentrations of rare earths in the present invention has stable physical and chemical properties, good glass-forming ability, excellent mid-infrared transmittance and fluorescence emission characteristics, and can be applied to mid-infrared lasers, opening up a new research path for the development of mid-infrared lasers.

[0020] 2. The present invention optimizes the preparation process of chalcogenide glass and adopts a multi-stage heating method to make the raw materials fully melted and uniform, so that elements such as Ga and La are effectively integrated into the chalcogenide glass to ensure high concentration doping of rare earths. The infrared chalcogenide glass prepared by the method of the present invention has good glass-forming ability, excellent thermochemical stability and mid-infrared optical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The transmission spectra of the infrared chalcogenide glass samples prepared in Examples 1 to 6;

[0022] Figure 2 Mid-infrared fluorescence spectra of the infrared chalcogenide glass samples prepared in Examples 1 to 6. DETAILED DESCRIPTION

[0023] The present invention is further described in detail below with reference to the accompanying drawings.

[0024] Example 1: Select rare earth sulfide Er2S3, the molar percentage composition of the infrared chalcogenide glass is: GeS2: 40%, Ga2S3: 24%, La2S3: 4%, LaCl3: 2%, CsCl: 10%, rare earth sulfide Er2S3: 20%. The preparation method of the infrared chalcogenide glass of Example 1 is: prepare the raw materials GeS2, Ga2S3, La2S3, LaCl3, CsCl and rare earth sulfide Er2S3 in the required proportion, weigh 20g of the raw materials in a glove box filled with argon and dry and mix them evenly; put the mixed raw materials into a pre-cleaned dry quartz ampoule, evacuate the quartz ampoule to a vacuum degree of less than 10 -3 Pa, and then the quartz ampoule is sealed with an oxygen-acetylene flame; the sealed quartz ampoule is placed in a rocking furnace, first slowly heated to 300°C at a heating rate of 1°C / min, and kept at this temperature for 2 hours; then slowly heated to 700°C at a heating rate of 2°C / min, and kept at this temperature for 2 hours; finally slowly heated to 950°C at a heating rate of 1°C / min, and then kept at 950°C for 12 hours while rocking, wherein the rocking rate is 5r / min and the rocking angle is 60°; stop rocking and stand upright for 1 hour, then take out of the furnace for quenching, then quickly put into a precision annealing furnace and keep at 380°C for 2 hours, and cool to room temperature with the furnace to obtain high-concentration rare earth-doped infrared chalcogenide glass.

[0025] Figure 1 (a) is the transmission spectrum of the 1.5 mm thick infrared chalcogenide glass sample prepared in Example 1. Figure 1 (a) It can be seen that the long-wave infrared cutoff edge of the infrared chalcogenide glass sample can reach 13 μm, and the transmittance in the range of 0.6 to 10 μm is close to 70%. Figure 2 (a) is the mid-infrared fluorescence spectrum of the infrared chalcogenide glass sample prepared in Example 1. Figure 2 In (a), an obvious fluorescence signal can be observed, with the emission range covering 2.6 to 2.9 μm and the emission peak located at 2.72 μm.

[0026] Example 2: Select rare earth sulfide Tm2S3, the molar percentage composition of the infrared chalcogenide glass is: GeS2: 45%, Ga2S3: 26%, La2S3: 4%, LaCl3: 2%, CsCl: 8%, rare earth sulfide Tm2S3: 15%. The preparation method of the infrared chalcogenide glass of Example 2 is: prepare the raw materials GeS2, Ga2S3, La2S3, LaCl3, CsCl and rare earth sulfide Tm2S3 in the required proportion, weigh 20g of the raw materials in a glove box filled with argon and dry and mix them evenly; put the mixed raw materials into a pre-cleaned dry quartz ampoule, evacuate the quartz ampoule to a vacuum degree of less than 10 -3 Pa, and then the quartz ampoule is sealed with an oxygen-acetylene flame; the sealed quartz ampoule is placed in a rocking furnace, first slowly heated to 350°C at a heating rate of 2°C / min, and kept at this temperature for 2 hours; then slowly heated to 720°C at a heating rate of 3°C / min, and kept at this temperature for 2 hours; finally, the temperature is slowly heated to 970°C at a heating rate of 1°C / min, and then kept at 970°C for 14 hours while rocking, wherein the rocking rate is 7r / min and the rocking angle is 90°; the rocking is stopped and the ampoule is left standing for 2 hours, then taken out of the furnace for quenching, and then quickly placed in a precision annealing furnace and kept at 360°C for 2 hours, and cooled to room temperature with the furnace to obtain a high-concentration rare earth-doped infrared chalcogenide glass.

