A reinforced concrete chloride ion directional absorption device and method

By using a measuring probe to detect resistivity and directional additives in a reinforced concrete chloride ion directional absorption device, the problems of filling body loss and magnesium alloy electrode corrosion are solved, directional repair and corrosion elimination are achieved, and the service life of the device is extended.

CN116641059BActive Publication Date: 2024-10-11NANJING HYDRAULIC RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310597528.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-10-11
Estimated Expiration
2043-05-25

AI Technical Summary

Technical Problem

The existing reinforced concrete chloride ion directional absorption device cannot observe the loss of the filling body from the outside and cannot be repaired directionally. Moreover, the magnesium alloy electrode is easy to rust, affecting the electrochemical activity and service life.

Method used

A device including a magnesium alloy electrode, a filling body and a mold box is designed. The resistivity of the filling body is detected by a measuring probe, additives in the filling body are directionally added to reduce rust products, and the humidity is monitored through a pulp layer and a humidity sensor to maintain the device. Cohesion.

Benefits of technology

It achieves directional repair of filling body loss and eliminates corrosion of magnesium alloy electrodes, prolongs the service life of the device, and ensures the chloride ion absorption effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116641059B_ABST
    Figure CN116641059B_ABST
Patent Text Reader

Abstract

The present invention discloses a reinforced concrete chloride ion directional absorption device and method, wherein a copper sheet is disposed on each of two oppositely disposed sides of a filling body, two measuring slots are disposed on the filling body between the two copper sheets, and a plurality of vertical additive injection channels are disposed in the filling body between the two measuring slots, the additive injection channels are disposed extending from the upper surface to the lower surface of the filling body, and the additive injection channels are disposed on both sides of a magnesium alloy electrode. The present invention can grasp the consumption of the filling body from the outside of the device through a measuring probe, and according to the measurement results, the consumed filling body is repaired in a directional manner by pouring additives into the additive injection channel, and the rust products of the magnesium alloy electrode can be eliminated in time on the basis of ensuring the chloride ion absorption effect, thereby extending the service life of the device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of reinforced concrete, and in particular relates to a reinforced concrete chloride ion directional absorption device and method. Background Art

[0002] The application number is 2014102808997, and the invention name is a device and method for directional absorption of chloride ions in reinforced concrete that is easy to install and replace. The device for directional absorption of chloride ions includes a magnesium alloy and a filling material that maintains the electrochemical activity of the magnesium alloy. The filling material is composed of gypsum powder, bentonite, sodium sulfate, active salt and water. Since the sulfuric acid solution of gypsum in the filling material will gradually decrease, it will affect the electrochemical activity of the magnesium alloy electrode, but the loss of the filling body cannot be seen from the outside of the device, and the filling material cannot be repaired in a direction. And because chloride ions and calcium ions easily cause magnesium alloy electrodes to rust after passing through the filling material, as the degree of rust increases, the external filling body needs to be disassembled regularly and the magnesium alloy electrode needs to be replaced. This application aims to reduce and eliminate the rust products of the magnesium alloy electrode and facilitate the replacement of the magnesium alloy electrode. Summary of the invention

[0003] The present invention aims to solve the technical problems that the existing device cannot check the loss of the filling body from the outside and cannot carry out directional repair, and provides a reinforced concrete chloride ion directional absorption device and method.

[0004] In order to solve the above technical problems, the present invention adopts the following solutions:

[0005] A reinforced concrete chloride ion directional absorption device comprises a magnesium alloy electrode, a filler for maintaining the electrochemical activity of the magnesium alloy electrode, and a mold box for containing the magnesium alloy electrode and the filler, wherein the mold box is installed on the surface of the reinforced concrete, the magnesium alloy electrode is buried in the middle of the filler in the mold box, the filler is a cubic structure, comprising four side surfaces and upper and lower bottom surfaces, the lower bottom surface of the filler is in close contact with the surface of the reinforced concrete; a cathode cable is welded to the steel bar, an anode cable is welded to the magnesium alloy electrode, and the cathode cable is electrically connected to the anode cable.

[0006] There is a potential difference between the magnesium alloy electrode in the chloride ion directional absorption device and the steel bar electrode in the reinforced concrete. The potential of the steel bar electrode is relatively positive. The magnesium alloy electrode and the steel bar electrode constitute the negative electrode and positive electrode of the primary battery respectively. The chloride ions in the reinforced concrete move toward the magnesium alloy electrode, and the calcium ions in the filling body move toward the steel bar electrode. A current is formed in the anode cable and the cathode cable, flowing from the steel bar electrode to the magnesium alloy electrode, and the chloride ions in the reinforced concrete are directionally absorbed into the filling body, so that the steel bars are protected.

