Ceramic product and preparation method thereof

By introducing a high-density, low-porosity secondary alumina particle distribution into ceramic products and adjusting the catalyst loading, the problem of high loading cost is solved, and economical and efficient catalyst use is achieved.

CN116648306BActive Publication Date: 2024-11-12SAINT GOBAIN CERAMICS & PLASTICS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180088148.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-12-29
Filing Date
2021-12-17
Publication Date
2024-11-12
Estimated Expiration
2041-12-17

AI Technical Summary

Technical Problem

The high loading of catalytic active materials in existing catalyst supports leads to high costs and is not economically feasible in low-volume reactors. Furthermore, traditional support structures make it difficult to adjust the loading of active catalysts.

Method used

A ceramic product containing multiple first and second alumina particles, wherein the second alumina particles have low ZnI2 dye penetration test values, are randomly distributed in a continuous matrix to form a high-density, low-porosity region to adjust the catalyst loading and optimize the porosity and surface area ratio by controlling the particle ratio and distribution.

Benefits of technology

This reduces the amount of catalyst used while maintaining or increasing the operating rate, reduces the amount of precious metals used in the reactor, provides an economic advantage, and avoids the problem of carrier cracking during heat treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116648306B_ABST
    Figure CN116648306B_ABST
Patent Text Reader

Abstract

The present invention discloses ceramic articles such as catalyst supports, which include a continuous matrix and a dispersed phase distributed within the matrix as a plurality of discrete regions. The matrix and the discrete regions have different dye penetration test values. The present invention also relates to methods of making and characterizing the ceramic articles, and catalyst bodies including these ceramic articles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure generally relates to a ceramic article comprising a plurality of first alumina particles forming a continuous matrix and a plurality of second alumina particles dispersed within the matrix, wherein the first plurality of alumina particles and the second plurality of alumina particles have different dye penetration test values. The present disclosure also relates to a catalyst having a catalytically active material bonded to a surface of the ceramic article. BACKGROUND

[0002] Catalysts are usually prepared by impregnating a carrier (usually a ceramic product made of ceramic material) with a catalytically active material (e.g., metal). Catalysts having a too high weight ratio of catalytically active material to carrier may be undesirable in some aspects. For example, even if the catalyst has a long life due to the high loading of catalytically active material, if used in a reactor with a lower catalyst loading per unit volume in a desired reactor, the catalyst may be too expensive and economically infeasible. Therefore, there is a need in the art for a ceramic carrier for a catalyst, wherein the structure of the ceramic carrier allows the loading of active catalyst materials in the catalyst body to be adjusted. Summary of the invention

[0003] The present disclosure relates to a ceramic article comprising a rigid formation of alumina particles. The rigid formation comprises a plurality of first alumina particles and a plurality of second alumina particles. The two plurality of particles are randomly distributed throughout the rigid formation. The second alumina particles have a ZnI2 dye penetration test value of no more than 5 atomic %, and the ZnI2 dye penetration test value of the first alumina particles is at least twice the ZnI2 dye penetration test value of the second alumina particles. The rigid formation has a total cross-sectional area. Each plurality of particles occupies a portion of the total cross-sectional area, and the cross-sectional area of ​​the second alumina particles is between 5% and 50% of the total cross-sectional area.

[0004] In some aspects, the ZnI2 Dye Penetration Test value of the dispersed phase (i.e., the second alumina powder) of an embodiment of a ceramic article is lower than the ZnI2 Dye Penetration Test value of the continuous matrix (i.e., the first alumina powder). One embodiment relates to a ceramic article, wherein the ratio of the Dye Penetration Test value of the first alumina particles to the Dye Penetration Test value of the second alumina particles is at least 2:1. One embodiment relates to a ceramic article, wherein the Dye Penetration Test value is obtained by a method including one or more of a scanning electron microscope (SEM) and an energy dispersive X-ray spectroscopy (EDS). One embodiment relates to a ceramic article, wherein the penetration test value is determined by a ZnI2 dye penetration test. One embodiment relates to a ceramic article, wherein a plurality of first alumina particles forming a continuous matrix have a ZnI2 Dye Penetration Test value equal to or greater than 10 atomic %. One embodiment relates to a ceramic article, wherein a plurality of second alumina particles forming a dispersed phase have a ZnI2 Dye Penetration Test value equal to or less than 5 atomic %.

[0005] In some aspects, embodiments of the ceramic article have a thickness of about 0.2 cm 3 / g and about 0.7cm 3 One embodiment relates to a ceramic article wherein the total pore volume is between about 0.3 cm 3 / g and about 0.6cm 3 One embodiment relates to a ceramic article, wherein the total pore volume of the ceramic article is about 0.35 cm 3 / g and about 0.5cm 3 One embodiment relates to a ceramic article wherein the total surface area is about 0.4 m 2 / g and about 3m 2 One embodiment relates to a ceramic article wherein the total surface area is about 0.4 m 2 / g and about 1.5m 2 One embodiment relates to a ceramic article wherein the total surface area is about 0.5 m 2 / g and about 0.85m 2 / g.

[0006] The present disclosure also relates to a metal-based catalyst body comprising a metal deposited on a ceramic article as described herein. One embodiment relates to a catalyst body wherein the metal is silver. One embodiment relates to a catalyst body comprising silver deposited on a ceramic article comprising a continuous alumina matrix and a dispersed alumina phase distributed within the continuous alumina matrix as a plurality of discrete regions, wherein: the article has a 0.3 cm 3 / g and 0.6cm 3 / g and the total pore volume between 0.5m 2 / g and 0.85m 2 / g of total surface area; the continuous alumina matrix has a ZnI2 dye penetration test value equal to or higher than 10%, and the dispersed alumina phase has a ZnI2 dye penetration test value equal to or less than 5 atomic%, and the dispersed alumina phase covers 5% to 50% of the cross-sectional area of ​​the ceramic article.

[0007] One embodiment is directed to a method of making a ceramic article, wherein the first plurality of alumina particles and the second plurality of alumina particles comprise alpha-alumina. One embodiment is directed to a method of making a ceramic article, wherein the second plurality of alumina particles comprise fused alumina. One embodiment is directed to a method of making a ceramic article, wherein the second plurality of alumina particles comprise plate-like alumina. One embodiment is directed to a method of making a ceramic article, the ceramic article comprising a binding material and wherein the binding material is magnesium silicate. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] The foregoing summary, as well as the following detailed description of the invention, will be better understood when read in conjunction with the appended drawings.

[0009] Figure 1 The surface area and water absorption of the ceramics are shown as a function of the amount of dispersed phase.

[0010] FIG. 2A to FIG. 2C The microstructure of the article of the present invention is shown at magnifications of 100X, 250X, and 500X, respectively.

[0011] Figure 3A and Figure 3B Shown are SEM images of articles of the invention that have been mounted in epoxy, sectioned and polished to a 1 μm finish.

[0012] Figure 4A and Figure 4B Energy dispersive X-ray spectroscopy (EDS) data processing for ZnI2 dye penetration testing is shown.

[0013] Figure 5A and Figure 5B EDS data for another embodiment of the present invention is shown. DETAILED DESCRIPTION

[0014] The present disclosure generally relates to ceramic articles that can be used in various applications, including catalyst support applications, such as as a catalyst support for a catalyst for direct oxidation of ethylene to produce ethylene oxide. The ceramic articles described herein include at least a plurality of first alumina particles and a plurality of second alumina particles. The present disclosure also relates to methods of preparing articles from the first alumina particles and the second alumina particles.

[0015] Without wishing to be bound by any particular theory, it is believed that as described herein, a ceramic article for preparing a catalyst support can be provided that solves the problem of how to adjust the amount of active catalyst material to be loaded on the support, thereby providing an economically more competitive catalyst, wherein, for example, a lower catalyst loading based on volume is desired in the reactor. As described herein, adding a high-density (i.e., low-porosity) region throughout the silver impregnated catalyst enables the catalyst to simulate a higher working rate than that possible in an otherwise identical catalyst that does not include a low-porosity region, thereby being able to reduce the amount of silver in the reactor while maintaining the production rate of the reactor. In some embodiments, such adjustments can simulate a high working rate in a catalyst system, such as an ethylene oxidation (EO) catalyst system. By introducing a large, high-density / low-porosity region into the support, there is now an area in the support that the active catalyst material cannot penetrate. However, in the matrix region surrounding the large, high-density / low-porosity region, the ratio of water absorption to surface area remains unchanged, thereby maintaining the expected concentration and particle size of the active catalyst material in the matrix region. By maintaining the ratio of water absorption to surface area in the matrix region, the expected initial catalytic performance is maintained compared to a support without large, high density / low porosity regions, even though the total loading of active catalyst material on the support is now reduced. In situations where the expected life of the catalyst is relatively short such that the use of higher amounts of active catalyst material does not provide an advantage in catalyst life, the use of lower amounts of active catalyst material (e.g., silver) can provide economic advantages. In addition, it is desirable that the shrinkage of the alumina used in the support is appropriately matched to avoid cracking around one or more alumina particles during heat treatment of the support during manufacturing. The porosity introduced due to any cracking will change the ratio of water absorption to surface area of ​​the matrix phase, which may compromise some of the advantages provided by the present invention.

