Catalysts and acetylation methods

By using metal-doped supported oxide catalysts modified with nitrogen-containing heterocyclic compounds, the problems of numerous side reactions and difficulty in catalyst recovery in alkynol synthesis have been solved, achieving efficient and environmentally friendly alkynol production and reducing production costs.

CN116651451BActive Publication Date: 2026-11-17SHANDONG NHU PHARMA +1
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202310595396.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2026-11-17
Estimated Expiration
2043-05-23

AI Technical Summary

Technical Problem

Existing methods for synthesizing alkynols suffer from numerous side reactions, low yields, difficulty in catalyst recovery, and high energy consumption, resulting in high production costs and significant environmental pressure.

Method used

Metal-doped supported oxide catalysts modified with nitrogen-containing heterocyclic compounds are used to suppress side reactions, improve reaction selectivity and yield, and enable catalyst recycling by providing steric hindrance and electronic effects on the catalyst surface through modifiers.

Benefits of technology

It improves the yield of alkynols and the utilization rate of raw materials, simplifies post-processing operations, reduces the generation of wastewater and waste salt, and lowers production costs, thus having environmental and economic advantages.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116651451B_ABST
    Figure CN116651451B_ABST
Patent Text Reader

Abstract

This invention relates to a catalyst for acetylation reactions and a method for acetylation. The catalyst includes a modifier and a metal oxide system, wherein the metal oxide system is a support oxide doped with a first metal element, and the modifier is present in at least a portion of the surface region of the metal oxide system. The acetylation method includes the step of reacting a carbonyl-containing compound with a terminal acetylation compound in the presence of the catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of fine chemicals. Specifically, this invention relates to a catalyst for acetylation reactions of carbonyl compounds, and further provides a method for acetylation of carbonyl compounds using the catalyst. Background Technology

[0002] Alkynes are an important class of fine chemical products, mainly used in the production of vitamin E intermediates, DV chrysanthemic acid (chrysanthemum ester intermediate), vitamin A, vitamin K1, carotenoid intermediates, synthetic rubber monomers, linalool and other fragrances.

[0003] Several methods have been provided for the preparation of alkynols. For example, references 1 and 2 describe the preparation of Grignard reagents containing an alkynyl group, which are then reacted with carbonyl compounds to obtain alkynols; reference 3 describes the use of an elimination reaction of a halogenated unsaturated alcohol to remove hydrogen halide to obtain alkynols.

[0004] Furthermore, in the industrial production of alkynols, ketones or aldehydes are typically used as raw materials. Acetylene gas is dissolved in liquid ammonia, and under the action of an alkaline catalyst, it reacts with the substrate to synthesize alkynols. The general reaction formula is as follows:

[0005]

[0006] R1 and R2 are hydrogen or hydrocarbon groups.

[0007] Reference 4 discloses the reaction of carbonyl compounds with acetylene in the presence of ammonia and alkali metal hydroxides, with the highest conversion rate of about 95% and the highest selectivity of about 99% in the examples.

[0008] Reference 5 discloses a method using ketones and acetylene as raw materials and potassium isobutoxide as a catalyst. The raw materials, ketones, acetylene, and potassium isobutoxide are continuously fed into the reactor. This patent uses only potassium isobutoxide as a catalyst and does not require the use of ammonia. However, the catalyst is expensive and difficult to recover.

[0009] Reference 6 discloses a method using ketones and acetylene as raw materials, flake potassium hydroxide as a catalyst, ether and water as solvents, and the addition of a nonionic surfactant. Water is first removed under azeotropic conditions, KOH is suspended in the organic phase, and after cooling to below 20°C, the ketone and acetylene are introduced to react under normal pressure. However, this method suffers from the low solubility of acetylene, which limits the reaction rate, and product separation is also challenging.

[0010] Reference 7 discloses a novel process for synthesizing alkynols from acetylene and ketones. In this process, acetylene is mixed with ammonia solvent and compressed, followed by the addition of ketones and potassium hydroxide catalyst. The alkynylation reaction is completed in a reactor, and ammonium chloride is added to terminate the reaction. The product is then subjected to pressurized degassing, atmospheric degassing, scraped evaporation, and ketone removal to obtain crude alkynols. Finally, membrane separation is used to remove water, yielding anhydrous alkynols. However, this method uses the strong base potassium hydroxide as a catalyst, which leads to various side reactions during the main reaction; furthermore, the addition of ammonium chloride to terminate the reaction results in the generation of waste salts.

[0011] Reference 8 discloses an acetylation method using N,N-dimethylformamide as a solvent and inorganic cyanides such as sodium cyanide and potassium cyanide as side reaction inhibitors. In the presence of a catalyst alkoxide or amino salt, saturated or unsaturated ketones or aldehydes undergo acetylation to yield the corresponding alkynols. However, this method requires multiple extractions, necessitating 30-200% of the solvent mass of water. The operation is cumbersome, generates significant amounts of wastewater, and the use of highly toxic cyanides poses safety risks to operators.

[0012] Despite the fact that, as mentioned above, existing technologies have explored various synthetic methods for alkynols to some extent, there is still room for further improvement.

[0013] References:

[0014] Reference 1: CN112375091A

[0015] Reference 2: CN104744211A

[0016] Reference 3: CN107032956A

[0017] Reference 4: CN1675152A

[0018] Reference 5: CN1769254A

[0019] Reference 6: CN102476978A

[0020] Reference 7: CN106117010A

[0021] Reference 8: CN110467519B Summary of the Invention

[0022] The problem the invention aims to solve

[0023] As mentioned earlier, the current large-scale industrial production of alkynols typically involves the alkynylation of aldehydes or ketones under alkaline conditions using a catalyst. This reaction is essentially a nucleophilic addition: the terminal CH bond of the alkyne breaks under alkaline catalysis to form an alkynyl carbanion, which acts as a nucleophile to attack the positively charged carbon atom in the carbonyl group (the carbonyl group is a polar functional group; the oxygen atom in the carbonyl group is more electronegative than the carbon atom, hence the oxygen carries a negative charge and the carbon carries a positive charge). However, under alkaline conditions, in addition to the main reaction described above, several side reactions also occur simultaneously, such as the further reaction of alkynols to form alkynyldiols and the thermal decomposition of alkynols. Furthermore, the aldol condensation reaction of the aldehydes or ketones themselves under alkaline conditions easily generates byproducts, and the occurrence of these side reactions all lead to low reaction yields.

[0024] Furthermore, in current industrial practices, the alkaline catalysts used in large quantities are almost impossible to recover and reuse, leading not only to high production costs but also to environmental problems. In addition, using ammonia as a solvent requires liquefaction at very low temperatures, resulting in substantial refrigeration energy consumption, which has become a significant burden on energy resources.

[0025] Therefore, in view of the aforementioned problems in the industrial production of alkynols in this field, the present invention primarily provides a reaction catalyst suitable for the preparation of alkynols from carbonyl-containing compounds and alkynyl-containing compounds. This catalyst is obtained by modifying a metal-doped support oxide with a nitrogen-containing heterocyclic compound. Furthermore, the catalyst of the present invention can suppress the occurrence of side reactions and imparts recyclability to the catalyst.

[0026] Furthermore, the present invention also provides a method for preparing acetylinol using the above-mentioned catalyst. This method not only has an improved yield, but also reduces or even eliminates the use of solvents. Therefore, it is a highly efficient and environmentally friendly acetylation method, which is beneficial to the large-scale industrial production of acetylinol and its downstream products.

[0027] Solution for solving the problem

[0028] Through long-term research, the inventors of this invention have discovered that the above-mentioned technical problems can be solved by implementing the following technical solution:

[0029] [1]. This invention first provides a catalyst for the preparation of alkynols via the reaction of a carbonyl-containing compound with a terminal alkynyl-containing compound, wherein,

[0030] The catalyst comprises a modifier and a metal oxide system, wherein the metal oxide system is a carrier oxide doped with a first metal element.

[0031] in,

[0032] The modifier includes nitrogen-containing heterocyclic compounds.

[0033] The first metallic element includes one or more of Pd, Ru, Pt, Nb, Bi, Cu, and Co, preferably a combination of two or more elements.

[0034] Furthermore, the modifier is present in at least a portion of the surface region of the metal oxide system.

[0035] [2]. According to the catalyst described in [1], wherein the carbonyl-containing compound has the molecular formula represented by the following formula (I):

[0036]

[0037] R1 and R2 may appear the same or different each time, and may be hydrogen or monovalent organic groups independently, or R1 and R2 may be linked to form a ring, provided that R1 and R2 are not both hydrogen at the same time.

[0038] [3]. The catalyst according to [1] or [2], wherein the terminal alkyne compound has the molecular formula of formula (II) below.

[0039]

[0040] R3 is hydrogen or a monovalent organic group.

[0041] [4]. The catalyst according to any one of [1] to [3], wherein the nitrogen-containing heterocyclic compound is selected from one or more of pyridine, imidazole, pyrazole, quinoline, and oxazoline compounds.

[0042] [5]. The catalyst according to any one of [1] to [4], wherein in the metal oxide system, the content of the first metal element is 0.1 to 10% of the mass of the doped support oxide.

[0043] [6]. The catalyst according to any one of [1] to [5], wherein the molar ratio of the nitrogen-containing heterocyclic compound to the first metal element in the catalyst is 10 to 20:1.