[0007] The filling material consists of gypsum powder, bentonite, sodium sulfate, active salt and water, wherein the weight percentage range of gypsum powder: bentonite: sodium sulfate: active salt: water is (55~65): (20~26): (3~4): (4~5): (6~11).

[0008] Due to the reaction with the electrode corrosion products, the effective ingredients in the filling material are gradually reduced, which will affect the electrochemical activity of the magnesium alloy electrode. However, the loss of the filling material cannot be seen from the outside of the directional absorption device, and the filling body cannot be repaired in a direction. Therefore, a copper sheet is provided on each of two oppositely arranged side surfaces of the filling body, and two measuring grooves are provided on the filling body between the two copper sheets. A plurality of vertical additive injection channels are provided in the filling body between the two measuring grooves. The additive injection channels extend from the upper surface to the lower surface of the filling body, and the additive injection channels are located on both sides of the magnesium alloy electrode.

[0009] The mold box is designed as a box structure with a bottom and a cover. Two long holes corresponding to the measuring slots are provided on the top cover of the mold box. The two long holes are arranged in parallel. A pouring hole connected to the additive injection channel is provided at a position corresponding to the additive injection channel on the top cover, and sealing covers are provided on the pouring hole and the two long holes. Two movable resistivity measuring probes are inserted into the measuring slot through the same long hole, so that the two probes extend into the mold box and are in close contact with the filling body, and the resistivity of the filling body between the two probes is measured, and the consumption of the filling body is judged by the measured resistivity value.

[0010] A sealing cover is provided on the pouring hole to prevent the additive from flowing out of the pouring hole. If it is determined that the filling body is consumed, the additive is injected into the additive injection channel near the consumed part. The additive is injected into the filling body in stages, 3 ml each time, and stays for 2 hours after each injection. After the additive seeps evenly in the filling body, the additive is continued to be injected into the filling body until the resistivity of the filling body reaches the target value.

[0011] The additive is composed of calcium sulfate solution, pure cellulose, air entraining agent, expanded glass particles and silica-based sand, and the mass ratio of the five components is (4~5): (0.2~0.3): (0.2~0.3): (0.2~0.3): (0.2~0.3).

[0012] Pure cellulose in the additive can increase the water retention capacity of the filling body, the air entraining agent can produce evenly distributed microbubbles, and the particle size of the expanded glass particles is between 1 and 4 mm to increase the porosity of the filling body; the particle size of the silica-based sand is less than 3 mm, which is mainly used to control the shrinkage risk of the filling body. Mixing the various components with the calcium sulfate solution in the above proportion and injecting the mixed calcium sulfate solution into the filling body can effectively reduce and eliminate the rust products of the magnesium alloy electrode.

[0013] Preferably, a pulp layer is provided between the bottom surface of the filling body and the reinforced concrete surface, and the chloride ion directional absorption device is adsorbed on the reinforced concrete surface through the pulp layer. A humidity sensor is provided in the pulp layer, and the humidity sensor has been treated for anti-seepage. The humidity sensor is connected to the PC end, and the humidity sensor converts the humidity inside the pulp into a resistance signal and transmits it to the PC end. The PC end converts this resistance signal into a digital signal to obtain real-time humidity data in the pulp. Initially, water is added to the pulp to keep its humidity at 100%, so that the humidity detection value of the humidity sensor is 100%, so as to ensure the cohesion of the chloride ion directional absorption device on the reinforced concrete surface. As time goes by, the detection value of the humidity sensor will decrease. When the detected value is lower than a certain threshold, it can be considered that water is added to the pulp layer. When it is necessary to change the installation position of the chloride ion directional absorption device on the reinforced concrete surface or remove it from the reinforced concrete surface, water is no longer continuously added to the pulp to reduce its humidity, so as to reduce the cohesion of the device on the reinforced concrete surface.

[0014] Preferably, one end of the anode cable extends out of the mold box and is connected to the cathode cable through a junction box, and a waterproof and sealed connection is adopted at the connection between the anode cable and the mold box.