[0016] One embodiment relates to a ceramic article comprising a continuous matrix comprising a plurality of first alumina particles and a dispersed phase comprising a plurality of second alumina particles. The second alumina particles distributed within the continuous matrix may be referred to as a plurality of discrete domains. The dispersed phase has a different ZnI2 dye penetration test value than the continuous matrix, and in a cross-section of the ceramic article, the dispersed phase covers from about 8% to about 40% of the cross-sectional area of ​​the ceramic article.

[0017] As used herein, the term "ratio" is defined as the numerical relationship between a first quantity of a particular characteristic (such as weight, particle size, atomic %, surface area, fraction of a cross-sectional surface area, etc.) and a second quantity of the same characteristic. Several illustrative examples will now be provided. In a first example, in a mixture of two aluminum oxide powders having a total mass of 100 grams and consisting of a first aluminum oxide and a second aluminum oxide, wherein the amount of the first aluminum oxide is 95 grams and the amount of the second aluminum oxide is 5 grams, the ratio of the first aluminum oxide to the second aluminum oxide is 95:5. For convenience, the ratio may be written as 19:1. If the amount of each aluminum oxide is expressed as a percentage of the total aluminum oxide, the percentage of the first aluminum oxide is 95 weight percent and the percentage of the second aluminum oxide is 5 weight percent. In a second example, if the d of the first aluminum oxide is 19:1, the percentage of the second aluminum oxide is 5 weight percent. 50 The particle size is 10 microns and the d of the second aluminum oxide 50 The particle size is 150 microns, then the ratio is 10:150, which can be simplified to 1:15. This ratio requires that the d 50 The particle size is the first alumina d 50 In the third example, if the surface area of ​​the first aluminum oxide is 5m 2 / g and the surface area of ​​the second alumina is 0.5m 2 / g, the ratio is 5:0.5, which can be written as 10:1. This ratio requires that the surface area of ​​the first aluminum oxide is ten times the surface area of ​​the second aluminum oxide. In the fourth example, if the total cross-sectional surface area of ​​the article is 10cm 2 And the total cross-sectional surface area of ​​the product is only occupied by 8cm 2 The first powder and occupies 2cm 2 If the total cross-sectional surface area of ​​the article is 10 cm, the ratio of the cross-sectional surface area occupied by the first powder and the second powder is 8:2, which can be written as 4:1. This ratio requires that the cross-sectional surface area occupied by the first powder is four times the cross-sectional surface area occupied by the second powder. Expressed as a percentage, the first powder occupies 80% of the total cross-sectional surface area and the second powder occupies 20% of the total cross-sectional surface area. In the fifth example, if the total cross-sectional surface area of ​​the article is 10 cm 2 And the total cross-sectional surface area is only occupied by 5cm 2 The first powder and occupies 5cm 2 If the total cross-sectional surface area of ​​the article is 20 cm, the ratio of the cross-sectional surface area occupied by the first powder and the second powder is 5:5, which can be written as 1:1. In percentage, the first powder occupies 50% of the total cross-sectional surface area and the second powder occupies 50% of the total cross-sectional surface area. In the sixth example, if the total cross-sectional surface area of ​​the article is 20 cm 2 And the total cross-sectional surface area is only occupied by 19.0cm 2 The first powder occupies 1.0cm 2In one embodiment, the ratio of the cross-sectional surface area occupied by the first powder and the second powder is 19:1. In terms of percentage, the first powder occupies 95% of the total surface area and the second powder occupies 5% of the total surface area. Therefore, in embodiments where the ratio of the cross-sectional area of ​​the first aluminum oxide particles to the cross-sectional area of ​​the second aluminum oxide particles is between 1.0:1.0 and 19.0:1.0, the cross-sectional surface area of ​​the first aluminum oxide is between 50% and 95% of the total cross-sectional surface area, and the cross-sectional surface area of ​​the second aluminum oxide is between 50% and 5% of the total cross-sectional surface area.

[0018] One embodiment of the invention described herein is a ceramic article comprising a rigid formation of alumina particles, the alumina particles comprising a plurality of first alumina particles and a plurality of second alumina particles. The two plurality of particles are randomly distributed throughout the rigid formation. The second alumina particles have a ZnI2 dye penetration test value of no more than 5 atomic %, and the ZnI2 dye penetration test value of the first alumina particles is at least twice the ZnI2 dye penetration test value of the second alumina particles. Each plurality of particles occupies a portion of the total cross-sectional area of ​​the rigid formation. The second alumina particles cover about 8% to about 40% of the cross-sectional area of ​​the ceramic article, more preferably 10% to 30% of the total cross-sectional area. Catalytically active metals are dispersed on the first alumina particles and the second alumina particles.

[0019] Another embodiment of the invention described herein is a method for making an article comprising a rigid formation of alumina particles and a catalytically active metal in contact with the particles. The method comprises the following steps: providing a plurality of first alpha alumina particles having a known weight and a d between about 0.2 microns and 100 microns; 50 A plurality of second alpha alumina particles are provided, which have a known weight and are selected from fused alumina and plate-like alumina. The second alumina particles have a d between about 5 microns and 400 microns. 50 Particle size. The first alumina particle size 50 The particle size of the second alumina particle 50 The ratio of the particle sizes is between 1:4 and 1:40. The ratio of the first alumina weight to the second alumina weight is between 1:1 and 19:1. The plurality of alumina particles are mixed to form a mixture, wherein the particles are randomly distributed throughout the mixture. The mixture is formed into a plurality of ductile articles. The ductile articles are heated to a sintering temperature of the alumina particles, thereby forming each ductile article into a rigid formation of alumina particles, wherein the particles in each plurality of particles are randomly distributed throughout the rigid formation. A catalytically active metal is deposited on the first alumina particles and the second alumina particles.

[0020] As used herein, continuous matrix refers to a portion of a ceramic article that has relatively constant morphological properties throughout the article in any direction and at least over distances greater than the longest particle of the dispersed phase. When viewing a cross-section of the article, the continuous matrix appears as discrete regions surrounding the dispersed phase, which appear as individual, independent particles that rarely contact another particle of the dispersed phase. The definition of continuous matrix applies although some formulations may include pores that may introduce interstices in the matrix. References Figure 2C , region 212 is part of a continuous matrix, region 206 is a discrete region of dispersed phase, and region 218 is a pore region. This definition applies and is not negated by inappropriate choice of highly magnified visual inspection techniques, i.e., at certain magnifications and due to a very limited (highly magnified) field of view, regions of the matrix may appear discontinuous.

[0021] As used herein, dispersed phase refers to discrete regions that are generally isolated and segregated relative to the surrounding continuous matrix. Although some dispersed regions may be adjacent to, in contact with, or sintered with other dispersed regions (see, e.g., Figure 3A , showing adjacent discrete regions 302 and 304 of dispersed phase), but this definition of dispersed phase applies. Figure 5A As shown, region 501 is part of a continuous matrix, while region 502 is a discrete region in the dispersed phase.

[0022] The dispersed phase coverage of the cross section can be measured at a magnification between 100X and 250X, but any other suitable magnification can be used. In some embodiments, the cross-sectional area has a first dimension between about 0.6mm and about 1.5mm and a second dimension between about 0.45mm and about 1mm. In some embodiments, the first dimension can be length, and the second dimension can be width. In some embodiments, in the cross section of the ceramic article, most of the plurality of discrete regions appear to have a longest dimension between about 10μm and about 150μm. Without wishing to be bound by any particular theory, the size may include any size of the discrete region, such as Feret's diameter (see, e.g., Henk G. Merkus, Particle Size Measurements: Fundamentals, Practice, Quality; January 1, 2009; Springer, p. 15).

[0023] The penetration test value is determined using a ZnI2 solution penetration test as described below. The ZnI2 dye penetration test value of the dispersed phase is lower than the ZnI2 dye penetration test value of the continuous matrix. Typically, the ZnI2 dye penetration test value is obtained by subjecting the ceramic article to a ZnI2 dye penetration test using a solution containing ZnI2. When the ceramic article is contacted with the ZnI2 solution, for example, by sinking the article into the solution, the solution will be absorbed into the ceramic article. The solution includes chemical compounds, which once absorbed into the ceramic article, can be determined to be absorbed into the article by various analytical methods.

[0024] Typically, the ZnI2 used to determine the penetration test value is dissolved in a suitable solvent such as water. One or more samples of the ceramic product are introduced into the resulting ZnI2 solution. Optionally, the solution with the ceramic material can be subjected to a vacuum, which can ensure that the solution penetrates better into the ceramic product. After removing the sample from the solution, it is dried to remove the solvent and leave the ZnI2 embedded in the ceramic product. The dried sample is fixed by placing the sample in a polymer or resin material. The sample can be optionally polished, cut, or both to provide a smooth cross-section of the ceramic product. The ceramic product sample is carbon coated and then analyzed by scanning electron microscopy (SEM) and / or energy dispersive X-ray spectroscopy. The penetration test value of the corresponding area can be calculated by calculating the amount of penetration test material in the continuous matrix and the dispersed phase.