[0044] [7]. Furthermore, the present invention also provides a method for preparing alkynols, wherein the method comprises:

[0045] The step of reacting a carbonyl compound with a terminal alkyne compound in the presence of a catalyst according to any one of [1] to [6] above.

[0046] [8]. The method according to [7], wherein the reaction is carried out with or without a solvent.

[0047] [9]. The method according to [7] or [8], wherein the temperature of the reaction is below 70°C and the reaction time is below 6 hours.

[0048]

[10] . The method according to any one of [7] to [9], wherein the catalyst is a newly prepared catalyst or a reused catalyst.

[0049] The effects of the invention

[0050] In this invention, through the implementation of the above technical solution, it has been found that the present invention can achieve the following technical effects:

[0051] (1) The acetylation method and catalyst for carbonyl compounds provided by the present invention not only inhibit the further formation of acetylinyl diol from acetylinyl alcohol, but also eliminate the thermal decomposition of acetylinyl alcohol products and the self-condensation reaction of substrate aldehydes or ketones, effectively improving product yield and raw material utilization.

[0052] (2) The acetylation method provided by the present invention has a simple reaction system and can be carried out successfully even without the use of solvent. Therefore, after the reaction, there is no need for extraction to extract the product, nor is there a need to add salt to quench the reaction. Moreover, the catalyst is easy to recover, and no wastewater or waste salt is generated. It is green and environmentally friendly, and greatly simplifies the post-processing operation.

[0053] (3) The heterogeneous metal-doped catalyst used in this invention is easy to recover and has stable performance, realizing the recycling of the catalyst, effectively reducing production costs, and helping to enhance the competitiveness of alkynols and their downstream products. Attached Figure Description

[0054] Figure 1 Here is a SEM image of the catalyst morphology in Example 17;

[0055] Figure 2 Here are the liquid-gas phase detection spectra and results for the acetylene reaction in Example 24;

[0056] Figure 3 The following is a gas-phase detection spectrum and results of the acetylene reaction in Example 43. Detailed Implementation

[0057] The present invention will now be described in detail. The descriptions of the technical features described below are based on representative embodiments and specific examples of the present invention, but the present invention is not limited to these embodiments and specific examples. It should be noted that:

[0058] In this specification, the range of values ​​referred to as "value A to value B" refers to the range including the endpoint values ​​A and B.

[0059] In this specification, the numerical range indicated by "above" or "below" refers to the numerical range that includes the stated number.

[0060] In this specification, the word "may" has two meanings: to perform a certain process and not to perform a certain process.

[0061] In this specification, the terms "optional" or "optional" are used to indicate the use or non-use of certain substances, components, procedures, application conditions, etc., and there are no restrictions on the manner of use.

[0062] In this specification, the term "unsaturated structure" refers to a structure formed by carbon-carbon double bonds, unless otherwise specified.

[0063] In this specification, the term "hydrocarbon group" is used to refer to an organic structure formed by carbon and hydrogen elements, and it can be an aromatic or non-aromatic group.

[0064] In this specification, the term "halogen" refers to fluorine, chlorine, bromine, or iodine. Fluorine, chlorine, or bromine are preferred, and bromine and chlorine are more preferred.

[0065] All unit names used in this manual are international standard unit names, and unless otherwise stated, the "%" used refers to weight or mass percentage content.

[0066] In this specification, references to "some specific / preferred embodiments," "other specific / preferred embodiments," "implementation," etc., refer to specific elements (e.g., features, structures, properties, and / or characteristics) related to that embodiment, which are included in at least one of the embodiments described herein and may or may not be present in other embodiments. Furthermore, it should be understood that these elements may be combined in any suitable manner in various embodiments.

[0067] The present invention mainly provides a catalyst suitable for the acetylation reaction of carbonyl compounds to prepare alkynols. At the same time, the present invention also provides a synthetic method for preparing alkynols using the catalyst.

[0068] Furthermore, this invention is primarily based on the following insights:

[0069] The catalyst of the present invention comprises: a metal oxide system obtained by doping with a first metal element and a modifier present in at least a portion of the surface of the metal oxide system.

[0070] It has been found that the basicity of the support oxide is significantly enhanced after first metal doping, which promotes the breaking of the CH bond in alkynes to form carbanions. These carbanions act as nucleophiles to attack substrates containing carbonyl groups (such as aldehydes or ketones), significantly improving the reaction rate and conversion. The substrate (aldehyde or ketone) is adsorbed on the active site on the catalyst surface, and the alkynol product is rapidly desorbed after the reaction, improving the selectivity of the reaction.

[0071] Furthermore, the modifiers on the catalyst also play a role in modifying the catalyst. Although the mechanism of the modified catalyst is not yet fully understood, it is speculated that the modifiers, which are bonded to the surface of the metal oxide system, although having significant steric hindrance, do not affect the catalytic basicity of the catalyst due to their electronic nature. Simultaneously, they prevent the alkynols, as products, from continuing to adsorb on the catalyst surface for nucleophilic addition reactions, thus avoiding the formation of alkynyl diol byproducts and improving the reaction yield. The nitrogen atom in the nitrogen heterocycle has electron-donating properties and can chelate with metals to form stable metal complexes; in addition, nitrogen atoms readily undergo electron transfer, enabling the recycling of the catalyst.

[0072] <First Aspect>

[0073] In a first aspect of the present invention, a catalyst suitable for acetylation reactions of carbonyl compounds and terminal alkynyl compounds is provided.

[0074] The catalyst of the present invention is a heterogeneous catalyst for the acetylation reaction, comprising a metal oxide system and a modifier present in at least a portion of the surface of the metal oxide system.

[0075] (Carbonyl-containing compounds)

[0076] For the carbonyl-containing compounds of the present invention, there are in principle no particular limitations on such carbonyl-containing compounds as long as they are useful for the preparation of alkynols.

[0077] In some specific embodiments of the present invention, the carbonyl-containing compounds of the present invention may have one or more carbonyl groups. Such carbonyl groups may exist in the form of aldehyde or ketone groups. In the case of containing one carbonyl group, the corresponding alkynol can be obtained by reaction with an alkynyl group; in the case of having multiple carbonyl groups, the corresponding compound having multiple alkynol groups can also be obtained. Alternatively, depending on actual needs, some carbonyl groups that do not need to undergo alkynylation can be protected, so that alkynylation can only occur at specific sites. Furthermore, the method of protection is not particularly limited and can be carried out by conventional methods known in the art.

[0078] In some specific embodiments of the present invention, the carbonyl-containing compound has the structure or molecular formula shown in formula (I):

[0079]

[0080] R1 and R2 may appear the same or different each time, and may be hydrogen or monovalent organic groups independently, or R1 and R2 may be linked to form a ring, provided that R1 and R2 are not both hydrogen at the same time.

[0081] There are no particular restrictions on the monovalent organic group as long as it does not affect the acetylation reaction. In some specific embodiments, the monovalent organic group can be selected from hydrocarbon groups with 1 to 50 carbon atoms, preferably 1 to 40, and more preferably 2 to 30 or 3 to 20.

[0082] These monovalent groups can be saturated hydrocarbon groups or hydrocarbon groups having one or more unsaturated structures. In other specific embodiments, these hydrocarbon group structures can have any straight-chain, branched, or cyclic structure, and these straight-chain, branched, or cyclic structures can also have one or more saturated structures (e.g., aromatic structures). In some preferred embodiments, they can be straight-chain, branched, or (partially) cyclic groups formed of 1 to 15 or 2 to 10 carbon atoms, and have one or two unsaturated structures.

[0083] Furthermore, as a monovalent group, the aforementioned hydrocarbon group may further have optional substituents, which are not limited to those selected from halogen groups, nitrogen-containing groups, sulfur-containing groups, oxygen-containing groups (e.g., alkoxy groups), etc. In addition, for the aforementioned hydrocarbon group, each pair of carbon atoms in the hydrocarbon chain may be separated by silicon, oxygen, sulfur atoms, or a group centered thereon.

[0084] Furthermore, in some preferred embodiments of the present invention, the compound of formula (I) may be selected from any one of the group consisting of formaldehyde, acetone, butanone, 6-methyl-5-hepten-2-one, 6-methyl-5-octen-2-one, 6-methyl-2-heptenone, geranylacetone, tetrahydrogeranylacetone, phytoketones and furfural.

[0085]

[0086] Furthermore, through the acetylation reaction described below in this invention, the corresponding structures formed (taking acetylene as an example) are: propargyl alcohol, 2-methyl-3-butyn-2-ol, 3-methyl-pentyn-3-ol, dehydrolinalool, dehydroethyllinalool, dihydrodehydrolinalool, furfuryl acetylenol, dehydronerol, tetrahydrodehydronerol, and dehydroisophytol, with the following structural formulas:

[0087]

[0088] (Contains terminal alkyne compounds)

[0089] The terminal alkyne compounds of this invention are primarily used to provide nucleophilic attacking groups for acetylation reactions. Therefore, this invention is not particularly limited to any compound capable of acetylation reactions.

[0090] In some specific embodiments, the terminal alkyne-containing compound has the molecular formula of formula (II).

[0091]

[0092] R3 is either hydrogen or a monovalent organic group. In principle, the monovalent organic group can have the same selection range as those described above. Considering the economics of synthesis and the downstream applicability of the alkynol product, R3 is preferably a hydrogen atom or an alkyl group with 1 to 5 carbon atoms; more preferably, R3 is a hydrogen atom.