[0027] Figure 1 (b) is the transmission spectrum of the 1.5 mm thick infrared chalcogenide glass sample prepared in Example 2. Figure 1 (b) It can be seen that the long-wave infrared cutoff edge of the infrared chalcogenide glass sample can reach 13 μm, and the transmittance in the range of 0.6 to 10 μm is close to 70%. Figure 2 (b) is the mid-infrared fluorescence spectrum of the infrared chalcogenide glass sample prepared in Example 2. Figure 2 In (b), an obvious dual-band fluorescence signal can be observed, with the luminescence range covering 2.3-2.5μm and 3.5-4.1μm, and the luminescence peaks located at 2.4μm and 3.8μm, respectively.

[0028] Example 3: Select rare earth sulfide Pr2S3, the molar percentage composition of the infrared chalcogenide glass is: GeS2: 38%, Ga2S3: 20%, La2S3: 6%, LaCl3: 5%, CsCl: 6%, rare earth sulfide Pr2S3: 25%. The preparation method of the infrared chalcogenide glass of Example 3 is: prepare the raw materials GeS2, Ga2S3, La2S3, LaCl3, CsCl and rare earth sulfide Pr2S3 in the required proportion, weigh 20g of the raw materials in a glove box filled with argon and dry and mix them evenly; put the mixed raw materials into a pre-cleaned dry quartz ampoule, evacuate the quartz ampoule to a vacuum degree of less than 10 -3 Pa, and then the quartz ampoule is sealed with an oxygen-acetylene flame; the sealed quartz ampoule is placed in a rocking furnace, first slowly heated to 380°C at a heating rate of 2°C / min, and kept at this temperature for 2 hours; then slowly heated to 740°C at a heating rate of 3°C / min, and kept at this temperature for 3 hours; finally, the temperature is slowly heated to 980°C at a heating rate of 1°C / min, and then kept at 980°C for 18 hours while rocking, wherein the rocking rate is 10r / min and the rocking angle is 70°; the rocking is stopped and the ampoule is left standing for 1 hour, then taken out of the furnace for quenching, and then quickly placed in a precision annealing furnace and kept at 370°C for 4 hours, and cooled to room temperature with the furnace to obtain a high-concentration rare earth-doped infrared chalcogenide glass.

[0029] Figure 1 (c) is the transmission spectrum of the 1.5 mm thick infrared chalcogenide glass sample prepared in Example 3. Figure 1 (c) It can be seen that the long-wave infrared cutoff edge of the infrared chalcogenide glass sample can reach 13 μm, and the transmittance in the range of 0.6 to 10 μm is close to 70%. Figure 2 (c) is the mid-infrared fluorescence spectrum of the infrared chalcogenide glass sample prepared in Example 3. Figure 2 In (c), an obvious fluorescence signal can be observed, with the emission range covering 3.0 to 5.0 μm and the emission peak located at 4.7 μm.

[0030] Example 4: Select rare earth sulfide Dy2S3, the molar percentage composition of the infrared chalcogenide glass is: GeS2: 50%, Ga2S3: 22%, La2S3: 5%, LaCl3: 4%, CsCl: 9%, rare earth sulfide Dy2S3: 10%. The preparation method of the infrared chalcogenide glass of Example 4 is: prepare the raw materials GeS2, Ga2S3, La2S3, LaCl3, CsCl and rare earth sulfide Dy2S3 in the required proportion, weigh 20g of the raw materials in a glove box filled with argon and dry and mix them evenly; put the mixed raw materials into a pre-cleaned dry quartz ampoule, evacuate the quartz ampoule to a vacuum degree of less than 10 -3Pa, and then the quartz ampoule is sealed with an oxygen-acetylene flame; the sealed quartz ampoule is placed in a rocking furnace, first slowly heated to 400°C at a heating rate of 3°C / min, and kept at this temperature for 3 hours; then slowly heated to 730°C at a heating rate of 2°C / min, and kept at this temperature for 3 hours; finally, the temperature is slowly heated to 1000°C at a heating rate of 2°C / min, and then kept at 1000°C for 20 hours while rocking, wherein the rocking rate is 13r / min and the rocking angle is 80°; the rocking is stopped and the ampoule is left standing for 3 hours, then taken out of the furnace for quenching, and then quickly placed in a precision annealing furnace and kept at 350°C for 3 hours, and cooled to room temperature with the furnace to obtain a high-concentration rare earth-doped infrared chalcogenide glass.