[0025] In some embodiments, the difference in penetration test values ​​is at least 5%. In other embodiments, the difference in penetration test values ​​is at least 5.1%, at least 5.2%, at least 5.3%, at least 5.4%, at least 5.5%, at least 5.6%, at least 5.7%, at least 5.8%, at least 5.9%, at least 6%, at least 6.1%, at least 6.2%, at least 6.3%, at least 6.4%, at least 6.5%, at least 6.6%, at least 6.7%, at least 6.8%, at least 6.9%, at least 7%, at least 7.1%, at least 7.2%, at least 7.3%, at least 7.4%, at least 7.5%, at least 7.6%, at least 7.7%, at least 7.8%, at least 7.9%, at least 8.1%, at least 8.2%, at least 8.3%, at least 8.4%, at least 8.5%, at least 8.6%, at least 8.7%, at least 8.8%, at least 8.9%, at least 8. 4%, at least 7.5%, at least 7.6%, at least 7.7%, at least 7.8%, at least 7.9%, at least 8%, at least 8.1%, at least 8.2%, at least 8.3%, at least 8.4%, at least 8.5%, at least 8.6%, at least 8.7%, at least 8.8%, at least 8.9%, at least 9%, at least 9.1%, at least 9.2%, at least 9.3%, at least 9.4%, at least 9.5%, at least 9.6%, at least 9.7%, at least 9.8%, at least 9.9% or at least 10%.

[0026] In some embodiments, the ZnI2 Dye Penetration Test value of the first alumina is at least three times the ZnI2 Dye Penetration value of the second alumina.

[0027] In some embodiments, the ZnI2 Dye Penetration Test value of the first alumina is at least four times the ZnI2 Dye Penetration value of the second alumina.

[0028] In some embodiments, the ratio of the Dye Penetration Test value of the continuous matrix to the Dye Penetration Test value of the dispersed phase is at least 2.0. In other embodiments, the ratio of the Dye Penetration Test value of the continuous matrix to the Dye Penetration Test value of the dispersed phase is at least 2.1, at least 2.2, at least 2.3, at least 2.4, at least 2.5, at least 2.6, at least 2.7, at least 2.8, at least 2.9, at least 3, at least 3.1, at least 3.2, at least 3.3, at least 3.4, at least 3.5, at least 3.6, at least 3.7, at least 3.8, at least 3.9, at least 4, at least 4.1, at least 4.2, at least 4.3, at least 4.4, at least 4.5, at least 4.6, at least 4.7, at least 4.8, at least 4.9 or at least 5.

[0029] In some embodiments, the continuous matrix has a ZnI2 penetration test value higher than 10%. In other embodiments, the continuous matrix has a ZnI2 penetration test value of at least 10%, at least 11%, at least 12%, at least 13%, at least 14%, at least 15%, at least 16%, at least 17%, at least 18%, at least 19%, at least 20%, at least 21%, at least 22%, at least 23%, at least 24%, at least 25%, at least 26%, at least 27%, at least 28%, at least 29%, at least 30%, at least 31%, at least 32%, at least 33%, at least 34%, at least 35%, at least 36%, at least 37%, at least 38%, at least 39%, at least 40%, at least 41%, at least 42%, at least 43%, at least 44%, at least 45%, at least 46%, at least 47%, at least 48%, at least 49% or at least 50%.

[0030] In some embodiments, the dispersed phase has a ZnI2 dye penetration test value equal to or less than 5%. In other embodiments, the dispersed phase has a ZnI2 dye penetration test value of less than 1%, less than 1.1%, less than 1.2%, less than 1.3%, less than 1.4%, less than 1.5%, less than 1.6%, less than 1.7%, less than 1.8%, less than 1.9%, less than 2%, less than 2.1%, less than 2.2%, less than 2.3%, less than 2.4%, less than 2.5%, less than 2.6%, less than 2.7%, less than 2.8%, less than 2.9%. , less than 3%, less than 3.1%, less than 3.2%, less than 3.3%, less than 3.4%, less than 3.5%, less than 3.6%, less than 3.7%, less than 3.8%, less than 3.9%, less than 4%, less than 4.1%, less than 4.2%, less than 4.3%, less than 4.4%, less than 4.5%, less than 4.6%, less than 4.7%, less than 4.8% or less than 4.9% ZnI2 dye penetration test value.

[0031] In some embodiments, the ceramic article has a thickness between about 0.2 cm 3 / g and about 0.7cm 3 In some embodiments, the ceramic article has a total pore volume between about 0.3 cm 3 / g and about 0.6cm 3 In some embodiments, the ceramic article has a total pore volume between about 0.35 cm 3 / g and about 0.5cm 3 / g. The total pore volume, median pore size and pore size distribution of the support can be measured by conventional mercury intrusion porosimetry equipment, in which liquid mercury is forced into the pores of the support. Greater pressure is required to force the mercury into smaller pores, and the measured value of the pressure increment corresponds to the volume increment in the pores penetrated and therefore to the size of the pores in the incremental volume. The pore size distribution and pore volume of alumina can be measured by mercury intrusion porosimetry using a Micromeritics 9520 Autopore IV (130° mercury contact angle, surface tension of mercury of 0.480 N / m, and correction for applied mercury compression), starting at 689 Pa and then increasing to 4.1×10 7 Pa. A minimum of one hundred data points is appropriate. As used herein, the median pore size is understood to mean the pore size corresponding to the point in the pore size distribution at which 50% of the total pore volume resides in pores having a pore size smaller (or larger) than that point.

[0032] In other embodiments, the ceramic article may have a thickness of about 0.20 cm 3 / g, about 0.21cm 3 / g, about 0.22cm 3 / g, about 0.23cm3 / g, about 0.24cm 3 / g, about 0.25cm 3 / g, about 0.26cm 3 / g, about 0.27cm 3 / g, about 0.28cm 3 / g, about 0.29cm 3 / g, 0.30cm 3 / g, about 0.31cm 3 / g, about 0.32cm 3 / g, about 0.33cm 3 / g, about 0.34cm 3 / g, about 0.35cm 3 / g, about 0.36cm 3 / g, about 0.37cm 3 / g, about 0.38cm 3 / g, about 0.39cm 3 / g, 0.40cm 3 / g, about 0.41cm 3 / g, about 0.42cm 3 / g, about 0.43cm 3 / g, about 0.44cm 3 / g, about 0.45cm 3 / g, about 0.46cm 3 / g, about 0.47cm 3 / g, about 0.48cm 3 / g, about 0.49cm 3 / g, 0.50cm 3 / g, about 0.51cm 3 / g, about 0.52cm 3 / g, about 0.53cm 3 / g, about 0.54cm 3 / g, about 0.55cm 3 / g, about 0.56cm 3 / g, about 0.57cm 3 / g, about 0.58cm 3 / g, about 0.59cm 3 / g, about 0.60cm 3 / g, about 0.61cm 3 / g, about 0.62cm 3 / g, about 0.63cm 3 / g, about 0.64cm 3 / g, about 0.65cm 3 / g, about 0.66cm 3 / g, about 0.67cm 3 / g, about 0.68cm 3 / g, about 0.69cm 3 / g or about 0.70cm 3 / g pore volume.

[0033] In some embodiments, the ceramic article has a thickness of about 0.4 m 2 / g and about 3m 2 In some embodiments, the ceramic article has a total surface area between about 0.4 m 2 / g and about 1.5m 2 In some embodiments, the ceramic article has a total surface area between about 0.5 m 2 / g and about 0.85m 2 / g total surface area.

[0034] A method for measuring the surface area of ​​ceramic articles will now be described. The specific surface area (SSA) of each ceramic article is determined using a gas adsorption analyzer according to the Brunauer-Emmett-Teller (BET) method, also referred to herein as "surface area", which uses liquid nitrogen to measure 5 points at 77 ° K. This method can be used to determine the SSA of thermally stable materials with type II or type IV nitrogen adsorption isotherms. The procedure follows the guidelines set by IUPAC (International Union of Pure and Applied Chemistry), which are also incorporated into ASTM and ISO standards, and the references are as follows: Thommes, M. et al., Physisorption of gases, with special reference to the evaluation of surface area and pore size distribution (IUPAC Technical Report). Pure Appl. Chem., 87 (9-10) (2015), pp. 1051-1069. Stephen Brunauer, PHEmmett, and Edward Teller, Adsorption of Gases in Multimolecular Layers. J. Am. Chem. Soc. 1938, 60, 2, 309-319. ASTM D3663-20 and ASTMC1069-09. ISO 9277:2010.

[0035] The surface area measurements included in this application were performed using a Micromeritics ASAP 2420 or ASAP 2460 with a test tube with a 20cc ball filled to the maximum level. The sample was degassed at 250°C for 2 hours, then cooled and backfilled with nitrogen. The sample tube was then loaded onto the analysis port and BET analysis was performed. The surface area was calculated by the BET equation. Five data points of N2 adsorption at relative pressures (P / Po) in the range of 0.05 to 0.30 were used for calculation, with the following relative pressures targeted: 0.100, 0.125, 0.175, 0.225, and 0.270 P / Po.