[0093] For the terminal alkyne compounds of the present invention, the purity in the acetylation reaction described below is preferably 99% or higher to reduce the occurrence of side reactions.

[0094] (Metal oxide system)

[0095] The metal oxide system of this invention is mainly used to provide catalytic basicity to enhance the nucleophilic reactivity of compounds containing terminal alkyne groups.

[0096] Specifically, the metal oxide system of the present invention can be obtained by doping a carrier oxide with a first metal element.

[0097] In some specific embodiments of the present invention, the first metallic element may include one or more of Pd, Ru, Pt, Nb, Bi, Cu, and Co. Preferably, from the perspective of improving substrate conversion and selectivity, the first metallic element includes a combination of two or more of the above elements.

[0098] There are no particular limitations on the support oxide, provided it provides sufficient basicity and reaction sites. In some specific embodiments, the support oxide may be an oxide of a metal (hereinafter referred to as the "second metal"). This second metal may contain one or a mixture of transition metals, main group metals, or both. In some specific embodiments of the invention, the second metal may include the same metal element as the first metal element, or the second metal may not include the same metal element as the first metal element. Furthermore, when the second metal includes the same metal element as the first metal element, the surface concentration of this same metal element in the metal oxide system is higher than its internal concentration.

[0099] Furthermore, considering the efficiency, selectivity, and yield of the acetylation reaction, the support oxides available for use in this invention can be selected from one or more of CeO2, BaCeO3, CaFeO3, LaCoO3, LaNiO3, LaFeO3, and γ-Al2O3, or a mixture thereof.

[0100] The morphology of the carrier oxide can be granular with a porous surface, and such carrier oxides can be obtained by self-production or commercial purchase.

[0101] Furthermore, for a carrier oxide doped with a first metal element, it means that at least a portion of the first metal element has entered the crystal structure of the carrier oxide.

[0102] (Modifier)

[0103] The main function of the modifier of this invention is to provide surface modification for metal oxide systems without affecting catalytic alkalinity, so as to provide an effective steric hindrance effect.

[0104] The modifiers of the present invention may include nitrogen-containing heterocyclic compounds, wherein the nitrogen atoms provide effective electronic effects, and the cyclic structure provides effective steric hindrance effects.

[0105] For the nitrogen-containing heterocyclic compounds described in this invention, there are no particular limitations as long as a nitrogen atom exists in a saturated or unsaturated ring structure. Preferably, these nitrogen-containing heterocyclic compounds can be selected from one or more of pyridine, imidazole, pyrazole, quinoline, and oxazoline compounds.

[0106] Furthermore, the nitrogen-containing ligand is preferably selected from one or more nitrogen-containing heterocyclic compounds of the following L1 to L10:

[0107]

[0108] For compounds with the above structure, other substituents may be present on the cyclic structure without limitation. Preferably, these substituents may be alkyl, cycloalkyl, aryl, etc., with a carbon number of 1 to 30 or 2 to 20.

[0109] Furthermore, there is no particular limitation on the way the modifier is combined with the metal oxide system. The modifier can be applied to at least a portion of the surface area of ​​the metal oxide system by means of impregnation or coating.

[0110] (catalyst)

[0111] As described above, the catalyst of the present invention comprises the aforementioned metal oxide system and a modifier present in at least a portion of the surface of the metal oxide system.

[0112] For the metal oxide system obtained by doping with a first metal element, the content of the first metal element can be 0.1 to 10% of the mass of the doped carrier oxide, preferably 0.5 to 9% by mass, more preferably 1 to 8% by mass, for example 1.5% by mass, 2% by mass, 2.5% by mass, 3% by mass, 3.5% by mass, 4% by mass, 4.5% by mass, 5% by mass, 5.5% by mass, 6% by mass, 6.5% by mass, 7% by mass, 7.5% by mass, etc.

[0113] Furthermore, regarding the amount of modifier used, in the catalyst, the molar ratio of the nitrogen-containing heterocyclic compound to the first metal element is 10-20:1, preferably 12-18:1, and more preferably 13-16:1.

[0114] <Second aspect>

[0115] In a second aspect of the present invention, a method for preparing the catalyst of the first aspect described above is provided, the method mainly comprising:

[0116] i. The first step of doping with a metallic element;

[0117] ii. Steps for loading modifiers.

[0118] (Step i)

[0119] The doping of the first metal element into the aforementioned carrier oxide is mainly achieved by inserting at least a portion of the first metal into the crystal structure of the carrier oxide to improve the overall alkalinity.

[0120] In some specific embodiments of the present invention, step i can be performed by calcining the first metal source and the carrier oxide.

[0121] The first metal source can be various acid salts or hydrates of the first metal, such as one or more of nitrates, hydrochlorides, sulfates, acetates, citrates, formates, ammonium salts, and their hydrates. Preferably, for ease of operation, these first metal sources are water-soluble metal salts.

[0122] In some specific implementations, the first metal source, the carrier oxide, and the solvent (water or organic solvent, etc.) can be mixed to form a mixed system. Preferably, they can be mixed at 100-160°C for 2-6 hours, so that the first metal source is adsorbed on the surface of the carrier oxide, and then removed and calcined.

[0123] There are no particular restrictions on the calcination conditions in principle. For example, calcination can be carried out under atmospheric conditions at 400–600°C to obtain a catalyst precursor doped with the first metallic element.

[0124] (Step ii)

[0125] There are no particular restrictions in principle regarding the loading method of the modifier. For example, in some specific embodiments, the catalyst precursor can be impregnated with a solution containing a dissolved or dispersed modifier, or coated (e.g., sprayed) onto the surface of the catalyst precursor with a solution containing a dissolved or dispersed modifier to obtain the catalyst of the present invention. In some preferred embodiments, the catalyst precursor can be impregnated in a solution containing a dispersed or dissolved modifier, preferably by mixing at 100–160°C for 2–6 hours.

[0126] (Other auxiliary methods)

[0127] There are no particular limitations on other auxiliary preparation methods besides the two steps mentioned above. For example, methods such as washing, stirring, and drying can be carried out appropriately with reference to various known methods in the art. Furthermore, there are no particular limitations on the organic solvents that may be used in the above steps, including alcohol solvents, aromatic solvents, etc.

[0128] <Third aspect>

[0129] In a third aspect of the invention, there is a method for carrying out an acetylation reaction using the catalyst of the first aspect of the invention.

[0130] Specifically, the acetylation reaction method of the present invention includes the step of reacting a carbonyl-containing compound with a terminal acetylation-containing compound in the presence of a catalyst.

[0131] In some specific embodiments, the acetylation reaction of the present invention is carried out with or without a solvent. Therefore, it is more economical and environmentally friendly compared to conventional industrial processes that use liquid ammonia as a necessary solvent.

[0132] Furthermore, for acetylation reactions, the solvents permitted in this invention are not particularly limited in principle as long as they are reaction inert. In some specific embodiments, these solvents may include alcohol solvents, aromatic solvents (e.g., toluene, xylene), ether solvents, etc.

[0133] Furthermore, the temperature of the acetylation reaction is typically below 70°C, preferably 30–60°C, more preferably 40–55°C, and the reaction time is below 6 hours, for example 2–4 hours.

[0134] In some preferred embodiments, the mass concentration of the catalyst in the reaction system is controlled to be below 9%, preferably 2-7%.

[0135] In addition, considering that some compounds containing terminal alkyne groups are in a gaseous state, the reaction can be carried out under pressure. For example, the acetylation reaction can be carried out under conditions of 0.15 to 0.25 MPa.

[0136] In this invention, the acetylation reaction does not require the use of catalytic inhibitors such as ammonium chloride to terminate the reaction, and the final product can be directly separated after the acetylation reaction is completed without the use of a solvent. At this time, a solid catalyst can also be obtained simultaneously with the separation of the final product.

[0137] Therefore, for the acetylation reaction of the present invention, the catalyst used can be a fresh catalyst (unused) prepared by the preparation method of the second aspect of the present invention, or a regenerated catalyst recovered from the completed acetylation reaction.

[0138] Regarding the catalyst recovery method, some specific implementation schemes may include:

[0139] When the conversion rate of the reactants (containing carbonyl compounds) is detected to be lower than a specified standard, such as 90% or 80%, it is defined as catalyst deactivation. After catalyst deactivation, it is removed from the reaction system, cleaned, and then placed in a vacuum drying oven at a temperature above 100°C for 4–6 hours to restore its activity.

[0140] Furthermore, for the acetylation reaction of the present invention, when the catalyst described above is used, the reaction conversion rate for carbonyl compounds is preferably 88% or more, preferably 90% or more, more preferably 95% or more, and the selectivity is 85% or more, preferably 90% or more, more preferably 92% or more.

[0141] Example

[0142] The embodiments of the present invention will be described in detail below with reference to the examples. Unless otherwise specified in the examples, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all commercially available conventional products.