[0031] Figure 1 (d) is the transmission spectrum of the 2.0 mm thick infrared chalcogenide glass sample prepared in Example 4. Figure 1 (d) It can be seen that the long-wave infrared cutoff edge of the infrared chalcogenide glass sample can reach 13 μm, and the transmittance in the range of 0.6 to 10 μm is about 60%. Figure 2 (d) is the mid-infrared fluorescence spectrum of the infrared chalcogenide glass sample prepared in Example 4. Figure 2 In (d), an obvious dual-band fluorescence signal can be observed, with the emission range covering 2.6-3.2μm and 3.8-5.0μm, and the emission peaks located at 2.8μm and 4.4μm, respectively.

[0032] Example 5: Select rare earth sulfide Ho2S3, the molar percentage composition of the infrared chalcogenide glass is: GeS2: 39%, Ga2S3: 18%, La2S3: 9%, LaCl3: 6%, CsCl: 10%, rare earth sulfide Ho2S3: 18%. The preparation method of the infrared chalcogenide glass of Example 5 is: prepare the raw materials GeS2, Ga2S3, La2S3, LaCl3, CsCl and rare earth sulfide Ho2S3 in the required proportion, weigh 20g of the raw materials in a glove box filled with argon and dry and mix them evenly; put the mixed raw materials into a pre-cleaned dry quartz ampoule, evacuate the quartz ampoule to a vacuum degree of less than 10 -3Pa, and then the quartz ampoule is sealed with an oxygen-acetylene flame; the sealed quartz ampoule is placed in a rocking furnace, first slowly heated to 330°C at a heating rate of 1°C / min, and kept at this temperature for 2 hours; then slowly heated to 680°C at a heating rate of 3°C / min, and kept at this temperature for 2 hours; finally slowly heated to 960°C at a heating rate of 2°C / min, and then kept at 960°C for 15 hours while rocking, wherein the rocking rate is 15r / min and the rocking angle is 120°; stop rocking and stand upright for 2 hours, then take out of the furnace for quenching, then quickly put into a precision annealing furnace and keep at 375°C for 2 hours, and cool to room temperature with the furnace to obtain high-concentration rare earth-doped infrared chalcogenide glass.

[0033] Figure 1 (e) is the transmission spectrum of the 2.0 mm thick infrared chalcogenide glass sample prepared in Example 5. Figure 1 (e) It can be seen that the long-wave infrared cutoff edge of the infrared chalcogenide glass sample can reach 13 μm, and the transmittance in the range of 0.6 to 10 μm is about 60%. Figure 2 (e) is the mid-infrared fluorescence spectrum of the infrared chalcogenide glass sample prepared in Example 5. Figure 2 In (e), an obvious dual-band fluorescence signal can be observed, with the luminescence range covering 2.5-3.5μm and 3.8-4.2μm, and the luminescence peaks located at 2.9μm and 3.9μm, respectively.