[0036] In other embodiments, the ceramic article has a thickness of about 0.5 m 2 / g, about 0.6m 2 / g, about 0.7m 2 / g, about 0.8m 2 / g, about 0.9m 2 / g, about 1m 2 / g, about 1.1m 2 / g, about 1.2m 2 / g, about 1.3m 2 / g, about 1.4m 2 / g, about 1.5m 2 / g, about 1.6m 2 / g, about 1.7m 2 / g, about 1.8m 2 / g, about 1.9m 2 / g, about 2m 2 / g, about 2.1m 2 / g, about 2.2m 2 / g, about 2.3m 2 / g, about 2.4m 2 / g, about 2.5m 2 / g, about 2.6m 2 / g, about 2.7m 2 / g, about 2.8m 2 / g, about 2.9m 2 / g or about 3.0m 2 / g total surface area.

[0037] As used herein, the "water absorption rate" of a carrier is determined using the following method. Two batches of 100 grams of carrier are weighed out using an analytical balance. The dry weight of each batch is recorded and the total dry weight (DW) of the combined batch is calculated. Each batch is placed in one of two stainless steel swing buckets, each of which has a size of 80 mm long × 60 mm wide × 70 mm high. The basket is composed of a 10-mesh stainless steel screen using a wire with a diameter of 0.889 mm (0.035 inches) and is suitable for use in an Eppendorf Swing Basket A-4-62 centrifuge, which can be obtained from Eppendorf North America in Hauppauge, New York, USA. The loaded wire basket is placed in a vacuum chamber and evacuated to 25 mm Hg for 2 minutes. The carriers are flooded with water until they are completely covered. Evacuate to 25 mm Hg again and hold for 2 minutes. Release the vacuum, and allow the chamber to return to atmospheric pressure and remain undisturbed for 2 minutes. The loaded wire basket is placed in an Eppendorf Swing Basket A-4-62 centrifuge and the loaded basket is spun at 300 revolutions per minute (rpm) for a total spin time of 1 minute. The carrier is emptied from the basket onto a single shallow dish, the weight of which has been pre-recorded. The centrifuge weight (CW) of the combined batch is calculated by weighing the dish with the carrier loaded thereon and subtracting the weight of the dish. The water absorption is determined by subtracting the dry weight (DW) from the centrifuge weight (CW) to obtain the difference, which is then divided by the dry weight (DW) and multiplied by 100.

[0038] As used herein, the bulk density of a powder is determined as follows. Using a 100mL graduated cylinder, weigh the graduated cylinder (A) to an accuracy of 0.01g, then place it on the platform of an automatic tap density analyzer and fix it. A certain volume of sample is added to the capacity of the graduated cylinder. The counter is set to 1000 taps and the tapping is started. When 1000 taps are completed, the volume (V) of the sample is read and recorded. The volume measurement value should be within 0.5mL. Weigh the sample and graduated cylinder (B) to an accuracy of 0.01g. The tapped bulk density can then be calculated as the weight of the powder (BA) divided by the recorded volume V.

[0039] In one embodiment, the ceramic article comprises a continuous alumina matrix and a dispersed alumina phase distributed within the matrix as a plurality of discrete domains, wherein the ceramic article has a thickness of about 0.3 cm 3 / g and 0.6cm 3 / g and the total pore volume between 0.5m 2 / g and 0.85m 2 / g; a majority of the plurality of discrete regions each have a size of about 10 μm to about 150 μm; the continuous alumina matrix has a ZnI2 dye penetration test value equal to or higher than 10%, and the dispersed alumina phase has a ZnI2 dye penetration test value equal to or less than 5%, and in a cross-section of the ceramic article having a first dimension between about 0.6 mm and about 1.5 mm and a second dimension between about 0.45 mm and about 1 mm, the dispersed alumina phase covers 5% to 50%, more preferably 8% to 40%, and even more preferably 10% to 30% of the cross-sectional area.

[0040] The present disclosure also relates to a catalyst comprising a metal deposited on a ceramic article as described herein. One embodiment relates to a catalyst wherein the metal is silver deposited on a ceramic article as described herein. The present disclosure relates to a method for adjusting the amount of metal loaded onto an article by changing the ratio between the amount of a first alumina powder used to prepare a carrier and the amount of a second alumina powder. Because the porosity of the dispersed phase is less than that of the continuous matrix (as reflected by the lower ZnI2 permeability test value of the dispersed phase), the dispersed phase has a lower metal catalyst loading than the continuous matrix. Therefore, by increasing the ratio of the dispersed phase to the continuous matrix in the ceramic article, the metal catalyst loading can be reduced, and conversely, by reducing the ratio of the dispersed phase to the continuous matrix in the ceramic article, the metal catalyst loading can be increased.

[0041] To produce the articles of the present invention, certain physical and chemical characteristics of the first alumina and the second alumina, particularly surface area and d 50 Particle Size. Powders useful in making articles of the present invention can be selected using the information in Table 1 and the following description as a guide.

[0042] Table 1

[0043]

[0044] Preferably, the first alumina powder is 50 The first alumina powder may be alpha alumina having a particle size between 0.2 microns and 100 microns, more preferably between 2 microns and 20 microns, and most preferably between 5 microns and 10 microns. The first alumina powder may be alpha alumina having a maximum firing temperature of about 1600°C and a surface area of ​​1 m 2 / g and 20m 2 / g, preferably between 1m 2 / g to 5m 2 / g and more preferably between 1m 2 / g to 2m 2 / g. The first alumina powder may contain internal pores that contribute significantly to its total surface area, the total surface area being a measure of the surface area contributed by the internal pores of the particle and the geometric surface area of ​​the particle. The first alumina powder should not be molten alumina nor plate-like alumina. As used herein, plate-like alumina is defined as alumina that has been heated to a temperature above 1,650°C and consists of plate-like crystals. As used herein, molten alumina is defined as calcined alumina that has been melted in an electric arc furnace, cooled, crushed and recast into a desired shape. Calcined alumina is alumina that has been heated at a temperature in excess of 1,050°C to drive off substantially all chemically bound water.

[0045] Preferably, the second alumina is alpha alumina selected from plate-like alumina and molten alumina. The second alumina powder is alpha alumina prepared in a process wherein the maximum firing temperature may be above the melting point of alumina (as in the case of molten alumina) or just below the melting point of alumina (as in the case of plate-like alumina). 50 The particle size may be between 5 microns and 400 microns, more preferably between 10 microns and 200 microns, and most preferably between 40 microns and 150 microns. Since the second alumina powder is fired at a temperature close to or above the melting point of alumina, the second alumina powder has very small internal pores. The lack of internal pores results in a lower total surface area than the first alumina powder of similar particle size because there are no internal pores that contribute to the total surface area. The second alumina powder that has not been subjected to a grinding process to reduce the particle size has a surface area of ​​0.2 μm. 2 / g and 2.0m 2 / g, preferably 0.10m 2 / g and 0.50m 2 / g, more preferably 0.14m 2 / g and 0.30m 2 / g of surface area.

[0046] Select the first aluminum oxide 50 Particle size and d of the second alumina 50 The ratio of the particle sizes can be used to control the total surface area of ​​an article made from the first alumina powder and the second alumina powder. As a general rule, the particle size of the first alumina powder should be much smaller than the particle size of the second alumina powder. Preferably, the d 90 Should be less than the d of the second aluminum oxide 10 More preferably, the first aluminum oxide has a d 95 Should be less than the d of the second aluminum oxide 05 Even more preferably, the first aluminum oxide has a d 99 Should be less than the d of the second aluminum oxide 01Preferably, the particle size distribution of the first alumina and the second alumina should be unimodal.

[0047] More specifically, the first alumina powder has a d 50 The particle size of the second alumina powder 50 The ratio of the particle size may be between 1:4 and 1:40, preferably between 1:5 and 1:20, more preferably between 1:8 and 1:15. These ratios indicate that the d 50 The particle size should not be larger than the first alumina powder. 50 The ratios also indicate that the d of the second alumina powder is not greater than 40 times, preferably not greater than 20 times, and more preferably not greater than 15 times. 50 The particle size should be the same as that of the first alumina powder. 50 At least 4 times, preferably at least 5 times, more preferably at least 8 times the particle size.

[0048] In addition to the absolute d 50 In addition to the particle size and their ratio, the surface area of ​​the first aluminum oxide powder and the second aluminum oxide powder can also be used to select powders that can be used to prepare the articles of the present invention. As a general rule, the surface area per gram of the first aluminum oxide powder should be much larger than the surface area per gram of the second aluminum oxide powder. More specifically, the ratio of the surface area of ​​the first aluminum oxide powder to the surface area of ​​the second aluminum oxide powder can be between 7:1 and 15:1, preferably between 5:1 and 10:1, and more preferably between 4:1 and 5:1. These ratios indicate that the surface area of ​​the first aluminum oxide powder should be no more than 15 times the surface area of ​​the second aluminum oxide powder, preferably no more than 10 times, and more preferably no more than 5 times. The ratio also indicates that the surface area of ​​the first aluminum oxide powder should be at least 7 times, preferably at least 5 times, and more preferably at least 4 times the surface area of ​​the second aluminum oxide powder.

[0049] The particles of the second alumina, which may be referred to herein as the dispersed phase, are randomly distributed throughout the continuous matrix phase. The second alumina particles are considered not to form a continuous phase if at least 70% of the second alumina particles visible in an SEM micrograph at the desired magnification of the article of the invention appear to be not in contact with other second alumina particles. The second alumina particles may appear to be physically isolated from other second alumina particles by a plurality of first alumina particles that completely or partially surround the second alumina particles.