[0143] Example 1

[0144] Add 1.25 g of Pd(NO3)2·2H2 and 1.62 g of Bi(NO3)2·5H2O to 30 mL of deionized water, stir at 400 r / min until completely dissolved, then add 10.0 g of BaCeO3 support, heat to 100 °C, continue stirring for 4 hours, remove water by rotary evaporation under reduced pressure, obtain a solid and place it in a vacuum drying oven at 100 °C to dry to constant weight; remove and place in a muffle furnace, calcine at 500 °C for 6 hours, cool and remove to obtain the precursor. 11.74 g of ligand 4,4'-bipyridine (L1, MW: 156.18) was dispersed in 30 mL of deionized water. After thorough mixing, the precursor was added, the temperature was raised to 120 °C, and the mixture was stirred at 400 r / min for 4 hours. The water was removed by rotary evaporation under reduced pressure to obtain a solid. The solid was placed in a vacuum drying oven at 100 °C and dried to constant weight to obtain catalyst 5.0% Pd-7.0% Bi / BaCeO3-L1.

[0145] Example 2

[0146] Add 1.25 g of Pd(NO3)2·2H2O and 1.16 g of Bi(NO3)2·5H2O to 30 mL of deionized water, stir at 400 r / min until completely dissolved, then add 10.0 g of BaCeO3 support, heat to 80 °C, continue stirring for 6 hours, remove water by rotary evaporation under reduced pressure, obtain a solid and place it in a vacuum drying oven at 100 °C to dry to constant weight; remove and place in a muffle furnace, calcine at 500 °C for 6 hours, cool and remove to obtain the precursor. 19.03 g of ligand L10 (MW: 253.11) was dispersed in 50 mL of deionized water and thoroughly mixed. The precursor was then added, and the mixture was heated to 120 °C and stirred at 400 r / min for 4 hours. The water was removed by rotary evaporation under reduced pressure to obtain a solid. The solid was then placed in a vacuum drying oven at 100 °C and dried to constant weight to obtain catalyst 5.0% Pd-5.0% Bi / BaCeO3-L10.

[0147] Example 3

[0148] Add 0.75 g of Pd(NO3)2·2H2O and 1.62 g of Bi(NO3)2·5H2O to 30 mL of deionized water. Stir at 400 r / min until completely dissolved. Then add 10.0 g of BaCeO3 support, heat to 100 °C, and continue stirring for 4 hours. Remove moisture by rotary evaporation under reduced pressure to obtain a solid, which is then dried to constant weight in a vacuum drying oven at 100 °C. After drying, place the solid in a muffle furnace and calcine at 600 °C for 4 hours. After cooling, remove the solid to obtain the precursor. Disperse 11.42 g of ligand L10 in 30 mL of deionized water and mix thoroughly. Add the precursor, heat to 120 °C, and stir at 400 r / min for 4 hours. Remove moisture by rotary evaporation under reduced pressure to obtain a solid, which is then dried to constant weight in a vacuum drying oven at 100 °C to obtain the catalyst 3.0%Pd-7.0%Bi / BaCeO3-L10.

[0149] Example 4

[0150] Add 1.17 g of PdCl2 to 30 mL of deionized water and stir at 400 rpm until completely dissolved. Then add 1.43 g of Nb2O5 and 10.0 g of CaFeO3 support. Heat to 100 °C and continue stirring for 4 hours. Remove moisture by rotary evaporation under reduced pressure to obtain a solid, which is then dried to constant weight in a vacuum drying oven at 100 °C. After drying, place the solid in a muffle furnace and calcine at 500 °C for 6 hours. After cooling, remove the solid to obtain the precursor. Disperse 20.55 g of ligand 2,2'-bipyridine (L2, MW: 156.18) in 50 mL of deionized water and mix thoroughly. Add the precursor, heat to 120 °C, and stir at 400 rpm for 4 hours. Remove moisture by rotary evaporation under reduced pressure to obtain a solid, which is then dried to constant weight in a vacuum drying oven at 100 °C to obtain the catalyst 7.0% Pd-5.0% Nb / CaFeO3-L2.

[0151] Example 5

[0152] Add 1.29 g of RuCl3·3H2O and 3.52 g of Ce(NH4)2(NO3)6 to 30 mL of deionized water, stir at 400 r / min until completely dissolved, then add 10.0 g of LaCoO3 support, heat to 100 °C, continue stirring for 4 hours, remove water by rotary evaporation under reduced pressure, obtain a solid and place it in a vacuum drying oven at 100 °C to dry to constant weight; remove and place in a muffle furnace, calcine at 600 °C for 4 hours, cool and remove to obtain the precursor. 8.38 g of ligand 4-aminopyridine (L3, MW: 94.11) was dispersed in 30 mL of deionized water. After thorough mixing, the precursor was added, the temperature was raised to 120 °C, and the mixture was stirred at 400 r / min for 4 hours. The water was removed by rotary evaporation under reduced pressure to obtain a solid. The solid was placed in a vacuum drying oven at 100 °C and dried to constant weight to obtain catalyst 5.0% Ru-9.0% Ce / LaCoO3-L3.

[0153] Example 6

[0154] Add 1.29 g of RuCl3·3H2O and 1.62 g of Bi(NO3)2·5H2O to 30 mL of deionized water, stir at 400 r / min until completely dissolved, then add 10.0 g of LaFeO3 support, heat to 100 °C, continue stirring for 4 hours, remove water by rotary evaporation under reduced pressure, obtain a solid and place it in a vacuum drying oven at 100 °C to dry to constant weight; remove and place in a muffle furnace, calcine at 600 °C for 5 hours, cool and remove to obtain the precursor. Disperse 8.38 g of ligand 4-aminopyridine (L3, MW: 94.11) in 30 mL of deionized water, stir thoroughly, add the precursor, heat to 120 °C, stir at 400 r / min for 4 hours, remove water by rotary evaporation under reduced pressure, obtain a solid and place it in a vacuum drying oven at 100 °C to dry to constant weight to obtain catalyst 5.0%Ru-7.0%Bi / LaFeO3-L3.

[0155] Example 7

[0156] Add 0.75 g of Pd(NO3)2·2H2O and 1.95 g of Ce(NH4)2(NO3)6 to 50 mL of deionized water, stir at 400 r / min, and after complete dissolution, add 10.0 g of BaCeO3 support, heat to 100 °C, continue stirring for 5 hours, remove water by rotary evaporation under reduced pressure, obtain a solid and place it in a vacuum drying oven at 100 °C to dry to constant weight; remove it and place it in a muffle furnace, calcine at 600 °C for 5 hours, cool and remove to obtain the precursor. 8.81 g of ligand 4,4'-bipyridine (L1) was dispersed in 30 mL of deionized water. After thorough mixing, the precursor was added, the temperature was raised to 120 °C, and the mixture was stirred at 400 r / min for 5 hours. The water was removed by rotary evaporation under reduced pressure to obtain a solid. The solid was placed in a vacuum drying oven at 100 °C and dried to constant weight to obtain catalyst 3.0% Pd-5.0% Ce / BaCeO3-L1.

[0157] Example 8

[0158] Add 0.86 g of PtCl4 and 3.14 g of Cu(OAc)2·H2O to 50 mL of deionized water, stir at 400 r / min until completely dissolved, then add 10.0 g of LaNiO3 support, heat to 100 °C, and continue stirring for 4 hours. Remove moisture by rotary evaporation under reduced pressure to obtain a solid, which is then dried in a vacuum drying oven at 100 °C until constant weight. After drying, place the solid in a muffle furnace and calcine at 600 °C for 4 hours. After cooling, remove the solid to obtain the precursor. Disperse 4.26 g of the ligand 3-aminopyrazole (L4, MW: 83.09) in 30 mL of deionized water, stir thoroughly, add the precursor, heat to 120 °C, and stir at 400 r / min for 4 hours. Remove moisture by rotary evaporation under reduced pressure to obtain a solid, which is then dried in a vacuum drying oven at 100 °C until constant weight to obtain the catalyst 5.0%Pt-10.0%Cu / LaNiO3-L4.

[0159] Example 9

[0160] Add 0.50 g of PdCl2 and 2.96 g of Co(OAc)2·4H2O to 50 mL of deionized water, stir at 400 r / min until completely dissolved, then add 10.0 g of LaFeO3 support, heat to 100 °C, and continue stirring for 4 hours. Remove moisture by rotary evaporation under reduced pressure to obtain a solid, which is then dried in a vacuum drying oven at 100 °C until constant weight. After drying, place the solid in a muffle furnace and calcine at 600 °C for 5 hours. After cooling, remove the solid to obtain the precursor. Disperse 4.17 g of the ligand 4-methylpyrazole (L5, MW: 82.11) in 30 mL of deionized water, stir thoroughly, add the precursor, heat to 120 °C, and stir at 400 r / min for 4 hours. Remove moisture by rotary evaporation under reduced pressure to obtain a solid, which is then dried in a vacuum drying oven at 100 °C until constant weight to obtain the catalyst 3.0%Pd-7.0%Co / LaFeO3-L5.

[0161] Example 10

[0162] Add 0.86 g of PtCl4 and 3.54 g of CuSO4·5H2O to 50 mL of deionized water, stir at 400 r / min until completely dissolved, then add 10.0 g of CeO2 support, heat to 120 °C, and continue stirring for 6 hours. Remove moisture by rotary evaporation under reduced pressure to obtain a solid, which is then dried in a vacuum drying oven at 100 °C until constant weight. After drying, place the solid in a muffle furnace and calcine at 500 °C for 6 hours. After cooling, remove the solid to obtain the precursor. Disperse 4.43 g of the ligand 5-aminoquinoline (L6, MW: 144.17) in 30 mL of deionized water, stir thoroughly, add the precursor, heat to 120 °C, and stir at 400 r / min for 6 hours. Remove moisture by rotary evaporation under reduced pressure to obtain a solid, which is then dried in a vacuum drying oven at 100 °C until constant weight to obtain the catalyst 5.0%Pt-9.0%Cu / CeO2-L6.

