An electron transport material and its use in electroluminescent devices
By using organic compounds with arylphosphine oxide or phenanthroline structures as electron transport materials in OLED devices, the energy level difference between the N-type and P-type charge generation layers was solved, improving electron injection efficiency and thermal stability, extending device lifetime, and reducing driving voltage.
Patent Information
- Application Number
- CN202310530416.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-12-08
- Filing Date
- 2023-05-12
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-05-12
AI Technical Summary
In existing OLED devices, the energy level difference between the N-type charge generation layer and the P-type charge generation layer leads to electron injection degradation, affecting device lifespan and performance, and the commonly used materials have insufficient thermal/electrical stability.
Organic compounds with arylphosphine oxide or phenanthrene phosphonoline structures are used as electron transport materials. By coordinating with alkali metal or alkaline earth metal compounds, the energy level difference is reduced, the electron injection efficiency is improved, and the thermal stability is enhanced.
This improved the luminescence performance and lifespan of OLED devices while reducing the driving voltage and enhancing the thermal stability and electron transport performance of the devices.
Smart Images

Figure CN116574131B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of organic electroluminescence technology, and in particular to an electron transport material and its application in electroluminescent devices. Background Technology
[0002] Organic light emission diodes (OLEDs) have been widely used in the display and lighting industries, especially in mobile phone displays. The latest mobile phone products launched by manufacturers such as Apple, Sumsang, Huawei and Xiaomi all use OLED screens. This is mainly due to the excellent characteristics of OLEDs, such as self-emission, wide viewing angle, high contrast, fast response speed and the ability to fabricate flexible devices.
[0003] When applying OLED devices to displays, low driving voltage, high luminous efficiency, and long lifespan are required. Generally, OLED devices can be divided into single-layer and multi-layer devices. To achieve a significant increase in OLED lifespan, multiple OLED devices are stacked together, forming a multi-layer OLED structure. A multi-layer OLED structure includes a first emitting layer containing a blue emitting layer and a second emitting layer containing yellow-green or green and red emitting layers, wherein the first and second emitting layers are stacked vertically; alternatively, blue, green, and red emitting layers can be used as the first emitting layer, and then blue, green, and red emitting layers are stacked on top of it as the second emitting layer.
[0004] Furthermore, tandem OLEDs include a charge generation layer positioned between a first light-emitting stack and a second light-emitting stack to improve current efficiency in each light-emitting layer while ensuring efficient charge distribution to the light-emitting stack. Typically, the charge generation layer includes an N-type charge generation layer and a P-type charge generation layer. In such a charge generation layer used in common tandem OLEDs, due to the energy level difference between the N-type and P-type charge generation layers, charge is generated at the interface between the P-type charge generation layer and the adjacent hole injection or hole transport layer, leading to electron injection degradation in the N-type charge generation layer.
[0005] When the N-type charge generation layer is doped with metal, the metal may diffuse into the P-type charge generation layer, leading to a reduction in OLED lifetime. In particular, common materials used for the charge generation layer lack sufficient thermal / electrical stability. Therefore, long-term operation of the OLED results in the degradation or deterioration of the materials used in the charge generation layer, and a significant reduction in electron injection efficiency from the N-type charge generation layer to the adjacent electron transport layer, leading to decreased OLED performance and lifetime. Summary of the Invention
[0006] One aspect of the present invention is to provide an organic compound that exhibits high thermal stability while possessing excellent electron injection / electron transport properties.
[0007] Another aspect of the present invention is to provide an organic electroluminescent device that improves luminescence performance and lifetime while having a reduced driving voltage, and an organic light-emitting display comprising the electroluminescent device.
[0008] One aspect of the present invention provides an organic compound represented by formula (A1) or (A2):
[0009]
[0010] Where X is selected from C or Si;
[0011] L1 and L2 are independently selected from hydrogen, deuterium, tritium, cyano, nitro, halogen, hydroxyl, alkylthio with 1 to 4 carbon atoms, alkyl with 1 to 30 carbon atoms, cycloalkyl with 1 to 20 carbon atoms, arylphosphine oxide, phenanthroline compound, and at least one of them is independently selected from arylphosphine oxide, phenanthroline compound.
[0012] The aryl group is a C6 to C50 aryl group with or without substituents, and the substituents are tritium, halogens, or C1-C8 alkyl groups.