[0050] In addition to the type of alumina, specific d 50In addition to the particle size and its ratio, the weight ratio of the first powder and the second powder can also be controlled to ensure that the cross-sectional area of ​​the second alumina particles is at least 5% to 50%, more preferably 8% to 40%, and even more preferably 10% to 30% of the total cross-sectional area of ​​the article. The weight ratio of the first alumina powder to the second alumina powder can be 15:1 to 1:1. Intermediate ratios of 14:1, 12:1, 10:1, 8:1, 7:1, 6:1, 5:1, 4:1, 3:1 and 2:1 are feasible.

[0051] One embodiment relates to a method of making a ceramic article, wherein the first alumina powder may be at least 85 wt% alpha-alumina. More preferably, the first alumina powder may be at least 90 wt%, 95 wt%, or 99 wt% alpha-alumina. One embodiment relates to a method of making a ceramic article, wherein the second alumina powder may be only molten alumina, only plate-like alumina, or a mixture of plate-like alumina and molten alumina.

[0052] As described herein, particle size was determined by laser scattering using a Horiba Particle LA-950 Laser Scattering Particle Size Distribution Analyzer. The analyzer uses the principles of Mie scattering theory to measure particle size and distribution in the range of 0.01 microns to 3000 microns. The median particle size, referred to herein as "d 50 ”, which means the particle size at which the equivalent spherical volume of particles larger than the median size is equal to that of particles smaller than the median size. The method includes adding 3 drops of 10% The solution was then dispersed by sonication, thereby breaking up the secondary particles into primary particles. This sonication was continued until d 50 There was no further change in the values, and when using the Horiba LA-950 particle size analyzer, typically 1 to 5 minutes of sonication were required.

[0053] In some embodiments, the method for preparing a ceramic article includes the use of a binding material, such as magnesium silicate. If desired, one or more optional additives may be included in the preparation of the ceramic article. For example, it may be desirable to include one or more additives to promote the formation of a shaped body and / or change one or more characteristics of the resulting ceramic article. Suitable additives may include any of a variety of known carrier additives, including but not limited to: binders, such as polyolefin oxides, cellulose, alkaline earth metal compounds such as magnesium silicate and calcium silicate, and alkali metal compounds; extrusion aids, such as petrolatum, hydrogenated oils, synthetic alcohols, synthetic esters, glycols, starches, polyolefin oxides, polyethylene glycols, and mixtures thereof; solvents, such as water; peptizing acids, such as monofunctional aliphatic carboxylic acids containing 1 to about 5 carbon atoms, such as formic acid, acetic acid and / or propionic acid; halogenated monofunctional aliphatic carboxylic acids containing 1 to about 5 carbon atoms, such as monochloro, dichloro and trichloroacetic acid, etc.; fluxes, adhesives, dispersants, burnout materials (also known as "pore formers"), strength enhancing additives, etc. It is well within the ability of one skilled in the art to select appropriate additives in appropriate amounts taking into account, for example, the preparation method and the desired properties of the resulting ceramic article.

[0054] In some embodiments, the method includes the use of formic acid. Formic acid can be used to stabilize the dispersion of particles in the mixture. In some embodiments, formic acid is added to the mixture at about 1% (w / w%), about 1.5% (w / w%), about 2% (w / w%), about 2.5% (w / w%), about 3% (w / w%), about 3.5% (w / w%), about 4% (w / w%), about 4.5% (w / w%), about 5% (w / w%), about 5.5% (w / w%), about 6% (w / w%), about 6.5% (w / w%), about 7% (w / w%) or about 7.5% (w / w%).

[0055] In some embodiments, the mixture also includes one or more thermally decomposable materials. The mixture may include thermally decomposable materials in an amount ranging from about 2% (w / w%) to about 40% (w / w%), or about 5% (w / w%) to about 30% (w / w%). Thermally decomposable materials can be used as pore formers. As used herein, thermally decomposable materials are solids in particle form. The thermally decomposable material is mixed with alumina powder before the heating step, for example, with a green mixture of at least two different types of alumina. Individual particles of thermally decomposable materials occupy a large number of small spaces in the mixture. Individual particles of thermally decomposable materials are removed by thermal decomposition during the heating step and / or the sintering step, thereby leaving holes in the ceramic product forming the carrier. Pores can also be referred to as multiple voids distributed throughout the ceramic product. In some embodiments, most of the holes made by using thermally decomposable materials are contained in a continuous matrix. For example, at least 50%, at least 60%, at least 70%, at least 80%, or at least 90% of the holes made by using thermally decomposable materials are contained in a continuous matrix.

[0056] The thermally decomposable material should not be dissolved in any other component used to prepare the ceramic article. Similarly, the thermally decomposable material should not dissolve any other component. Because the thermally decomposable material occupies a certain volume before the heating step, and the space occupied by the material generally remains unoccupied after the heating step is completed, the material is used as a pore former. The thermally decomposable material that can be used in the method of the present invention is generally an organic material. Suitably, the chemical formula of the organic material includes carbon and hydrogen. The thermally decomposable material can be a synthetic or naturally occurring material or a mixture thereof. Preferably, the thermally decomposable material can be an organic material having a decomposition temperature not greater than the sintering temperature of the alumina powder. This ensures that the thermally decomposable material is at least partially removed before or while sintering the alumina powder. In order to promote decomposition, the chemical formula of the thermally decomposable material can preferably include carbon, hydrogen and oxygen. The decomposition temperature can be reduced due to the presence of oxygen.

[0057] In some embodiments, the mixture also includes one or more naturally occurring thermally decomposable materials, which result in the formation of pores during burnout. As used herein, naturally occurring thermally decomposable materials do not include polymers in the formulation and do not include other processing aids. In contrast, naturally occurring thermally decomposable materials refer to burnout materials that are optionally included when preparing ceramic products to promote the forming of the formed body and / or change the porosity of the resulting ceramic products. Typically, the burnout material is burned out, sublimated or volatilized during drying, calcining and / or sintering. Examples of suitable burnout materials include, but are not limited to, crushed nut shells, such as pecans, cashews, walnuts, peaches, apricots and hazelnuts. Any other naturally occurring thermally decomposable material known in the art can be used. In some embodiments, the pore volume in the resulting ceramic product is no more than 0.1 mL / g due to the use of burnout materials. In some embodiments, the mixture does not contain naturally occurring thermally decomposable materials.

[0058] Thermally decomposable materials can be synthetic materials.Synthetic materials can be polymeric materials.It is not desirable to be bound by any particular theory, and as used herein, synthetic materials are expected to exclude naturally occurring thermally decomposable materials.Polymeric materials can be formed using emulsion polymerization, including suspension polymerization, which is generally preferred because polymers can be obtained in the form of fine particles directly used as thermally decomposable materials.Preferably, polymeric materials can be formed using anionic polymerization.Polymeric materials can be olefin polymers and copolymers, for example, polyethylene, polypropylene, polystyrene, polyvinyl alcohol, ethylene-vinyl acetate and ethylene-vinyl alcohol copolymers, diene polymers and copolymers such as polybutadiene, EPDM rubber, styrene-butadiene copolymers and butadiene-acrylonitrile rubber, polyamides such as polyamide-6 and polyamide-66, polyesters such as polyethylene terephthalate.Preferably, polymeric materials can be hydrocarbon polymers, such as polyolefins, more preferably polypropylene.

[0059] The thermally decomposable material may be sieved or otherwise classified to limit the size of individual particles to a particular size range. If desired, a first thermally decomposable material having particles within a first size range may be combined with a second thermally decomposable material having particles within a second size range to obtain a multimodal distribution of pore sizes in the porous ceramic article. The limitation on the size range is determined by the size of the pores created in the porous ceramic article of the support.

[0060] In some embodiments, the mixture also comprises one or more polymers or copolymers selected from hydroxypropyl methylcellulose, vinyl chloride copolymers, vinyl acetate copolymers, olefin polymers, olefin copolymers, polyethylene, polypropylene, polystyrene, polyvinyl alcohol, ethylene-vinyl acetate copolymers, ethylene-vinyl alcohol copolymers, diene polymers, diene copolymers, polybutadiene, ethylene propylene diene monomer (EPDM) rubber, styrene-butadiene copolymers, butadiene acrylonitrile rubber, polyamide, polyamide-6, polyamide-66, polyester, polyethylene terephthalate, hydrocarbon polymers, polyolefins and polypropylene. The one or more polymers or copolymers can be used as lubricants and / or pore formers.

[0061] The carrier body can be formed by the mixture by any convenient forming method, such as spray drying, agglomeration or compression, and preferably they are formed by extrusion of the mixture. For applicable methods, reference can be made to, for example, U.S. Patents 5,145,824, 5,512,530, 5,384,302, 5,100,859 and 5,733,842, each of which is incorporated herein by reference. In order to promote such forming methods, especially extrusion, the mixture can be appropriately compounded with 2% w / w to 25% w / w, preferably 5% w / w to 15% w / w of processing aids. Processing aids (also referred to as the term "extrusion aids") are known in the art, such as "Kirk-Othmer Encyclopedia of Chemical Technology", 4th edition, volume 5, page 610. Suitable processing aids are generally liquid or greasy substances, such as vaseline, hydrogenated oil, synthetic alcohol, synthetic ester, glycol or polyolefin oxide. Boric acid may also be added to the mixture, for example in an amount up to 0.5% w / w%, more typically in an amount of 0.01% w / w% to 0.5% w / w%.All formulation weights are based on the total weight of ceramics such as alumina and zirconia in the mixture.