[0015] The manufacturing method of the reinforced concrete chloride ion directional absorption device comprises the following steps:

[0016] Step 1, fixing the mold box body on the reinforced concrete surface;

[0017] Step 2, first fix a copper sheet on each of two opposite inner side walls of the box, then fill half of the filling material into the box and compact it, place the magnesium alloy electrode on the surface of the compacted filling material, so that the magnesium alloy electrode is equidistant from the inner walls of the box; connect the anode cable to the magnesium alloy electrode and extend it out of the box, and perform waterproof sealing treatment on the connection between the anode cable and the box; insert an insert block into the filling material on both sides of the magnesium alloy electrode and close to the inner wall of the box, insert multiple vertical additive casting pipes into the filling material between the two insert blocks, and arrange the multiple additive casting pipes at equal intervals, and then fill the remaining filling material into the box and compact it;

[0018] Step 3, seal the top cover of the mold box to the box body, make the long hole on the top cover correspond to the plug block, and perform waterproof sealing treatment on the connection between the top cover and the box body;

[0019] Step 4, connecting the anode cable and the cathode cable together through a junction box;

[0020] Step 5, after the filling body in the mold box is shaped, open the top cover, take out the insert, form two measuring grooves on the filling body, take out the additive pouring tube, form multiple vertical additive injection channels in the filling body, and connect the top cover to the box body again for waterproof sealing, and set openable sealing covers on the pouring hole and two long holes of the top cover.

[0021] Preferably, in order to increase and control the cohesion of the absorption device on the reinforced concrete surface, the following steps are also included before step 1:

[0022] A layer of paper pulp is brushed on the reinforced concrete surface, a humidity sensor is arranged in the paper pulp layer, a mold box is placed on the paper pulp layer, and the humidity sensor is located in the paper pulp layer between the bottom surface of the mold box and the reinforced concrete surface.

[0023] A method for directional repairing a reinforced concrete chloride ion directional absorption device: after the absorption device is installed on the reinforced concrete surface, two movable resistivity measuring probes are inserted into a measuring slot in the same long hole, so that the two probes extend into a mold box and are in close contact with a filling body, and the resistivity of the filling body between the two probes is measured, and the initial resistivity is measured at this time; after the absorption device is used for a period of time, the resistivity of the filling body between the two probes is measured in the same long hole by the same method, if the resistivity measured at this time is 1.2 times the initial resistivity, it is considered that the filling body between the two probes needs to be repaired, and additives are poured into additive injection channels at corresponding / adjacent positions until the resistivity is reduced to 1.05 times the initial resistivity, and it is considered that the filling body between the two probes is repaired.

[0024] The pure cellulose in the additive can increase the water retention capacity of the filling body, the air entraining agent can produce evenly distributed microbubbles, and the particle size of the expanded glass particles is between 1 and 4 mm to increase the porosity of the filling body; the particle size of the silica-based sand is less than 3 mm, which is mainly used to control the shrinkage risk of the filling body. Mixing the various components with the calcium sulfate solution in the above proportion and injecting the mixed calcium sulfate solution into the filling body can effectively reduce and eliminate the rust products of the magnesium alloy electrode.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] The present invention can grasp the consumption of the filler from the outside of the device through the measuring probe, and according to the measurement result, the additive is poured into the additive injection channel to carry out direction repair on the consumed filler, and on the basis of ensuring the chloride ion absorption effect, the rust products of the magnesium alloy electrode can be eliminated in time, thereby extending the service life of the device. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a cross-sectional view structure of the absorption device connected to the reinforced concrete surface;

[0028] Figure 2 It is a top view structure of the filling body. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Embodiment 1:

[0030] A reinforced concrete chloride ion directional absorption device comprises a magnesium alloy electrode 1, a filler 4 for maintaining the electrochemical activity of the magnesium alloy electrode, and a mold box 14 for containing the magnesium alloy electrode and the filler. The mold box is a bottomless and covered box structure, which is fixedly installed on the surface of reinforced concrete 6. The magnesium alloy electrode is buried in the middle of the filler in the mold box. The structure of the filler is a cube, including four side surfaces and upper and lower bottom surfaces. The lower bottom surface of the filler is in close contact with the surface of the reinforced concrete. Two oppositely arranged side surfaces of the filler are each provided with a copper sheet 11, which is in close contact with the filler. The upper ends of the two copper sheets can extend out of the box, such as Figure 1 As shown, it may not be extended. Two measuring slots 13 are provided on the filling body between the two copper sheets, and a plurality of vertical additive injection channels 5 are provided in the filling body between the two measuring slots 13, and the additive injection channels are extended from the upper surface to the lower surface of the filling body, and the additive injection channels 5 are located on both sides of the magnesium alloy electrode; two long strip holes corresponding to the measuring slots are provided on the top cover of the mold box, and the two long strip holes are arranged in parallel, and a pouring hole communicating with the additive injection channel is provided on the top cover at a position corresponding to the additive injection channel, and a sealing cover is provided on the pouring hole and the two long strip holes; two movable resistivity measuring probes 12 are inserted into the measuring slot through the same long strip hole, so that the two probes 12 extend into the mold box and are in close contact with the filling body, and the resistivity of the filling body between the two probes is measured; the cathode cable 9 is welded to the steel bar 7, and the anode cable 8 is welded to the magnesium alloy electrode 1, and the cathode cable and the anode cable are electrically connected through the junction box 10. The additive is composed of calcium sulfate solution, pure cellulose, air entraining agent, expanded glass particles and silica-based sand, and the mass ratio of the five components is (4~5): (0.2~0.3): (0.2~0.3): (0.2-0.3): (0.2-0.3). Embodiment 2:

[0031] The manufacturing method of the reinforced concrete chloride ion directional absorption device comprises the following steps:

[0032] Step 1, fix the mold box body on the reinforced concrete surface;

[0033] Step 2, first fix a copper sheet on each of the two inner side walls of the box body that are opposite to each other, then fill half of the filling material into the box and compact it, the filling material can be composed of gypsum powder, bentonite, sodium sulfate, active salt and water, wherein the weight percentage of gypsum powder: bentonite: sodium sulfate: active salt: water is in the range of (55-65): (20-26): (3-4): (4-5): (6-11). The filling material can also be the material described in the existing application number 2014102808997. The magnesium alloy electrode is placed on the surface of the compacted filling material, so that the magnesium alloy electrode is equidistant from the inner wall of the mold box, the anode cable is connected to the magnesium alloy electrode and extends out of the box, and the connection between the anode cable and the box is waterproof and sealed; an insert block is inserted into the filling material on both sides of the magnesium alloy electrode and close to the inner wall of the box, and multiple vertical additive pouring pipes are inserted into the filling material between the two insert blocks, and the multiple additive pouring pipes are arranged at equal intervals, and then the remaining filling material is loaded into the box and compacted;

[0034] Step 3, seal the top cover of the mold box to the box body, make the long hole on the top cover correspond to the plug block, and perform waterproof sealing treatment on the connection between the top cover and the box body;

[0035] Step 4, connecting the anode cable 8 and the cathode cable together through the junction box 10;

[0036] Step 5, after the filling body in the mold box is shaped, open the top cover, take out the plug, form two measuring grooves 13 on the filling body, take out the additive pouring pipe, form multiple vertical additive injection channels 5 in the filling body, and connect the top cover to the box body again to waterproof and seal, and set openable sealing covers on the pouring hole and two long holes of the top cover. Embodiment 3:

[0037] In this embodiment, based on the embodiment 1, a pulp layer 2 is provided between the bottom surface of the filling body 4 and the reinforced concrete surface, the chloride ion directional absorption device is adsorbed on the reinforced concrete surface through the pulp layer, and a humidity sensor 3 is provided in the pulp layer to monitor the humidity data in the pulp layer in real time. Embodiment 4:

[0038] Based on Example 2, this embodiment further includes the following steps before step 1:

[0039] A layer of paper pulp is brushed on the reinforced concrete surface, a humidity sensor is set in the paper pulp layer, and a mold box is placed on the paper pulp layer so that the humidity sensor is located in the paper pulp layer between the bottom surface of the mold box and the reinforced concrete surface. Embodiment 5:

[0040] A method for directional repairing the reinforced concrete chloride ion directional absorption device, after the absorption device is installed on the reinforced concrete surface, two movable resistivity measuring probes 12 are inserted into the measuring slot in the same long hole, so that the two probes extend into the mold box and are in close contact with the filling body, and the resistivity of the filling body between the two probes is measured, and the initial resistivity is measured at this time; after the absorption device is used for a period of time, the resistivity of the filling body between the two probes is measured in the same long hole by the same method, if the resistivity measured at this time is 1.2 times the initial resistivity, it is considered that the filling body between the two probes needs to be repaired, and additives are poured into the additive injection channel 5 at the corresponding / adjacent position until the resistivity is reduced to 1.05 times the initial resistivity, and it can be considered that the filling body between the two probes is repaired.