[0013] R1-R2 are independently selected from hydrogen, deuterium, tritium, cyano, nitro, halogen, hydroxyl, alkylthio with 1 to 4 carbon atoms, alkyl with 1 to 30 carbon atoms, cycloalkyl with 1 to 20 carbon atoms, aryloxy with 6 to 30 carbon atoms, alkoxy with 1 to 30 carbon atoms, alkylamino with 1 to 30 carbon atoms, aromaticamino with 6 to 30 carbon atoms, arylalkylamino with 6 to 30 carbon atoms, heteroarylamino with 2 to 24 carbon atoms, and carbon. The alkylsilyl group having 1 to 30 atoms, the arylsilyl group having 6 to 30 carbon atoms, the alkenyl group having 2 to 30 carbon atoms, the alkynyl group having 2 to 24 carbon atoms, the aralkyl group having 7 to 30 carbon atoms, the aryl group having 6 to 30 carbon atoms, the heteroaryl group having 5 to 60 carbon atoms, or the heteroarylalkyl group having 6 to 30 carbon atoms, wherein the heteroatom in the heteroarylamino, heteroaryl, or heteroarylalkyl group is at least one of N, O, S, Si, or Se.
[0014] Preferably, at least one of L1 and L2 has any of the structures in formulas (B1)-(B5);
[0015]
[0016] X = C,
[0017] Ar1 and Ar2 are independently selected from C6 to C50 aryl groups (with or without substituents), C4 to C60 heteroaryl groups (with or without substituents), or Ar1 and Ar2 are linked together, or Ar1 or Ar2 is linked to the benzene ring on the spirofluorene ring, by any of the following forms: single bond, oxygen atom, sulfur atom, methylene, dimethylmethylene, C6 to C10 arylene groups (with or without substituents), or C4 to C10 heteroaryl groups (with or without substituents). The substituents are deuterium, halogen, C1-C6 alkyl, or C6-C10 aryl.
[0018] R3-R4 are independently selected from hydrogen, deuterium, tritium, cyano, nitro, halogen, hydroxyl, alkylthio with 1 to 4 carbon atoms, alkyl with 1 to 30 carbon atoms, cycloalkyl with 1 to 20 carbon atoms, aryloxy with 6 to 30 carbon atoms, alkoxy with 1 to 30 carbon atoms, alkylsilyl with 1 to 30 carbon atoms, arylsilyl with 6 to 30 carbon atoms, aralkyl with 7 to 30 carbon atoms, aryl with 6 to 30 carbon atoms, heteroaryl with 5 to 60 carbon atoms, or heteroarylalkyl with 6 to 30 carbon atoms.
[0019] Preferably, the aryl group has 6 to 20 aromatic ring atoms.
[0020] The heteroaryl group preferably has 4 to 40 aromatic ring atoms with carbon atoms, and the heteroatom is at least one of N, O, and S.
[0021] Preferably, L1 and L2 are independently selected from any of the structures in formulas (B1)-(B5).
[0022] Preferably, its general structural formula is shown in (C1)-(C7).
[0023]
[0024] Ar1 and Ar2 are each independently selected from phenyl, naphthyl, anthraceneyl, phenanthrene, dihydrophenanthrene, alkylphenyl, biphenyl, alkylbiphenyl, halophenyl, alkoxyphenyl, haloalkoxyphenyl, cyanophenyl, silylphenyl, naphthyl, alkylnaphthyl, halonaphthyl, cyanonaphthyl, silylnaphthyl, phenylnaphthyl, pyridyl, alkylpyridyl, halopyridyl, cyanopyridyl, alkoxypyridyl, silylpyridyl, phenylpyridyl, pyrimidinyl, halopyrimidinyl, cyanopyrimidinyl, alkoxypyrimidinyl, phenylpyrimidinyl, quinolinyl, isoquinolinyl, phenylquinolinyl, quinoxaline Ar1 and Ar2 are linked together in a ring by any of the following forms: alkyl, pyrazinyl, quinazolinyl, naphthiophenyl, benzothiopheneyl, benzofuranyl, dibenzothiopheneyl, arylthiazolyl, dibenzofuranyl, fluorenyl, carbazolyl, imidazolyl, carbaolinyl, phenanthrene, terphenyl, terpyridyl, phenylterpyridyl, triphenylene, fluoranyl, and diazafluorenyl, or Ar1 and Ar2 are linked together, Ar1 is linked to the benzene ring on the spirofluorene ring, or Ar2 is linked to the benzene ring on the spirofluorene ring by a single bond, a C6 to C10 arylene group with or without a substituent, or a C4 to C10 heteroarylene group with or without a substituent.