[0034] Example 6: Select rare earth sulfides Er2S3 and Ho2S3, and the molar percentage composition of the infrared chalcogenide glass is: GeS2: 44%, Ga2S3: 20%, La2S3: 6%, LaCl3: 6%, CsCl: 10%, rare earth sulfide Er2S3: 7%, rare earth sulfide Ho2S3: 7%. The preparation method of the infrared chalcogenide glass of Example 6 is: prepare the raw materials GeS2, Ga2S3, La2S3, LaCl3, CsCl, rare earth sulfide Er2S3 and rare earth sulfide Ho2S3 in the required proportion, weigh 20g of the raw materials in a glove box filled with argon and dry and mix them evenly; put the mixed raw materials into a pre-cleaned dry quartz ampoule, evacuate the quartz ampoule to a vacuum degree of less than 10 -3Pa, and then the quartz ampoule is sealed with an oxygen-acetylene flame; the sealed quartz ampoule is placed in a rocking furnace, first slowly heated to 410°C at a heating rate of 1°C / min, and kept at this temperature for 2 hours; then slowly heated to 750°C at a heating rate of 3°C / min, and kept at this temperature for 2 hours; finally slowly heated to 990°C at a heating rate of 2°C / min, and then kept at 990°C for 15 hours while rocking, wherein the rocking rate is 14r / min and the rocking angle is 100°; stop rocking and stand upright for 2 hours, then take out of the furnace for quenching, then quickly put into a precision annealing furnace and keep at 380°C for 2 hours, and cool to room temperature with the furnace to obtain high-concentration rare earth-doped infrared chalcogenide glass.

[0035] Figure 1 (f) is the transmission spectrum of the 2.0 mm thick infrared chalcogenide glass sample prepared in Example 6. Figure 1 (f) It can be seen that the long-wave infrared cutoff edge of the infrared chalcogenide glass sample can reach 13 μm, and the transmittance in the range of 0.6 to 10 μm is about 75%. Figure 2 (f) is the mid-infrared fluorescence spectrum of the infrared chalcogenide glass sample prepared in Example 6. Figure 2 In (f), an obvious ultra-wideband fluorescence signal can be observed, with the emission range covering 2.5 to 3.1 μm, and the emission peaks located at 2.7 μm and 2.84 μm, respectively.

Claims

1. A high concentration rare earth doped infrared chalcogenide glass, characterized in that: The infrared chalcogenide glass has a molar percentage composition of: GeS2: 30-55%, Ga2S3: 15-40%, La2S3: 1-12%, LaCl3: 1-9%, CsCl: 5-20%, rare earth sulfide RE2S3: 1-35%, wherein the rare earth RE is at least one of Er, Tm, Pr, Ho, and Dy.

2. The high-concentration rare earth doped infrared chalcogenide glass according to claim 1, characterized in that: In the infrared chalcogenide glass, the sum of the molar percentage contents of Ga and La is greater than 45%.

3. The method for preparing a high-concentration rare earth-doped infrared chalcogenide glass according to claim 1 or 2, characterized in that: The following steps are involved: (1) Prepare the required proportions of raw materials GeS2, Ga2S3, La2S3, LaCl3, CsCl and rare earth sulfide RE2S3 and weigh them in an inert gas-filled and dry environment; (2) After the prepared raw materials are fully mixed, they are placed in a quartz ampoule and the quartz ampoule is evacuated to a vacuum degree of less than 10 -3 Pa, then seal the quartz ampoule with hydrogen-oxygen flame or oxyacetylene flame; (3) Place the sealed quartz ampoule in a rocking furnace and slowly heat it to 850-1000°C in a multi-stage heating method. Then, keep it at 850-1000°C for 12-24 hours while rocking. After standing it upright for 1-3 hours, take it out of the furnace for quenching. Then, quickly place it in a precision annealing furnace and keep it at 350-420°C for 2-6 hours. After cooling it to room temperature, a high-concentration rare earth-doped infrared chalcogenide glass is obtained.

4. The method for preparing a high-concentration rare earth-doped infrared chalcogenide glass according to claim 3, characterized in that: In step (1), the purity of the raw materials GeS2, Ga2S3, La2S3, LaCl3, CsCl and rare earth sulfide RE2S3 is above 4 N.

5. The method for preparing a high-concentration rare earth-doped infrared chalcogenide glass according to claim 3, characterized in that: In step (1), the inert gas is nitrogen or argon.

6. The method for preparing a high-concentration rare earth-doped infrared chalcogenide glass according to claim 3, characterized in that: In step (3), the process of the multi-stage heating method is as follows: first, slowly heat the temperature to 300-450°C at a heating rate of 1-3°C / min, and keep it at this temperature for 1-3 hours; then slowly heat the temperature to 650-750°C at a heating rate of 1-4°C / min, and keep it at this temperature for 1-3 hours; finally, slowly heat the temperature to 850-1000°C at a heating rate of 1-2°C / min.