[0062] In some embodiments, the method further comprises extruding the mixture before calcining and / or sintering. In some embodiments, the method further comprises forming the mixture into one or more discrete bodies before calcining and / or sintering; for example, the mixture can be formed into a carrier body. Typically, the size of the carrier body is determined by the size of the reactor in which they are to be deposited. However, it is generally found that the use of carrier bodies in the form of cylinders, spheres, donuts, etc. is very convenient. The cylinders can be solid or hollow, straight or curved, and they can have a length of 4mm to 20mm, typically 5mm to 15mm, an outer diameter of 4mm to 20mm, typically 5mm to 15mm, and an inner diameter of 0.1mm to 6mm, typically 0.2mm to 4mm. The ratio of the length to the outer diameter of the cylinder can be in the range of 0.5 to 2, typically 0.8 to 1.2.

[0063] The formed parts can be made into various shapes, such as cylindrical, spherical, annular or multi-lobed. For example, a continuous rod of extruded paste can be formed by cutting the rod into pellets of the desired size. A ring-based molded structure (such as a "carriage wheel") of any desired configuration or any other extruded shape with a constant cross-section (such as, for example, a multi-lobed structure and a small honeycomb body) can be formed by extruding the paste through a properly shaped die and then cutting the rod into pellets of a constant cross-section. The molded product can also be a large honeycomb monomer form. However, the extrusion / pressing method is not limited to these shapes. The part may have an outer diameter of about 0.8 mm to about 25 mm or an average width when it is non-circular, but other sizes may also be formed. Reference may be made to U.S. Patent Publication 2012 / 0171407, which is incorporated herein by reference, for further describing the multi-lobed carrier. In addition, the size of the ceramic product carrier is generally not limited, and may include any size suitable for a catalytic reactor (e.g., an ethylene oxidation reactor). For example, the ceramic product support can be in the shape of a cylinder having a length of 5 to 15 mm, an outer diameter of 5 to 15 mm, and an inner diameter of 0.2 to 4 mm. In some embodiments, the ceramic product support can have a length-to-outer diameter ratio of 0.8 to 1.2. In addition, the ceramic product support can be in the shape of a hollow cylinder having a wall thickness of 1 to 7 mm. With the benefit of the present disclosure, those skilled in the art will be able to select a ceramic product support of a suitable shape and size, for example, taking into account the type and configuration of the catalytic reactor in which the ceramic product support will be used, such as the length and inner diameter of the tube within the catalytic reactor.

[0064] In some embodiments, the method also includes drying the molded body. The formed molded body can be dried to remove at least a portion of the water present (if any). Water may be converted into steam during the heating step described below and adversely affect the physical integrity of the molded body. Can be dried after preparing the mixture and optionally forming the mixture into a plurality of molded bodies. The drying step can be combined with the heating step by controlling the thermal curve of the oven or kiln. Drying can be carried out between 20°C and 400°C, or between 30°C and 300°C, typically for up to about 100 hours, and preferably from about 5 minutes to about 50 hours. Typically, drying is carried out to the extent that the mixture contains less than 2% w / w of water.

[0065] Calcination and / or sintering are generally carried out at a sufficiently high temperature and for a sufficiently long time, lasting up to about 100 hours, and preferably from about 5 minutes to about 50 hours. In some embodiments, calcination and / or sintering may be carried out at one or more temperatures, one or more pressures, and for one or more time periods sufficient to sinter at least 50%, or at least 75%, or at least 85%, or at least 90%, or at least 95% of a mixture of at least two types of alumina. In some embodiments, the method includes heating the mixture at a temperature of at least 1200°C. In some embodiments, the method includes heating the mixture at a temperature of up to 1600°C. In some embodiments, the method includes heating the mixture at a temperature between about 1200°C and about 1600°C. Calcination and / or sintering may be carried out in any suitable atmosphere, including but not limited to air, nitrogen, argon, helium, carbon dioxide, water vapor, and the like. In those embodiments in which the shaped body also includes an organic burnout material, at least one of the heating and / or calcining is carried out at least partially or entirely in an oxidizing atmosphere, such as in an oxygen-containing atmosphere. As used herein, calcining and / or sintering refers to the process of firing and consolidating a green body made and formed from powder particles. The particles bond with adjacent particles to form a rigid formation of alumina particles. Voids may exist between particles and / or within particles and together contribute to the porosity of the ceramic article.

[0066] After calcination and / or sintering, the resulting ceramic article may be optionally washed and / or treated before depositing the active catalytic material. Likewise, if desired, any raw materials used to form the ceramic article may be washed and / or treated before calcination and / or sintering. Any method known in the art for washing and / or treatment may be used according to the present disclosure, provided that such method does not negatively affect the performance of the resulting support or catalyst. For descriptions of such methods, reference is made to U.S. Patents 6,368,998, 7,232,918, 7,741,499 and WO 2007 / 092022, each of which is incorporated herein by reference. If washing is required, it is generally carried out at a temperature of 15° C. to 120° C. for up to about 100 hours and preferably for a time of about 5 minutes to about 50 hours. Washing may be carried out in a continuous or batch manner. Examples of suitable washing solutions may include, but are not limited to, water (e.g., deionized water), aqueous solutions containing one or more salts (e.g., ammonium salts), amine solutions (e.g., ethylenediamine), organic diluent aqueous solutions, and combinations thereof. Similarly, suitable aqueous solutions may be acidic, alkaline, or neutral. The amount of washing solution should be such that the ceramic article is impregnated until the incipient wetness point of the ceramic article is reached. Alternatively, a larger amount may be used, and excess solution may be removed from the wet ceramic article, for example, by centrifugation. In addition, after any washing and / or treatment steps, and preferably before depositing the catalytic article, the ceramic article is dried or calcined. For example, the ceramic article may be dried in a stream of air, for example, at a temperature of about 80° C. to about 400° C., for a sufficient period of time.

[0067] The formed ceramic article can be used directly as a catalyst, or as a catalytic support after the shaped body is impregnated with a solution of a catalytically active substance during or after its formation and optionally activated by a suitable post-treatment. Suitable catalytically active substances include transition metal elements, such as those from Groups VB, VIIIB and IB of the Periodic Table of Elements, for example vanadium, gold, platinum group metals, etc. In some embodiments, the metal is a catalytically active metal, including, for example, silver, cobalt, ruthenium and / or iron. In particular, silver is a preferred metal. Exemplary applications in which the support can be used include direct ethylene oxidation, but the ceramic article is intended to be used in any application.

[0068] Example

[0069] Methods for making supports for epoxidation reactions are described in many publications, including US 5,100,859 and US6,831,037, which are incorporated herein by reference. For example, see the disclosure in US 5,100,859, which begins at column 2, line 6 and continues to column 6, line 43. The following examples describe some embodiments of the present invention in more detail. These examples are provided for illustrative purposes only and should not be considered to limit the present invention. Support A is a comparative example. Supports B, C, D and E are embodiments of the present invention described herein.

[0070] Carrier A (Comparative Example)

[0071] Carrier A (i.e., the comparative carrier in the present disclosure) was prepared according to the teaching of US 5,100,859 (Gerdes) with respect to carrier L disclosed therein, but with the following modifications. The only alumina powder used in comparative carrier A had a d 50 Particle size, 1.4m 2 / g surface area, 0.78g / cc bulk density, and will be referred to herein as the first plurality of alumina particles. The first plurality of alumina particles are combined with zirconium oxide, magnesium silicate, walnut shell powder, boric acid and an extrusion aid. The combination of the first plurality of alumina particles, zirconium oxide, magnesium silicate and walnut shell powder is defined herein as a dry mixture of carrier A. The combined weight of the dry mixture with water, boric acid and extrusion aid is defined herein as a wet mixture of carrier A, which is extruded to form a hollow cylinder, then dried and fired. In carrier A, the first plurality of alumina particles form a single continuous matrix phase throughout the carrier. Carrier A does not contain a dispersed phase. The physical and chemical characteristics of the fired cylinder, which may be referred to as a ceramic article, carrier or support, are determined using the above-mentioned analytical techniques. The water absorption of carrier A is 48.7g / g, and the surface area is 0.78m 2 / g.

[0072] Vector B (embodiment of the present invention)

[0073] Carrier B is an embodiment of the present invention and was prepared according to the method described immediately above for preparing comparative Carrier A, except that 10 weight percent of the dry mixture of Carrier A was replaced with an equal mass of a plurality of fused alumina particles (referred to herein as a second plurality of alumina particles) to form a dry mixture of Carrier B. The second plurality of alumina particles had a d of 119.7 microns. 50 , 0.2m 2 / g surface area and a bulk density of 2.1 g / cc. The dry mixture of Carrier B was combined with water, boric acid, and an extrusion aid to produce a wet mixture of Carrier B, which was then extruded to form a hollow cylinder, which was dried and fired. The physical and chemical characteristics of the fired cylinders were determined. Carrier B had a water absorption of 46.70 g / g and a surface area of ​​0.74 m 2 / g.