[0025] R1-R4 are independently selected from hydrogen, deuterium, tritium, alkyl with 1 to 6 carbon atoms, cycloalkyl with 1 to 8 carbon atoms, aralkyl with 7 to 10 carbon atoms, aryl with 6 to 10 carbon atoms, heteroaryl with 5 to 10 carbon atoms, or heteroarylalkyl with 6 to 10 carbon atoms, wherein the heteroatom in the heteroaryl or heteroarylalkyl group is at least one of N, O, or S.
[0026] R1-R4 are independently selected from hydrogen, deuterium, tritium, alkyl groups with 1 to 4 carbon atoms, cycloalkyl groups with 1 to 6 carbon atoms, and aralkyl groups with 7 to 10 carbon atoms.
[0027] Preferably, the structure of the present invention is as shown in the following formula, but is not limited to the listed structural formulas:
[0028]
[0029]
[0030]
[0031]
[0032] The second invention is to provide an organic electroluminescent device in which at least one of the electron transport layer and the charge generation layer comprises the organic compound described in this invention.
[0033] The third invention is a lighting or display element comprising the aforementioned organic electroluminescent device.
[0034] The organic compound of this invention has a helical central framework, characterized by a high decomposition temperature or a high glass transition temperature, thus exhibiting excellent thermal stability. Therefore, it can prevent the organic compound from deteriorating or degrading due to Joule heating generated during operation. Consequently, when used in electroluminescent devices, this organic compound can increase the lifespan of the electroluminescent device.
[0035] The substituents in this invention adopt arylphosphine oxide structures, phenanthroline structures, or a mixture of both. Both of these structures possess excellent electron transport properties and can be used as materials for electron transport layers. In particular, these two structures can coordinate with alkali metal or alkaline earth metal compounds as dopants for N-type charge generation layers, reducing the energy level difference between the N-type and P-type charge generation layers. This promotes electron injection into the N-type charge generation layer and maximizes electron transfer from the N-type charge generation layer to the adjacent electron transport layer, thereby reducing the device's driving voltage. Detailed Implementation
[0036] The present invention will be further described in detail below with reference to the embodiments.
[0037] This invention does not require specific methods for synthesizing the materials. To describe the invention in more detail, the following examples are provided, but the invention is not limited thereto. Unless otherwise specified, all raw materials used in the following synthesis are commercially available products.
[0038] Example 1:
[0039] Synthesis of compound structure 13
[0040]
[0041] Add (13a) (25g) and tetrahydrofuran (4L) to a 5L four-necked flask. Replace with N2 three times. Lower the ethanol bath to below -80℃ using liquid nitrogen. Add n-BuLi (50.6ml) dropwise, maintaining the temperature below -80℃ with stirring for 0.5h. Then add diphenylphosphine chloride (27.92g) dropwise for 0.5h. After the addition is complete, allow the temperature to rise naturally to room temperature for 2h. Quench with 200ml of ethanol. Rotate the resulting organic solution to dryness. Add 3L of DCM and stir. Wash three times with water. Rotate the resulting organic suspension to dryness. Add 1L of DCM to the resulting solid. Stir and add H2O2 (47.02g) dropwise at room temperature. Continue stirring and react at room temperature for 2h. After the reaction is complete, wash with sodium thiosulfate and water. Directly mix the organic solution with water and purify by column chromatography. Yield: 52%. 1H NMR data are as follows: 1H NMR(400MHz, CDCl3)δ7.42(d,J=7.7Hz,1H),7.29–7.22(m,6H),7.07–6.97(m,7H),6.91–6.81 (m,3H),3.83(td,J=6.8,4.3Hz,2H),2.03(ddd,J=58.8,7.1,4.4Hz,2H),1.50–1.27(m,51H).
[0042] Example 2:
[0043] Synthesis of compound structure 21
[0044]
[0045] The synthesis of compound (21b) was the same as that of compound (13), except that the ratio of n-BuLi, diphenylphosphine chloride, and hydrogen peroxide was halved. The 1H NMR data are as follows: 1H NMR (400MHz, CDCl3) δ 8.03 (d, J = 2.1Hz, 1H), 7.88–7.76 (m, 4H), 7.66 (dt, J = 7.1, 1.9Hz, 5H), 7.60 (dd, J = 8.1, 1.8Hz, 1H), 7.58–7.53 (m, 2H), 7.51–7.44 (m, 4H), 7.40–7.31 (m, 4H), 6.92 (d, J = 2.2Hz, 1H), 6.76–6.69 (m, 2H).