[0163] Example 11

[0164] Add 1.29 g of RuCl3·3H2O and 1.62 g of Bi(NO3)2·5H2O to 50 mL of deionized water, stir at 400 r / min, and after complete dissolution, add 10.0 g of γ-Al2O3 support, heat to 120 °C, continue stirring for 6 hours, remove water by rotary evaporation under reduced pressure, obtain a solid and place it in a vacuum drying oven at 100 °C to dry to constant weight; remove it and place it in a muffle furnace, calcine at 500 °C for 6 hours, cool and remove to obtain the precursor. 22.82 g of ligand 2,2'-biquinoline (L7, MW: 256.3) was dispersed in 30 mL of deionized water. After thorough mixing, the precursor was added, the temperature was raised to 120 °C, and the mixture was stirred at 400 r / min for 6 hours. The water was removed by rotary evaporation under reduced pressure to obtain a solid. The solid was placed in a vacuum drying oven at 100 °C and dried to constant weight to obtain catalyst 5.0% Ru-7.0% Bi / γ-Al2O3-L7.

[0165] Example 12

[0166] Add 0.86 g of PtCl4 and 1.62 g of Bi(NO3)2·5H2O to 50 mL of deionized water, stir at 400 r / min, and after complete dissolution, add 10.0 g of BaCeO3 support, heat to 100 °C, continue stirring for 6 hours, remove water by rotary evaporation under reduced pressure, obtain a solid and place it in a vacuum drying oven at 100 °C to dry to constant weight; remove it and place it in a muffle furnace, calcine at 500 °C for 6 hours, cool and remove it to obtain the precursor. 4.67 g of ligand 4,4-dimethyloxazoline (L8, Mw: 101.15) was dispersed in 30 mL of deionized water. After thorough mixing, the precursor was added, the temperature was raised to 120 °C, and the mixture was stirred at 400 r / min for 6 hours. The water was removed by rotary evaporation under reduced pressure to obtain a solid. The solid was placed in a vacuum drying oven at 100 °C and dried to constant weight to obtain catalyst 5.0% Pt-7.0% Bi / BaCeO3-L8.

[0167] Example 13

[0168] Add 0.50 g of PdCl2 and 1.96 g of Ce(NH4)2(NO3)6 to 50 mL of deionized water, stir at 400 rpm until completely dissolved, then add 10.0 g of LaFeO3 support, heat to 100 °C, and continue stirring for 4 hours. Remove moisture by rotary evaporation under reduced pressure to obtain a solid, which is then dried to constant weight in a vacuum drying oven at 100 °C. After drying, place the solid in a muffle furnace and calcine at 500 °C for 6 hours. After cooling, remove the solid to obtain the precursor. Disperse 12.85 g of ligand L9 in 50 mL of deionized water, stir thoroughly, add the precursor, heat to 120 °C, and stir at 400 rpm for 6 hours. Remove moisture by rotary evaporation under reduced pressure to obtain a solid, which is then dried to constant weight in a vacuum drying oven at 100 °C to obtain the catalyst 3.0%Pd-5.0%Ce / LaFeO3-L9.

[0169] Example 14

[0170] Add 0.25 g of Pd(NO3)2·2H2O and 1.62 g of Bi(NO3)2·5H2O to 50 mL of deionized water, stir at 400 r / min until completely dissolved, then add 10.0 g of BaCeO3 support, heat to 100 °C, and continue stirring for 5 hours. Remove moisture by rotary evaporation under reduced pressure to obtain a solid, which is then dried to constant weight in a vacuum drying oven at 100 °C. After drying, place the solid in a muffle furnace and calcine at 500 °C for 6 hours. After cooling, remove the solid to obtain the precursor. Disperse 4.76 g of ligand L10 in 30 mL of deionized water, stir thoroughly, add the precursor, heat to 120 °C, and stir at 400 r / min for 6 hours. Remove moisture by rotary evaporation under reduced pressure to obtain a solid, which is then dried to constant weight in a vacuum drying oven at 100 °C to obtain the catalyst 1.0%Pd-7.0%Bi / LaFeO3-L10.

[0171] Example 15

[0172] Add 0.83 g of PdCl2 and 2.74 g of Ce(NH4)2(NO3)6 to 50 mL of deionized water, stir at 400 rpm until completely dissolved, then add 10.0 g of LaCoO3 support, heat to 160 °C, and continue stirring for 5 hours. Remove moisture by rotary evaporation under reduced pressure to obtain a solid, which is then dried to constant weight in a vacuum drying oven at 100 °C. After drying, place the solid in a muffle furnace and calcine at 500 °C for 8 hours. After cooling, remove the solid to obtain the precursor. Disperse 19.03 g of ligand L10 in 50 mL of deionized water, stir thoroughly, add the precursor, heat to 120 °C, and stir at 400 rpm for 6 hours. Remove moisture by rotary evaporation under reduced pressure to obtain a solid, which is then dried to constant weight in a vacuum drying oven at 100 °C to obtain the catalyst 5.0%Pd-7.0%Ce / LaCoO3-L10.

[0173] Example 16

[0174] Add 0.75 g of Pd(NO3)2·2H2O and 1.62 g of Bi(NO3)2·5H2O to 50 mL of deionized water, stir at 400 r / min until completely dissolved, then add 10.0 g of BaCeO3 support, heat to 160 °C, and continue stirring for 5 hours. Remove moisture by rotary evaporation under reduced pressure to obtain a solid, which is then dried to constant weight in a vacuum drying oven at 100 °C. After drying, place the solid in a muffle furnace and calcine at 500 °C for 6 hours. After cooling, remove the solid to obtain the precursor. Disperse 12.85 g of ligand L10 in 50 mL of deionized water, stir thoroughly, add the precursor, heat to 120 °C, and stir at 400 r / min for 6 hours. Remove moisture by rotary evaporation under reduced pressure to obtain a solid, which is then dried to constant weight in a vacuum drying oven at 100 °C to obtain the catalyst 3.0%Pd-7.0%Bi / BaCeO3-L10.

[0175] Example 17

[0176] Add 1.25 g of Pd(NO3)2·2H2O and 1.62 g of Bi(NO3)2·5H2O to 30 mL of deionized water, stir at 400 r / min until completely dissolved, then add 10.0 g of BaCeO3 support, heat to 160 °C, continue stirring for 5 hours, remove water by rotary evaporation under reduced pressure, obtain a solid and place it in a vacuum drying oven at 100 °C to dry to constant weight; remove and place in a muffle furnace, calcine at 500 °C for 6 hours, cool and remove to obtain the precursor. Disperse 11.89 g of ligand L10 in 50 mL of deionized water, stir thoroughly, add the precursor, heat to 120 °C, stir at 400 r / min for 6 hours, remove water by rotary evaporation under reduced pressure, obtain a solid and place it in a vacuum drying oven at 100 °C to dry to constant weight to obtain catalyst 5.0%Pd-7.0%Bi / BaCeO3-L10. Scanning electron microscopy images of the catalyst morphology are as follows: Figure 1 As shown.

[0177] Example 18

[0178] Add 0.75 g of Bi(NO3)2·5H2O and 3.52 g of Ce(NH4)2(NO3)6 to 30 mL of deionized water, stir at 400 r / min until completely dissolved, then add 10.0 g of BaCeO3 support, heat to 140 °C, continue stirring for 5 hours, remove water by rotary evaporation under reduced pressure, obtain a solid and place it in a vacuum drying oven at 100 °C to dry to constant weight; remove and place in a muffle furnace, calcine at 500 °C for 6 hours, cool and remove to obtain the precursor. Disperse 16.95 g of ligand L10 in 50 mL of deionized water, stir thoroughly, add the precursor, heat to 120 °C, stir at 400 r / min for 6 hours, remove water by rotary evaporation under reduced pressure, obtain a solid and place it in a vacuum drying oven at 100 °C to dry to constant weight to obtain catalyst 7.0%Bi-9.0%Ce / BaCeO3-L10.

[0179] Example 19

[0180] Add 1.62 g of Bi(NO3)2·5H2O and 3.63 g of CoCl2·6H2O to 30 mL of deionized water, stir at 400 r / min until completely dissolved, then add 10.0 g of BaCeO3 support, heat to 140 °C, and continue stirring for 5 hours. Remove moisture by rotary evaporation under reduced pressure to obtain a solid, which is then dried to constant weight in a vacuum drying oven at 100 °C. After drying, place the solid in a muffle furnace and calcine at 500 °C for 6 hours. After cooling, remove the solid to obtain the precursor. Disperse 16.95 g of ligand L10 in 50 mL of deionized water, stir thoroughly, add the precursor, heat to 120 °C, and stir at 400 r / min for 6 hours. Remove moisture by rotary evaporation under reduced pressure to obtain a solid, which is then dried to constant weight in a vacuum drying oven at 100 °C to obtain the catalyst 7.0%Bi-9.0%Co / BaCeO3-L10.