[0074] Carrier C (embodiment of the present invention)

[0075] Carrier C is an embodiment of the present invention and is prepared according to the method described above for preparing Carrier A, except that 25 weight percent of the dry mixture of Carrier A is replaced with an equal mass of a plurality of fused alumina particles (referred to herein as a second plurality of alumina particles) to form a dry mixture of Carrier C. The second plurality of alumina particles has a d of 119.7 microns. 50 , 0.2m 2 / g surface area and a bulk density of 2.1 g / cc. The dry mixture of Support C was combined with water, boric acid, and an extrusion aid to produce a wet mixture of Support C, which was then extruded to form a hollow cylinder, which was dried and fired. The physical and chemical characteristics of the fired cylinders were determined. Support C had a water absorption of 42.86 g / g and a surface area of ​​0.63 m 2 / g.

[0076] Vector D (embodiment of the present invention)

[0077] Carrier D is an embodiment of the present invention and is prepared according to the method described above for preparing Carrier A, except that 40 weight percent of the dry mixture of Carrier A is replaced with an equal mass of a plurality of fused alumina particles (referred to herein as a second plurality of alumina particles) to form a dry mixture of Carrier D. The second plurality of alumina particles has a d of 119.7 microns. 50 , 0.2m 2 / g surface area and a bulk density of 2.1 g / cc. The dry mixture of Support D was combined with water, boric acid, and an extrusion aid to produce a wet mixture of Support D, which was then extruded to form a hollow cylinder, which was dried and fired. The physical and chemical characteristics of the fired cylinders were determined. Support D had a water absorption of 37.70 g / g and a surface area of ​​0.53 m 2 / g.

[0078] Vector E (embodiment of the present invention)

[0079] Carrier E is an embodiment of the present invention and is prepared according to the method described above for preparing Carrier A, except that 50 weight percent of the dry mixture of Carrier A is replaced with an equal mass of a plurality of fused alumina particles (referred to herein as a second plurality of alumina particles) to form a dry mixture of Carrier E. The second plurality of alumina particles has a d of 119.7 microns. 50 , 0.2m 2 / g surface area and a bulk density of 2.1 g / cc. The dry mixture of Support E was combined with water, boric acid, and an extrusion aid to produce a wet mixture of Support E, which was then extruded to form hollow cylinders, which were dried and fired. The physical and chemical characteristics of the fired cylinders were determined. Support E had a water absorption of 35.64 g / g and a surface area of ​​0.43 m 2 / g.

[0080] Figure 1 The surface area and water absorption of the support are shown to be dependent on the amount of dispersed phase alumina in the support. Curve 101 shows the relationship between the surface area of ​​the support and the weight percentage of the dispersed phase, which is calculated as a percentage of the dry mixture of support A. Curve 102 shows the relationship between the water absorption of the support and the weight percentage of the dispersed phase, which is calculated as a percentage of the dry mixture of support A.

[0081] FIG. 2A to FIG. 2C The backscattered electron (BSE) micrograph shows the microstructure of the ceramic product of the present invention. Figure 2A , Figure 2B and Figure 2C The second alumina powder phase (respectively Figure 2A , Figure 2B and Figure 2C The second alumina powder has a particle size that is significantly larger than the first alumina powder. Figure 2A The magnification is 100X. Figure 2B The magnification is 250X. Figure 2C The magnification is 500X.

[0082] Figure 3A and Figure 3BIdentification of dispersed phase particles in a polished cross section of a ceramic article that was epoxy-fixed and polished to a 1 micron finish is shown. The samples were gold coated using a SPI sputter coater to prevent charging. Images were generated with a Zeiss Merlin SEM using an accelerating voltage of 2 keV and a beam current of 100 pA. The type of SEM used is not critical but needs to be able to produce images suitable for image analysis software to identify and separate the dispersed phase. For larger sized diluent particles, SEM images were obtained at 100X magnification (see Figure 3A ), and for smaller sized diluent particles, SEM images were obtained at 250X magnification to obtain a particle count of ≥100 in each image. Image analysis software was used to identify, separate and isolate the dispersed phase particles. See Figure 3B . ImageJ software, an open source image processing program developed by the National Institutes of Health and the Laboratory for Optical and Computational Instrumentation and available for download at imageJ.net, was used to perform the analysis, determine the total area coverage of the dispersed phase in each image, and the Feret mean particle size for each image. The type of image analysis software used is not critical, and one skilled in the art will be familiar with the image processing necessary to identify and separate the dispersed phase. The area coverage of the dispersed phase was determined for four images of carrier E and one image of carrier C. The area coverage of the dispersed phase was determined from these images to be in the range of 9% to 23%. The data in Table 2 show that the area coverage of carrier C was 9.1%, while the area coverage of the four images of carrier E was approximately 20%.

[0083] Table 2

[0084] 100x magnification

[0085]

[0086] The ZnI2 dye penetration test value is determined using the following ZnI2 solution penetration test. First, 220g of ZnI2 is placed in 1,000mL of water at 20°C to form a ZnI2 solution. 5g of the ceramic product sample is introduced into 100mL of the ZnI2 solution. The container containing the ceramic product sample in the solution is placed in a container under vacuum for 20 hours. The sample is removed from the solution, dried at 50°C for 24 hours, and then dried at 110°C for a minimum of 2 hours. The dried sample is fixed in epoxy resin within 30 minutes of being removed from the drying oven to avoid re-absorption of water. After the epoxy resin is cured, the sample is polished to a 3 micron finish and kept in a drying oven at 100°C.

[0087] The distribution of iodide on the alumina particles was characterized using a S4300 SEM manufactured by Hitachi and an EDS detector manufactured by Oxford Instruments, an Aztec SEM system using an X-MaxN 150 detector, and Aztec version 3.3SP1 software. The polished samples were carbon coated to prevent charging. SEM-EDS images were taken within the parameter range shown in Table 3.

[0088] Table 3

[0089]

[0090] EDS data was collected using manually selected areas that included at least one of the second alumina particles and an equivalent area of ​​the first alumina particle. The EDS software was then able to generate the concentrations of iodine and zinc in the corresponding areas. Although both iodine and zinc concentrations can be used to compare the amount of penetration, iodine is preferred.

[0091] The region of the second alumina particle as one particle in the dispersed phase is Figure 4A 4 is depicted as region 402. The amount of iodine in region 402 is determined using EDS. Figure 4B It is shown Figure 4A EDS image of the location of ZnI2. Figure 4B The dark areas in the graph indicate the absence of ZnI2, while the light areas indicate the presence of ZnI2. Figure 4A The amount of iodine in the equivalent area of ​​the matrix phase identified as area 401 in FIG. The amount of iodine collected in each phase represents the amount of iodine penetration in a given phase. Table 4 shows analytical data from two different carrier D embodiments. In Table 4, the amount of iodine in the dispersed phase is 0.43 atomic %, while the amount of iodide in the matrix phase is 14.68 atomic %. The amount of iodine present in the dispersed phase is much lower than the amount of iodine in the matrix phase and is believed to be related to the amount of catalytically active metals such as silver that will be deposited on the same alumina particles when the ceramic article of the present invention is made for use as a catalyst support.

[0092] Table 4

[0093]

[0094] In Table 4, percentages refer to atomic weight percentages.

[0095] The fused alumina particles are not infiltrated by ZnI 2. SEM images show significantly larger and impermeable particles distributed throughout the continuous matrix, as shown in Figure 5A See particles 502, 504 and 506. Figure 5B It is shown Figure 5A EDS image of the location of ZnI2. Figure 5B The dark areas in the graph indicate the absence of ZnI2, while the light areas indicate the presence of ZnI2. The ZnI2 dye penetration test demonstrated the ability to create an impermeable phase distributed in a matrix phase.

[0096] Implementation

[0097] Embodiment 1. A ceramic product comprising:

[0098] (a) a rigid formation of aluminum oxide particles, the rigid formation comprising a first plurality of aluminum oxide particles and a second plurality of aluminum oxide particles, wherein the two plurality of particles are randomly distributed throughout the rigid formation

[0099] 1) wherein the second aluminum oxide particles have a ZnI2 dye penetration test value of no greater than 5 atomic %, and wherein the ZnI2 dye penetration test value of the first aluminum oxide particles is at least twice the ZnI2 dye penetration test value of the second aluminum oxide particles;

[0100] 2) wherein the rigid formation has a total cross-sectional area, and each of the plurality of particles occupies a portion of the total cross-sectional area, and the cross-sectional area of ​​the second alumina particles is between 5% and 50% of the total cross-sectional area; and

[0101] (b) a catalytically active metal dispersed on the first alumina particles and the second alumina particles.

[0102] Embodiment 2. An article according to Embodiment 1, wherein the ZnI2 Dye Penetrant Test value of the first aluminum oxide is at least three times the ZnI2 Dye Penetrant Test value of the second aluminum oxide.

[0103] Embodiment 3. An article according to Embodiment 1, wherein the ZnI2 Dye Penetrant Test value of the first aluminum oxide is at least four times the ZnI2 Dye Penetrant Test value of the second aluminum oxide.

[0104] Embodiment 4. An article according to Embodiment 1, wherein the first aluminum oxide has a ZnI2 dye penetration test value greater than 10 atomic %.