[0046] Synthesis of compound (21c)
[0047] (21b) (13.5 g), Pd(dppf)Cl2 (306 mg), KOAc (4.1 g), and dioxane (125 ml) were added to a 500 ml single-necked flask and heated to reflux for 4 h. After cooling to room temperature, 125 ml of DCM was added, the mixture was filtered through silica gel, the organic phase was evaporated to dryness, dissolved again in DCM, washed three times with deionized water, and the organic phase was evaporated to dryness. The resulting solid was added to 100 ml of THF, heated to reflux, and completely dissolved. Hexane was then added to crystallize the mixture, filtered, and the filter cake was dried. Yield: 74%. The proton NMR data are as follows: ¹H NMR (400MHz, CDCl₃) δ 8.03 (d, J = 2.1 Hz, 1H), 7.87–7.82 (m, 3H), 7.70–7.63 (m, 7H), 7.58–7.53 (m, 2H), 7.50–7.45 (m, 4H), 7.36–7.29 (m, 5H), 6.77–6.71 (m, 2H), 1.24 (s, 12H).
[0048] Synthesis of compound (21)
[0049] 3 g of (21c), 1.27 g of 21d, 10.48 mg of Pd(OAC)₂, 3 g of Na₂CO₃, 26.18 mg of tricyclohexylphosphine, 300 mL of toluene, 75 mL of ethanol, and 24 mL of water were added to a 1000 mL single-necked flask and heated to reflux for 24 h. The reaction mixture was concentrated to approximately 50 mL, and 200 mL of methanol was added. The mixture was filtered to obtain a yellow solid. THF and methanol were added to the solid, and the mixture was heated to reflux and stirred for 0.5 h. After cooling to room temperature, the mixture was filtered, and the filter cake was dried. The yield was 65%. The 1H NMR data are as follows: 1 H NMR (400MHz, CDCl3) δ9.31(s,1H),9.15(d,J=3.7Hz,1H),8.22–8.15(m,2H),8.04(d,J=7.9Hz,1H),7.94(d,J=7.7Hz,1H),7.83 (d,J=7.7Hz,3H),7.76–7.69(m,2H),7.61–7.46(m,8H),7.36(dd,J=16.8,9.4Hz,7H),7.14–7.09(m,3H),6.77(d,J=7.6Hz,2H).
[0050] Example 3:
[0051] Synthesis of compound structure 24
[0052]
[0053] The synthesis of compound (24) was the same as that of compound (21), except that the starting material (13a) was replaced with (24a). The proton NMR data are as follows: 1 H NMR (400MHz, CDCl3) δ9.31(s,1H),9.15(d,J=3.7Hz,1H),8.22–8.15(m,2H),8.04(d,J=7.9Hz,1H),7.94(d,J=7.7Hz,1H),7.83(d,J=7 .7Hz,3H),7.76–7.69(m,2H),7.61–7.46(m,8H),7.36(dd,J=16.8,9.4Hz,5H),7.14–7.09(m,3H),6.77(d,J=7.6Hz,2H).1.31(s,18H).
[0054] Example 4:
[0055] Synthesis of compound structure 39
[0056]
[0057] The synthesis of compound (39) was the same as that of compound (21), except that the starting material (21d) was replaced with (39a). The proton NMR data are as follows: 1 H NMR (400MHz, CDCl3) δ9.18–9.11(m,1H),8.59(d,J=8.0Hz,1H),8.17(d,J=8.0Hz,1H),8.06(dd,J=8.1,5.3Hz,2H),7.93(dd,J=7.9,2.6Hz,1H) ,7.84–7.70(m,3H),7.67(d,J=2.3Hz,2H),7.62–7.40(m,10H),7.34(qd,J=7.8,2.8Hz,6H),7.08(dd,J=8.6,6.6Hz,2H),6.74(d,J=7.8Hz,2H).