[0181] Example 20

[0182] Add 1.26 g of Pd(NO3)2·2H2O to 30 mL of deionized water, stir at 400 r / min until completely dissolved, then add 10.0 g of BaCeO3 support, heat to 140 °C, continue stirring for 5 hours, remove moisture by rotary evaporation under reduced pressure, obtain a solid and place it in a vacuum drying oven at 100 °C to dry to constant weight; remove and place in a muffle furnace, calcine at 500 °C for 6 hours, cool and remove to obtain the precursor. Disperse 23.79 g of ligand L10 in 50 mL of deionized water, stir thoroughly, add the precursor, heat to 120 °C, stir at 400 r / min for 6 hours, remove moisture by rotary evaporation under reduced pressure, obtain a solid and place it in a vacuum drying oven at 100 °C to dry to constant weight to obtain catalyst 5.0% Pd / BaCeO3-L10.

[0183] Example 21

[0184] Add 2.09 g of Bi(NO3)2·5H2O to 30 mL of deionized water, start stirring at 400 r / min, and after complete dissolution, add 10.0 g of BaCeO3 support, heat to 140 °C, continue stirring for 5 hours, remove water by rotary evaporation under reduced pressure, obtain a solid and place it in a vacuum drying oven at 100 °C to dry to constant weight; remove it and place it in a muffle furnace, calcine at 500 °C for 6 hours, cool and remove it to obtain catalyst 9.0% Bi / BaCeO3.

[0185] Example 22

[0186] In a high-pressure reactor, 50.0 g of acetone and 2.5 g of catalyst 5.0% Pd-7.0% Bi / BaCeO3-L1 (catalyst mass concentration 5.0%) were added. The reactor was purged with nitrogen three times, followed by purging with acetylene three times. Stirring was started, and the temperature was set to 40°C. The reaction was carried out at a constant temperature, maintaining an acetylene pressure of 0.20 MPa. After 4.0 hours of reaction, the pressure was released, the reaction solution was discharged, and the catalyst was filtered out. Gas chromatography analysis of the reaction solution showed an acetone conversion rate of 98.61% and a selectivity of 95.53% for 2-methyl-3-butyn-2-ol.

[0187] The reaction solution was distilled under reduced pressure to recover unreacted raw materials, yielding 68.11 g of crude 2-methyl-3-butyn-2-ol, with a calculated yield of 94.08%.

[0188] Example 23

[0189] In a high-pressure reactor, 50.0 g of acetone and 1.5 g of catalyst 5.0% Pd-5.0% Bi / BaCeO3-L10 (catalyst mass concentration 3.0%) were added. The reactor was purged with nitrogen three times, followed by purging with acetylene three times. Stirring was started, and the temperature was set to 50°C. The reaction was carried out at a constant temperature, maintaining an acetylene pressure of 0.20 MPa. After 4.0 hours of reaction, the pressure was released, the reaction solution was discharged, and the catalyst was filtered out. Gas chromatography analysis of the reaction solution showed an acetone conversion rate of 98.82% and a selectivity of 96.71% for 2-methyl-3-butyn-2-ol.

[0190] The reaction solution was distilled under reduced pressure to recover unreacted raw materials, yielding 69.09 g of crude 2-methyl-3-butyn-2-ol, with a calculated yield of 95.43%.

[0191] Example 24

[0192] In a high-pressure reactor, add 50.0 g acetone, 3.5 g catalyst (5.0% Pd-7.0% Bi / BaCeO3-L10, catalyst mass concentration 7.0%), and 50.0 g ethanol. Purge the mixture three times with nitrogen, then purge three times with acetylene. Start stirring and set the temperature to 60°C. Maintain a constant temperature reaction and keep the acetylene pressure at 0.20 MPa. After 4.5 hours of reaction, release the pressure, discharge the reaction solution, and filter out the catalyst. Gas chromatography analysis of the reaction solution showed an acetone conversion of 99.62% and a selectivity of 99.53% for 2-methyl-3-butyn-2-ol. The gas chromatogram of the reaction solution is shown below. Figure 1 As shown.

[0193] The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials, yielding 71.71 g of crude 2-methyl-3-butyn-2-ol, with a calculated yield of 99.05%.

[0194] Example 25

[0195] In a high-pressure reactor, add 50.0 g of acetone, 2.5 g of catalyst (5.0% Pd-5.0% Bi / BaCeO3-L10, catalyst mass concentration 5.0%), and 50.0 g of deionized water. Purge the mixture three times with nitrogen, then purge three times with acetylene. Start stirring and set the temperature to 60°C. Maintain a constant temperature reaction and keep the acetylene pressure at 0.20 MPa. After 4 hours of reaction, release the pressure, discharge the reaction solution, and filter out the catalyst. Gas chromatography analysis of the reaction solution showed an acetone conversion rate of 98.62% and a selectivity of 93.28% for 2-methyl-3-butyn-2-ol.

[0196] The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials, yielding 66.27 g of crude 2-methyl-3-butyn-2-ol, with a calculated yield of 91.53%.

[0197] Example 26

[0198] In a high-pressure reactor, 70.0 g of butanone, 3.51 g of catalyst 3.0% Pd-5.0% Bi / BaCeO3-L10 (catalyst mass concentration 5.0%), and 70.0 g of ethanol were added. The reactor was purged with nitrogen three times, followed by purging with acetylene three times. Stirring was started, and the temperature was set to 60°C for constant temperature reaction, maintaining an acetylene pressure of 0.20 MPa. After 4 hours of reaction, the pressure was released, the reaction solution was expelled, and the catalyst was filtered out. Gas chromatography analysis of the reaction solution showed a butanone conversion rate of 98.73% and a 3-methyl-pentyn-3-ol selectivity of 94.93%.

[0199] The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials, yielding 90.19 g of crude 3-methyl-pentyn-3-ol, with a calculated yield of 94.67%.

[0200] Example 27

[0201] In a high-pressure reactor, 100.0 g of 6-methyl-5-hepten-2-one, 7.0 g of catalyst (7.0% Pd-5.0% Nb / CaFeO3-L2, catalyst mass concentration 7.0%), and 100.0 g of ethanol were added. The reactor was purged with nitrogen three times, followed by purging with acetylene three times. Stirring was started, and the temperature was set to 50°C. The reaction was carried out at a constant temperature, maintaining an acetylene pressure of 0.20 MPa. After 3 hours of reaction, the pressure was released, the reaction solution was expelled, and the catalyst was filtered out. Gas chromatography analysis of the reaction solution showed a 98.02% conversion rate of 6-methyl-5-hepten-2-one and a 95.78% selectivity for dehydrolinalool.

[0202] The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials, yielding 112.86 g of crude dehydrolinalool, with a calculated yield of 93.56%.

[0203] Example 28

[0204] In a high-pressure reactor, 100.0 g of 6-methyl-5-octen-2-one, 5.0 g of catalyst (5.0% Ru-9.0% Ce / LaCoO3-L3, catalyst mass concentration 5.0%), and 100.0 g of ethanol were added. The reactor was purged with nitrogen three times, followed by purging with acetylene three times. Stirring was started, and the temperature was set to 50°C. The reaction was carried out at a constant temperature, maintaining an acetylene pressure of 0.20 MPa. After 4.5 hours of reaction, the pressure was released, the reaction solution was expelled, and the catalyst was filtered out. Gas chromatography analysis of the reaction solution showed a 98.12% conversion rate of 6-methyl-5-octen-2-one and a 97.48% selectivity for dehydroethyl linalool.

[0205] The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials, yielding 113.21 g of crude dehydroethyl linalool, with a calculated yield of 95.48%.

[0206] Example 29

[0207] In a high-pressure reactor, 100.0 g of 6-methyl-2-heptanone, 5.0 g of catalyst (5.0% Ru-9.0% Ce / LaCoO3-L3, catalyst mass concentration 5.0%), and 100.0 g of ethanol were added. The reactor was purged with nitrogen three times, followed by purging with acetylene three times. Stirring was started, and the temperature was set to 60°C. The reaction was carried out at a constant temperature, maintaining an acetylene pressure of 0.20 MPa. After 4 hours of reaction, the pressure was released, the reaction solution was expelled, and the catalyst was filtered out. Gas chromatography analysis of the reaction solution showed a 98.30% conversion rate of 6-methyl-2-heptanone and a 97.63% selectivity for dihydrodehydrolinalool.

[0208] The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials, yielding 115.26 g of crude dihydrodehydrolinalool, with a calculated yield of 95.80%.

[0209] Example 30

[0210] In a high-pressure reactor, 100.0 g of furfural, 5.0 g of catalyst (5.0% Ru-7.0% Bi / LaFeO3-L3, catalyst mass concentration 5.0%), and 100.0 g of toluene were added. The reactor was purged with nitrogen three times, followed by purging with acetylene three times. Stirring was started, and the temperature was set to 40°C. The reaction was carried out at a constant temperature, maintaining an acetylene pressure of 0.20 MPa. After 3.5 hours of reaction, the pressure was released, the reaction solution was expelled, and the catalyst was filtered out. Gas chromatography analysis of the reaction solution showed a furfural conversion rate of 98.44% and a furfural acetylene alcohol selectivity of 97.89%.

[0211] The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials, yielding 123.61 g of crude furfuryl ethynyl alcohol, with a calculated yield of 95.25%.