[0105] Embodiment 5. An article according to Embodiment 1, wherein the first aluminum oxide has a ZnI2 dye penetration test value greater than 15 atomic %.

[0106] Embodiment 6. The article of embodiment 1, wherein the second aluminum oxide has a Dye Penetration Test value of no greater than 3 atomic %.

[0107] Embodiment 7. The article of Embodiment 1, wherein the ratio of the Dye Penetrant Test value of the first aluminum oxide to the Dye Penetrant Test value of the second aluminum oxide is at least 2:1.

[0108] Embodiment 8. An article according to Embodiment 1, wherein the cross-sectional area of ​​the second aluminum oxide particles is between 8% and 40% of the total cross-sectional area.

[0109] Embodiment 9. An article according to Embodiment 1, wherein the cross-sectional area of ​​the second aluminum oxide particles is between 10% and 30% of the total cross-sectional area.

[0110] Embodiment 10. The article of embodiment 1, further comprising a total pore volume between about 0.2 cm3 / g and about 0.6 cm3 / g.

[0111] Embodiment 11. The article of embodiment 10, wherein the total pore volume is between about 0.3 cm3 / g and about 0.5 cm3 / g.

[0112] Embodiment 12. The article of embodiment 10, wherein the total pore volume is between about 0.35 cm3 / g and about 0.5 cm3 / g.

[0113] Embodiment 13. The article of embodiment 1, wherein the catalytically active metal is selected from the group consisting of silver, platinum, palladium, nickel, and copper.

[0114] Embodiment 14. A method for making a ceramic article comprising a rigid formation of alumina particles and a catalytically active metal in contact with the particles, the method comprising:

[0115] (a) providing a plurality of first alpha alumina particles, the first alpha alumina particles having a known weight and a d50 particle size between about 0.2 microns and 100 microns;

[0116] (b) providing a plurality of second alpha alumina particles, the second alpha alumina particles having a known weight and selected from fused alumina and platy alumina, the second alumina particles having a d50 particle size between about 5 microns and 400 microns, wherein a ratio of the d50 particle size of the first alumina particles to the d50 particle size of the second alumina particles is between 1:4 and 1:40, and wherein a ratio of the weight of the first alumina to the weight of the second alumina is between 1:1 and 15:1;

[0117] (c) mixing the plurality of alumina particles to form a mixture, wherein the particles are randomly distributed throughout the mixture;

[0118] (d) forming the mixture into a plurality of ductile articles;

[0119] (e) heating the ductile articles to a sintering temperature of the alumina particles, thereby forming each ductile article into a rigid formation of alumina particles, wherein the particles in each plurality of particles are randomly distributed throughout the rigid formation; and

[0120] (f) depositing a catalytically active metal on the first alumina particles and the second alumina particles.

[0121] Embodiment 15. The method of Embodiment 14, wherein the ratio of the weight of the first aluminum oxide to the weight of the second aluminum oxide is between 1:1 and 10:1.

[0122] Embodiment 16. The method of Embodiment 14, wherein the ratio of the weight of the first aluminum oxide to the weight of the second aluminum oxide is between 1:1 and 5:1.

[0123] Embodiment 17. The method of Embodiment 14, wherein the ratio of the d50 particle size of the first aluminum oxide particles to the d50 particle size of the second aluminum oxide particles is between 1:5 and 1:20.

[0124] Embodiment 18. The method of Embodiment 14, wherein the ratio of the d50 particle size of the first aluminum oxide particles to the d50 particle size of the second aluminum oxide particles is between 1:8 and 1:15.

[0125] Embodiment 19. The method of Embodiment 14, wherein the second alumina particles have a d50 particle size between 10 microns and 200 microns.

[0126] Embodiment 20. The method of Embodiment 14, wherein the second alumina particles have a d50 particle size between 40 microns and 150 microns.

[0127] Embodiment 21. The method of Embodiment 14, wherein the plurality of first alumina particles have a surface area between 1.0 m2 / g and 20.0 m2 / g.

[0128] Embodiment 22. The method of Embodiment 14, wherein the plurality of first alumina particles have a surface area between 1.0 m2 / g and 5.0 m2 / g.

[0129] Embodiment 23. The method of Embodiment 14, wherein the plurality of first alumina particles have a surface area between 1.0 m2 / g and 2.0 m2 / g.

[0130] Embodiment 24. The method of Embodiment 14, wherein the plurality of second alumina particles have a surface area between 0.01 m2 / g and 2.00 m2 / g.

[0131] Embodiment 25. The method of Embodiment 14, wherein the plurality of second alumina particles have a surface area between 0.10 m2 / g and 0.50 m2 / g.

[0132] Embodiment 26. The method of Embodiment 14, wherein the plurality of second alumina particles have a surface area between 0.14 m2 / g and 0.30 m2 / g.

[0133] Embodiment 27. The method of Embodiment 14, wherein the second alumina particles consist essentially of fused alumina.

[0134] Embodiment 28. The method of Embodiment 14, wherein the second alumina particles are composed of fused alumina.

[0135] Embodiment 29. The method of Embodiment 14, wherein the second alumina particles consist essentially of platy alumina.

[0136] Embodiment 30. The method of Embodiment 14, wherein the second alumina particles consist of platy alumina.

[0137] Embodiment 31. A method according to Embodiment 14, wherein the second alumina particles consist essentially of platy alumina and fused alumina.

[0138] Embodiment 32. A method according to Embodiment 14, wherein the second alumina particles are composed of platy alumina and fused alumina.

[0139] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs. All patents and publications mentioned herein are incorporated by reference in their entirety.

[0140] When ranges are used herein to describe, for example, physical or chemical properties such as molecular weight or chemical formula, all combinations and subcombinations of ranges and specific embodiments thereof are intended to be included. When referring to a number or a numerical range, the use of the term "about" means that the number or numerical range referred to is an approximation within the experimental variability (or within the statistical experimental error), so the number or numerical range can vary. The variation is typically 0% to 5% of the number or numerical range.

[0141] When used in the appended claims in their original and amended forms, the transitional terms "comprising," "consisting essentially of," and "consisting of" define the scope of the claims with respect to excluding unrecited appended claim elements or steps, if any, from the scope of the claim. The term "comprising" is intended to be inclusive or open-ended, and does not exclude any additional, unrecited elements, methods, steps, or materials. The term "consisting of" excludes any elements, steps, or materials other than those specified in the claim, and in the latter case, excludes impurities normally associated with the specified materials. The term "consisting essentially of" limits the scope of the claim to the specified elements, steps, or materials and those elements, steps, or materials that do not materially affect the basic and novel characteristics of the claimed invention. In alternative embodiments, all compounds, compositions, formulations, and methods described herein that embody the present invention may be more specifically defined by any of the transitional terms "comprising," "consisting essentially of," and "consisting of." The term "comprising" (and related terms such as "including" or "containing" or "having") includes those embodiments, such as, for example, embodiments of any composition of matter, method, or process that "consists of" or "consists essentially of the described features."

Claims

1. A ceramic product comprising: (a) a rigid formation of aluminum oxide particles, the rigid formation comprising a first plurality of aluminum oxide particles and a second plurality of aluminum oxide particles, wherein the two plurality of particles are randomly distributed throughout the rigid formation 1) wherein the second aluminum oxide particles have a ZnI2 dye penetration test value of no greater than 5 atomic %, and wherein the ZnI2 dye penetration test value of the first aluminum oxide particles is at least twice the ZnI2 dye penetration test value of the second aluminum oxide particles; 2) wherein the rigid formation has a total cross-sectional area, and each of the plurality of particles occupies a portion of the total cross-sectional area, and the cross-sectional area of ​​the second alumina particles is between 5% and 50% of the total cross-sectional area; and (b) a catalytically active metal dispersed on the first alumina particles and the second alumina particles.

2. The article of claim 1, wherein the first aluminum oxide has a ZnI2 dye penetrant test value that is at least three times greater than the second aluminum oxide's ZnI2 dye penetrant test value.

3. The article of claim 1, wherein the first aluminum oxide has a ZnI2 Dye Penetrant Test value that is at least four times greater than the second aluminum oxide's ZnI2 Dye Penetrant Test value.

4. The article of claim 1, wherein the first aluminum oxide has a ZnI2 dye penetration test value greater than 10 atomic %.

5. The article of claim 1, wherein the first aluminum oxide has a ZnI2 dye penetration test value greater than 15 atomic %.

6. The article of claim 1, wherein the second aluminum oxide has a Dye Penetration Test value of no greater than 3 atomic %.

7. The article of claim 1, wherein the cross-sectional area of ​​the second aluminum oxide particles is between 8% and 40% of the total cross-sectional area.

8. The article of claim 1, wherein the cross-sectional area of ​​the second aluminum oxide particles is between 10% and 30% of the total cross-sectional area.

9. The article according to claim 1, further comprising: 3 / g and 0.6cm 3 / g total pore volume between.

10. The article of claim 9, wherein the total pore volume is within 0.3 cm 3 / g and 0.5cm 3 / g.

11. The article of claim 9, wherein the total pore volume is within 0.35 cm 3 / g and 0.5cm 3 / g.

12. The article of claim 1 wherein the catalytically active metal is selected from the group consisting of silver, platinum, palladium, nickel, and copper.