[0041] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A reinforced concrete chloride ion directional absorption device, comprising a magnesium alloy electrode, a filler (4) for maintaining the electrochemical activity of the magnesium alloy electrode, and a mold box (14) for containing the magnesium alloy electrode and the filler, the mold box (14) being installed on the surface of the reinforced concrete (6), the magnesium alloy electrode (1) being buried in the middle of the filler in the mold box, the filler being a cubic structure, comprising four side surfaces and an upper and lower bottom surface, the lower bottom surface of the filler being in close contact with the surface of the reinforced concrete; a cathode cable (9) being welded to a steel bar (7), an anode cable (8) being welded to the magnesium alloy electrode (1), the cathode cable being electrically connected to the anode cable; and characterized in that: The mold box is a box structure without a bottom and with a cover, wherein two oppositely disposed side surfaces of the filling body are each provided with a copper sheet (11), two measuring slots (13) are provided on the filling body between the two copper sheets, and a plurality of vertical additive injection channels (5) are provided in the filling body between the two measuring slots (13), the additive injection channels extending from the upper surface to the lower surface of the filling body, and the additive injection channels (5) are located on both sides of the magnesium alloy electrode; The top cover of the mold box is provided with two long holes corresponding to the measuring slots, the two long holes are arranged in parallel, a pouring hole communicating with the additive injection channel is provided at a position corresponding to the additive injection channel on the top cover, and sealing covers are provided on the pouring hole and the two long holes; Two movable resistivity measuring probes (12) are inserted into the same long hole into the measuring groove, so that the two probes extend into the mold box and are in close contact with the filling body, and the resistivity of the filling body between the two probes is measured.

2. A reinforced concrete chloride ion directional absorption device according to claim 1, characterized in that: A pulp layer (2) is provided between the bottom surface of the filling body (4) and the reinforced concrete surface. The chloride ion directional absorption device is adsorbed on the reinforced concrete surface through the pulp layer. A humidity sensor (3) is provided in the pulp layer to monitor humidity data in the pulp layer in real time.

3. A reinforced concrete chloride ion directional absorption device according to claim 1, characterized in that: The additive is composed of calcium sulfate solution, pure cellulose, air entraining agent, expanded glass particles and silica-based sand, and the mass ratio of the five components is (4~5): (0.2~0.3): (0.2~0.3): (0.2-0.3): (0.2-0.3).

4. A reinforced concrete chloride ion directional absorption device according to claim 1, characterized in that: One end of the anode cable (8) extends out of the mold box (14) and is connected to the cathode cable through a junction box (10). The connection between the anode cable and the mold box (14) is sealed with a waterproof connection.

5. The method for manufacturing the reinforced concrete chloride ion directional absorption device according to claim 1, characterized in that: The following steps are involved: Step 1, fixing the mold box body on the reinforced concrete surface; Step 2, first fix a copper sheet on each of two opposite inner side walls of the box, then fill half of the filling material into the box and compact it, place the magnesium alloy electrode on the surface of the compacted filling material, so that the magnesium alloy electrode is equidistant from the inner walls of the box; connect the anode cable to the magnesium alloy electrode and extend it out of the box, and perform waterproof sealing treatment on the connection between the anode cable and the box; insert an insert block into the filling material on both sides of the magnesium alloy electrode and close to the inner wall of the box, insert multiple vertical additive casting pipes into the filling material between the two insert blocks, and arrange the multiple additive casting pipes at equal intervals, and then fill the remaining filling material into the box and compact it; Step 3, seal the top cover of the mold box to the box body, make the long hole on the top cover correspond to the plug block, and perform waterproof sealing treatment on the connection between the top cover and the box body; Step 4, connecting the anode cable (8) and the cathode cable together through a junction box (10); Step 5, after the filling body in the mold box is formed, open the top cover, take out the plug, form two measuring grooves (13) on the filling body, take out the additive pouring pipe, form multiple vertical additive injection channels (5) in the filling body, and connect the top cover to the box body again in a waterproof and sealed manner, and set openable sealing covers on the pouring hole and the two long holes of the top cover.

6. The method for manufacturing the reinforced concrete chloride ion directional absorption device according to claim 5, characterized in that: Before step 1, the following steps are also included: A layer of paper pulp is brushed on the reinforced concrete surface, a humidity sensor is arranged in the paper pulp layer, a box is placed on the paper pulp layer, and the humidity sensor is located in the paper pulp layer between the lower surface of the filling body and the reinforced concrete surface.

7. A method for directional repairing the reinforced concrete chloride ion directional absorption device according to claim 1, characterized in that: After the absorption device is installed on the reinforced concrete surface, two movable resistivity measuring probes (12) are inserted into the measuring slot in the same long hole, so that the two probes (12) extend into the mold box and are in close contact with the filling body, and the resistivity of the filling body between the two probes is measured. The initial resistivity is measured at this time. After the absorption device has been used for a period of time, the resistivity of the filling body between the two probes is measured in the same long hole by the same method. If the resistivity measured at this time is 1.2 times the initial resistivity, it is considered that the filling body between the two probes needs to be repaired, and additives are poured into the additive injection channel (5) at the corresponding / adjacent position until the resistivity is reduced to 1.05 times the initial resistivity. It can be considered that the filling body between the two probes is repaired.