[0212] Example 31

[0213] In a high-pressure reactor, 100.0 g of geranylacetone, 7.0 g of catalyst (3.0% Pd-5.0% Ce / BaCeO3-L1, catalyst mass concentration 7.0%), and 100.0 g of isopropanol were added. The reactor was purged with nitrogen three times, followed by acetylene purging three times. Stirring was started, and the temperature was set to 60°C. The reaction was carried out at a constant temperature, maintaining an acetylene pressure of 0.20 MPa. After 4 hours of reaction, the pressure was released, the reaction solution was discharged, and the catalyst was filtered out. Gas chromatography analysis of the reaction solution showed a geranylacetone conversion rate of 97.64% and a dehydroneryl alcohol selectivity of 97.23%.

[0214] The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials, yielding 107.58 g of crude dehydronervate tertrol, with a calculated yield of 94.87%.

[0215] Example 32

[0216] In a high-pressure reactor, 100.0 g of tetrahydrogeranylacetone, 7.0 g of catalyst (5.0% Pt-10.0% Cu / LaNiO3-L4, mass concentration 7.0%), and 100.0 g of methanol were added. The reactor was purged with nitrogen three times, followed by purging with acetylene three times. Stirring was started, and the temperature was set to 50°C. The reaction was carried out at a constant temperature, maintaining an acetylene pressure of 0.20 MPa. After 5.0 hours of reaction, the pressure was released, the reaction solution was expelled, and the catalyst was filtered out. Gas chromatography analysis of the reaction solution showed a geranylacetone conversion rate of 97.82% and a tetrahydrodehydroneryl tertrol selectivity of 96.05%.

[0217] The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials, yielding 106.12 g of crude tetrahydrodehydroneraniol, with a calculated yield of 93.81%.

[0218] Example 33

[0219] In a high-pressure reactor, 100.0 g of phytoketone, 7.0 g of catalyst (3.0% Pd-7.0% Co / LaFeO3-L5, catalyst mass concentration 7.0%), and 100.0 g of ethanol were added. The reactor was purged with nitrogen three times, followed by purging with acetylene three times. Stirring was started, and the temperature was set to 60°C. The reaction was carried out at a constant temperature, maintaining an acetylene pressure of 0.20 MPa. After 5.0 hours of reaction, the pressure was released, the reaction solution was discharged, and the catalyst was filtered out. Gas chromatography analysis of the reaction solution showed a phytoketone conversion rate of 97.42% and a dehydroisophytol selectivity of 97.35%.

[0220] The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials, yielding 103.90 g of crude dehydroisophytol, with a calculated yield of 94.72%.

[0221] Example 34

[0222] In a high-pressure reactor, 100.0 g of acetone, 7.0 g of catalyst (5.0% Pt-9.0% Cu / CeO2-L6, catalyst mass concentration 7.0%), and 100.0 g of ethanol were added. The reactor was purged with nitrogen three times, followed by purging with acetylene three times. Stirring was started, and the temperature was set to 60°C. The reaction was carried out at a constant temperature, maintaining an acetylene pressure of 0.20 MPa. After 5.0 hours of reaction, the pressure was released, the reaction solution was discharged, and the catalyst was filtered out. Gas chromatography analysis of the reaction solution showed an acetone conversion rate of 98.48% and a selectivity of 96.01% for 2-methyl-3-butyn-2-ol.

[0223] The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials, yielding 68.31 g of crude 2-methyl-3-butyn-2-ol, with a calculated yield of 94.26%.

[0224] Example 35

[0225] In a high-pressure reactor, 100.0 g of butanone, 7.0 g of catalyst (5.0% Ru-7.0% Bi / γ-Al₂O₃-L₇, catalyst mass concentration 7.0%), and 100.0 g of ethanol were added. The reactor was purged with nitrogen three times, followed by purging with acetylene three times. Stirring was started, and the temperature was set to 40°C. The reaction was carried out at a constant temperature, maintaining an acetylene pressure of 0.20 MPa. After 5.0 hours of reaction, the pressure was released, the reaction solution was discharged, and the catalyst was filtered out. Gas chromatography analysis of the reaction solution showed a butanone conversion rate of 96.57% and a 3-methyl-pentyn-3-ol selectivity of 95.62%.

[0226] The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials, yielding 125.43 g of crude 3-methyl-pentyn-3-ol, with a calculated yield of 92.16%.

[0227] Example 36

[0228] In a high-pressure reactor, 100.0 g of 6-methyl-5-hepten-2-one, 7.0 g of catalyst (5.0% Pt-7.0% Bi / BaCeO3-L8, catalyst mass concentration 7.0%), and 100.0 g of ethanol were added. The reactor was purged with nitrogen three times, followed by purging with acetylene three times. Stirring was started, and the temperature was set to 60°C. The reaction was carried out at a constant temperature, maintaining an acetylene pressure of 0.20 MPa. After 4.0 hours of reaction, the pressure was released, the reaction solution was expelled, and the catalyst was filtered out. Gas chromatography analysis of the reaction solution showed a 97.69% conversion rate of 6-methyl-5-hepten-2-one and a 96.73% selectivity for dehydrolinalool.

[0229] The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials, yielding 113.83 g of crude dehydrolinalool, with a calculated yield of 94.36%.

[0230] Example 37

[0231] In a high-pressure reactor, 100.0 g of 6-methyl-5-octen-2-one, 9.0 g of catalyst 3.0% Pd-5.0% Ce / LaFeO3-L9 (catalyst mass concentration 9.0%), and 100.0 g of ethanol were added. The reactor was purged with nitrogen three times, followed by purging with acetylene three times. Stirring was started, and the temperature was set to 60°C. The reaction was carried out at a constant temperature, maintaining an acetylene pressure of 0.20 MPa. After 3.0 hours of reaction, the pressure was released, the reaction solution was expelled, and the catalyst was filtered out. Gas chromatography analysis of the reaction solution showed that the conversion rate of 6-methyl-5-octen-2-one was 98.64%, and the selectivity of dehydroethyl linalool was 96.51%.

[0232] The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials, yielding 112.71 g of crude dehydroethyl linalool, with a calculated yield of 95.06%.

[0233] Example 38

[0234] In a high-pressure reactor, 100.0 g of 6-methyl-2-heptanone, 7.0 g of catalyst 1.0% Pd-7.0% Bi / LaFeO3-L10 (catalyst mass concentration 7.0%), and 100.0 g of ethanol were added. The reactor was purged with nitrogen three times, followed by purging with acetylene three times. Stirring was started, and the temperature was set to 50°C. The reaction was carried out at a constant temperature, maintaining an acetylene pressure of 0.20 MPa. After 4.0 hours of reaction, the pressure was released, the reaction solution was expelled, and the catalyst was filtered out. Gas chromatography analysis of the reaction solution showed a 95.31% conversion of 6-methyl-5-octen-2-one and a 96.34% selectivity for dihydrodehydrolinalool.

[0235] The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials, yielding 110.36 g of crude dihydrodehydrolinalool, with a calculated yield of 91.73%.

[0236] Example 39

[0237] In a high-pressure reactor, 100.0 g of furfural, 5.0 g of catalyst (5.0% Pd-7.0% Ce / LaCoO3-L10, catalyst mass concentration 5.0%), and 100.0 g of ethanol were added. The reactor was purged with nitrogen three times, followed by purging with acetylene three times. Stirring was started, and the temperature was set to 50°C. The reaction was carried out at a constant temperature, maintaining an acetylene pressure of 0.20 MPa. After 6.0 hours of reaction, the pressure was released, the reaction solution was discharged, and the catalyst was filtered out. Gas chromatography analysis of the reaction solution showed a furfural conversion rate of 99.31% and a furfural acetylene alcohol selectivity of 98.29%.

[0238] The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials, yielding 126.53 g of crude furfuryl ethynyl alcohol, with a calculated yield of 97.50%.

[0239] Example 40

[0240] In a high-pressure reactor, 100.0 g of geranylacetone, 5.0 g of catalyst (3.0% Pd-7.0% Bi / BaCeO3-L10, catalyst mass concentration 5.0%), and 100.0 g of ethanol were added. The reactor was purged with nitrogen three times, followed by purging with acetylene three times. Stirring was started, and the temperature was set to 60°C. The reaction was carried out at a constant temperature, maintaining an acetylene pressure of 0.20 MPa. After 3.5 hours of reaction, the pressure was released, the reaction solution was expelled, and the catalyst was filtered out. Gas chromatography analysis of the reaction solution showed a geranylacetone conversion rate of 99.52% and a dehydroneryl alcohol selectivity of 98.37%.

[0241] The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials, yielding 110.69 g of crude dehydronervate tertrol, with a calculated yield of 97.61%.

[0242] Example 41

[0243] In a high-pressure reactor, 100.0 g of 6-methyl-5-octen-2-one, 5.0 g of catalyst (5.0% Pd-7.0% Bi / BaCeO3-L10, catalyst mass concentration 5.0%), and 100.0 g of ethanol were added. The reactor was purged with nitrogen three times, followed by purging with acetylene three times. Stirring was started, and the temperature was set to 60°C. The reaction was carried out at a constant temperature, maintaining an acetylene pressure of 0.20 MPa. After 3.0 hours of reaction, the pressure was released, the reaction solution was expelled, and the catalyst was filtered out. Gas chromatography analysis of the reaction solution showed a 99.72% conversion rate of 6-methyl-5-octen-2-one and a 98.58% selectivity for dehydroethyl linalool.

[0244] The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials, yielding 116.48 g of crude dehydroethyl linalool, with a calculated yield of 98.24%.