[0058] Example 5:
[0059] Synthesis of compound structure 60
[0060]
[0061] The synthesis of compound (60) was the same as that of compound (39), except that the starting material (21c) was replaced with (13a), and the feed ratio of starting material (21d) was doubled. The proton NMR data are as follows: 1 H NMR(400MHz, CDCl3) δ9.19(dd,J=4.4,1.8Hz,2H),8.67(dd,J=8.0,1.7Hz,2H),8.16(dd,J=8.0,1.7Hz,5H),8.05 (d,J=8.4Hz,2H),7.84–7.49(m,11H),7.43(dd,J=8.1,1.8Hz,2H),7.35(d,J=1.7Hz,2H),6.81(d,J=1.8Hz,2H).
[0062] Example 6:
[0063] Synthesis of compound structure 96
[0064]
[0065] The synthesis of compound (96) was the same as that of compound (60), except that the starting material (13a) was replaced with (96a). The proton NMR data are as follows: 1H NMR(400MHz, CDCl3) δ9.05(dd,J=4.0,1.8Hz,2H),8.42(dd,J=8.3,1.8Hz,2H),8.23(dd,J=8.1,0.8Hz,2H),8.02–7.92( m,10H),7.87–7.78(m,4H),7.63(dd,J=8.3,4.0Hz,2H),7.34(dtd,J=18.8,6.7,1.6Hz,4H),6.87(dd,J=7.0,1.6Hz,2H).
[0066] Those skilled in the art should understand that the above preparation method is merely an exemplary example, and they can obtain other compound structures of the present invention by improving it.
[0067] The decomposition temperature and melting point of each example and comparative example were tested using thermogravimetric analysis (TGA) and differential scanning calorimetry (DSC), and the data are shown in Table 1:
[0068] Table 1
[0069] compound Thermal decomposition temperature (0.5%) (°C) Glass transition temperature (°C) Comparative Example 1 363 133 Comparative Example 2 345 125 Example 1 405 156 Example 2 414 166 Example 3 412 150 Example 4 436 165 Example 5 443 220 Example 6 440 215
[0070] The structural formulas for Comparative Example 1 and Comparative Example 2 are as follows:
[0071]
[0072] As can be seen from Table 1, the compound structures of the present invention all have high thermal decomposition temperature and glass transition temperature, which is beneficial to the thermal stability of the device, especially in high heat and high humidity reliability experiments, resulting in a longer device life.
[0073] Example 7:
[0074] To fabricate an organic electroluminescent substrate using the organic electroluminescent material of this invention, firstly, a transparent conductive ITO glass substrate is sequentially washed with deionized water, ethanol, acetone, and then deionized water, dried at 80°C, and then treated with oxygen plasma for 30 minutes. Then, it is deposited in a vapor deposition machine under a vacuum of <4*10⁻⁶. -4 A 20 nm thick HATCN layer was deposited as a hole injection layer under Pa; a 40 nm thick hole transport layer was formed by depositing compound HTL; a 10 nm thick EBL (electron blocking layer) was deposited on the hole transport layer; then a 25 nm thick EML (BH:BD = 97:3%, light-emitting layer) was deposited; and an ETL (electron transport layer) was deposited on the light-emitting layer. The electron transport layer was composed of two materials, ET and LiQ, wherein the ET material is the compound structure of the present invention (13). A 1 nm thick ytterbium metal was deposited as an electron injection layer and a 100 nm thick Ag metal was deposited as the device cathode.
[0075] The material structure used in the device is shown below:
[0076]
[0077] The organic electroluminescent devices of Examples 8-12 and Comparative Examples 1 and 2 were fabricated in the same way as those of Example 7, except that the ET materials were respectively Structure 21, Structure 24, Structure 39, Structure 60, Structure 96 of the present invention and Comparative Examples 1 and 2.
[0078] The value was measured at 10 mA / cm 2 The electrical and optical properties of the electroluminescent devices of Examples 7-12 and Comparative Examples 1 and 2 were measured, with a 50 mA / cm² value. 2 The device lifespan is shown in Table 2.
[0079] Table 2
[0080]
[0081]
[0082] As can be seen from Table 2, the compound structure of the present invention, when used as an electroluminescent device prepared by ETL, shows a decreasing voltage trend and a significantly improved lifetime.
[0083] Example 13:
[0084] Tandem OLED devices were fabricated using the organic electroluminescent material of this invention. First, a transparent conductive ITO glass substrate was sequentially washed with deionized water, ethanol, acetone, and then deionized water, dried at 80°C, and then treated with oxygen plasma for 30 minutes. Then, it was deposited in a vapor deposition machine under a vacuum of <4*10⁻⁶. -4 Under Pa conditions, 20 nm HATCN, 10 nm HTL, 5 nm EBL, 20 nm EML, 35 nm ET, 100 nm n-CGL, 10 nm HATCN, 10 nm HTL, 5 nm EBL, 20 nm EML, 35 nm ETL (ET:LiQ), 1 nm Yb, and 1000 nm Ag were deposited. n-CGL is ytterbium metal doped with 5% in compound structure 13 of this invention. HTL, EBL, EML, and LiQ are the same materials used in Example 7.
[0085] The ET material in this tandem OLED device structure is shown in the following structure:
[0086]
[0087] The organic electroluminescent devices of Examples 14-18 and Comparative Examples 1 and 2 were fabricated in the same way as in Example 13, except that the n-CGL materials were respectively doped with ytterbium in Structures 21, 24, 39, 60, and 96 of the present invention and in Comparative Examples 1 and 2.
[0088] The value was measured at 10 mA / cm 2 The electrical and optical properties of the electroluminescent devices of Examples 13-18 and Comparative Examples 1 and 2 were measured, with a 50 mA / cm² value. 2 The device lifespan is shown in Table 3.
[0089] Table 3
[0090]
[0091]
[0092] As can be seen from Table 3, the compound structure of the present invention, when used as a tandem OLED device prepared from n-CGL material, exhibits a lower voltage and a significantly improved lifetime compared to the comparative example.
Claims
1. An organic compound having a general structural formula as shown in one of (C2)-(C5): , , , R1-R4 are independently selected from hydrogen, deuterium, tritium, alkyl groups having 1 to 10 carbon atoms, and cycloalkyl groups having 1 to 20 carbon atoms; Ar1 and Ar2 are independently selected from C6 to C50 aryl groups.
2. The organic compound according to claim 1, wherein the aryl groups in Ar1 and Ar2 are C6 to C20 aryl groups.
3. The organic compound according to claim 1, wherein, Ar1 and Ar2 are each independently selected from phenyl, naphthyl, anthracene, phenanthryl, biphenyl, phenylnaphthyl, fluorenyl, and fluoranthracene.
4. The organic compound according to claim 3, wherein R1-R4 are independently selected from hydrogen, deuterium, tritium, alkyl groups having 1 to 6 carbon atoms, and cycloalkyl groups having 1 to 8 carbon atoms.
5. The organic compound according to claim 4, wherein R1-R4 are independently selected from hydrogen, deuterium, tritium, alkyl groups having 1 to 4 carbon atoms, and cycloalkyl groups having 1 to 6 carbon atoms.
6. The organic compound according to claim 1, wherein its structure is shown in one of the following formulas:
7. An organic electroluminescent device, comprising: First electrode and second electrode; It is placed between the first electrode and the second electrode and includes a first light-emitting stack, the first light-emitting stack including a hole transport layer, a light-emitting layer and an electron transport layer; It is placed between the first light-emitting stack and the second electrode and includes a second light-emitting stack, the second light-emitting stack including a hole transport layer, a light-emitting layer and an electron transport layer; A charge generation layer is placed between the first light-emitting stack and the second light-emitting stack; Wherein, at least one of the electron transport layer and the charge generation layer comprises an organic compound according to any one of claims 1 to 6.
8. The organic electroluminescent device according to claim 7, wherein, The charge generation layer includes an N-type charge generation layer and a P-type charge generation layer, and the organic compound is located in the N-type charge generation layer.
9. The organic electroluminescent device according to claim 8, wherein, The N-type charge-generating layer comprises the organic compound and an alkali metal or alkaline earth metal compound.
10. The organic electroluminescent device according to claim 9, further comprising: A third light-emitting layer is placed between the second light-emitting layer and the second electrode; A charge generation layer is placed between the second and third light-emitting layers; The charge-generating layer contains the organic compound.
11. A lighting or display element, characterized in that: Includes the organic electroluminescent device according to any one of claims 7-10.
Citation Information
Patent Citations
Phosphorescent OLED having double hole-blocking layers
CN101978528A
Organic light-emitting device
CN106910831A
Organic compound, light emitting diode including same and organic light emitting diode display
CN108218858A
Compound containing silicon spirofluorene unit, preparation method of compound and organic electroluminescent device
CN109897066A
Organic light emitting diode display device and preparation method thereof
CN110311050A