[0245] Example 42

[0246] In a high-pressure reactor, 100.0 g of 6-methyl-5-octen-2-one, 1.0 g of catalyst 5.0% Pd-7.0% Bi / BaCeO3-L10 (catalyst mass concentration 1.0%), and 100.0 g of ethanol were added. The reactor was purged with nitrogen three times, followed by purging with acetylene three times. Stirring was started, and the temperature was set to 60°C. The reaction was carried out at a constant temperature, maintaining an acetylene pressure of 0.20 MPa. After 5.0 hours of reaction, the pressure was released, the reaction solution was expelled, and the catalyst was filtered out. Gas chromatography analysis of the reaction solution showed a conversion rate of 89.49% for 6-methyl-5-octen-2-one and a selectivity of 97.61% for dehydroethyl linalool.

[0247] The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials, yielding 103.43 g of crude dehydroethyl linalool, with a calculated yield of 87.23%.

[0248] Example 43

[0249] In a high-pressure reactor, 100.0 g of 6-methyl-5-hepten-2-one (98.5% purity), 5.0 g of catalyst 5.0% Pd-7.0% Bi / BaCeO3-L10 (catalyst mass concentration 5.0%), and 100.0 g of ethanol were added. The reactor was purged with nitrogen three times, followed by purging with acetylene three times. Stirring was started, and the temperature was set to 60°C. The reaction was carried out at a constant temperature, maintaining an acetylene pressure of 0.20 MPa. After 5.0 hours of reaction, the pressure was released, the reaction solution was discharged, and the catalyst was filtered out. Gas chromatography analysis of the reaction solution showed a 98.69% conversion of 6-methyl-5-hepten-2-one and a 97.74% selectivity for dehydrolinalool. The gas chromatogram of the reaction solution is shown below. Figure 2 As shown.

[0250] The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials, yielding 125.07 g of crude dehydrolinalool, with a calculated yield of 96.37%.

[0251] Example 44

[0252] In a high-pressure reactor, 50.0 g of formaldehyde, 5.0 g of catalyst (5.0% Pd-7.0% Bi / BaCeO3-L10, catalyst mass concentration 5.0%), and 100.0 g of ethanol were added. The reactor was purged with nitrogen three times, followed by purging with acetylene three times. Stirring was started, and the temperature was set to 30°C. The reaction was carried out at a constant temperature, maintaining an acetylene pressure of 0.20 MPa. After 4.0 hours of reaction, the pressure was released, the reaction solution was discharged, and the catalyst was filtered out. Gas chromatography analysis of the reaction solution showed a formaldehyde conversion rate of 99.67% and a propargyl alcohol selectivity of 98.38%.

[0253] The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials, yielding 91.41 g of crude propargyl alcohol, with a calculated yield of 97.92%.

[0254] Example 45

[0255] In a high-pressure reactor, 100.0 g of tetrahydrogeranylacetone, 10.0 g of catalyst 7.0% Bi-9.0% Ce / BaCeO3-L10 (catalyst mass concentration 10.0%), and 100.0 g of ethanol were added. The reactor was purged with nitrogen three times, followed by purging with acetylene three times. Stirring was started, and the temperature was set to 40°C. The reaction was carried out at a constant temperature, maintaining an acetylene pressure of 0.20 MPa. After 6.0 hours of reaction, the pressure was released, the reaction solution was expelled, and the catalyst was filtered out. Gas chromatography analysis of the reaction solution showed a tetrahydrogeranylacetone conversion of 90.71% and a tetrahydrodehydronerol selectivity of 89.64%.

[0256] The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials, yielding 91.74 g of crude tetrahydrodehydroneraniol, with a calculated yield of 81.10%.

[0257] Example 46

[0258] In a high-pressure reactor, 100.0 g of phytoketone, 10.0 g of catalyst 7.0% Bi-9.0% Co / BaCeO3-L10 (catalyst mass concentration 10.0%), and 100.0 g of ethanol were added. The reactor was purged with nitrogen three times, followed by purging with acetylene three times. Stirring was started, and the temperature was set to 60°C. The reaction was carried out at a constant temperature, maintaining an acetylene pressure of 0.20 MPa. After 6.0 hours of reaction, the pressure was released, the reaction liquid was expelled, and the catalyst was filtered out. Gas chromatography analysis of the reaction liquid showed a phytoketone conversion rate of 91.52% and a dehydroisophytol selectivity of 85.23%.

[0259] The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials, yielding 85.20g of crude dehydroisophytol, with a calculated yield of 77.67%.

[0260] Example 47

[0261] In a high-pressure reactor, 100.0 g of 6-methyl-5-octen-2-one, 10.0 g of 5.0% Pd / BaCeO3-L10 catalyst (catalyst mass concentration 10.0%), and 100.0 g of ethanol were added. The reactor was purged with nitrogen three times, followed by purging with acetylene three times. Stirring was started, and the temperature was set to 60°C. The reaction was carried out at a constant temperature, maintaining an acetylene pressure of 0.20 MPa. After 6.0 hours of reaction, the pressure was released, the reaction solution was expelled, and the catalyst was filtered out. Gas chromatography analysis of the reaction solution showed a conversion rate of 89.82% for 6-methyl-5-octen-2-one and a selectivity of 86.29% for dehydroethyl linalool.

[0262] The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials, yielding 91.67 g of crude dehydroethyl linalool, with a calculated yield of 77.31%.

[0263] Comparative Example 1

[0264] In a high-pressure reactor, 100.0 g of 6-methyl-5-octen-2-one, 10.0 g of 9.0% Bi / BaCeO3 catalyst (catalyst mass concentration 10.0%), and 100.0 g of ethanol were added. The reactor was purged with nitrogen three times, followed by purging with acetylene three times. Stirring was started, and the temperature was set to 60°C. The reaction was carried out at a constant temperature, maintaining an acetylene pressure of 0.20 MPa. After 6.0 hours of reaction, the pressure was released, the reaction solution was expelled, and the catalyst was filtered out. Gas chromatography analysis of the reaction solution showed a conversion rate of 80.26% for 6-methyl-5-octen-2-one and a selectivity of 62.34% for dehydroethyl linalool.

[0265] The reaction solution was distilled under reduced pressure to recover the solvent and unreacted raw materials, yielding 58.72 g of crude dehydroethyl linalool, with a calculated yield of 49.52%.

[0266] The above embodiments and comparative data are shown in Table 1:

[0267] Table 1:

[0268]

[0269] Example 48

[0270] The catalyst recovered in Example 43 was directly used in the catalyst reuse experiment, and the reaction conditions and operation were the same as in Example 43.

[0271] The experimental results are shown in Table 2.

[0272] Table 2:

[0273] Apply Substrate Conversion rate Selective crude product quantity Yield 1 6-Methyl-5-hepten-2-one 98.69% 97.75% 125.03g 96.35% 2 6-Methyl-5-hepten-2-one 98.58% 97.66% 124.74g 96.12% 3 6-Methyl-5-hepten-2-one 98.60% 97.67% 124.81g 96.18% 4 6-Methyl-5-hepten-2-one 98.46% 97.61% 124.58g 96.0%

[0274] It should be noted that although the technical solution of the present invention has been described with specific examples, those skilled in the art will understand that the present invention should not be limited thereto.

[0275] The various embodiments of the present invention have been described above. These descriptions are exemplary and not exhaustive, nor are they limited to the disclosed embodiments. Many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments. The terminology used herein is chosen to best explain the principles, practical application, or technical improvements to the embodiments in the market, or to enable others skilled in the art to understand the embodiments disclosed herein.

Claims

1. A catalyst for preparing alkynols via the reaction of a carbonyl-containing compound with a terminal alkynyl-containing compound, characterized in that, The catalyst comprises a modifier and a metal oxide system, wherein the metal oxide system is a support oxide doped with a first metal element, and the support oxide is selected from one or more of CeO2, BaCeO3, CaFeO3, LaCoO3, LaNiO3, LaFeO3, and γ-Al2O3, or a mixture thereof. Using a carrier oxide doped with the first metal element means that at least a portion of the first metal element has entered the crystal structure of the carrier oxide. in, The modifier comprises a nitrogen-containing heterocyclic compound, which is selected from one or more nitrogen-containing heterocyclic compounds from the following L1 to L10: The first metallic element includes one or more of Pd, Ru, Pt, Nb, Bi, Cu, and Co. Furthermore, the modifier is present in at least a portion of the surface region of the metal oxide system; The carbonyl-containing compound has the molecular formula represented by the following formula (I): (I) Among them, R1 and R2 may be the same or different each time they appear, and are independently hydrogen or monovalent organic groups, or R1 and R2 may be connected to form a ring, provided that R1 and R2 are not both hydrogen at the same time; The compound containing the terminal alkyne group is acetylene.

2. The catalyst according to claim 1, characterized in that, In the metal oxide system, the content of the first metal element is 0.1 to 10% of the mass of the doped carrier oxide.

3. The catalyst according to claim 1 or 2, characterized in that, In the catalyst, the molar ratio of the nitrogen-containing heterocyclic compound to the first metal element is 10 to 20:

1.

4. The catalyst according to claim 1 or 2, characterized in that, The first metallic element includes two or more elements selected from Pd, Ru, Pt, Nb, Bi, Cu, and Co.

5. A method for preparing alkynols, characterized in that, The method includes: The step of reacting a carbonyl-containing compound with a terminal alkyne-containing compound in the presence of the catalyst according to any one of claims 1 to 4, wherein the reaction is carried out with or without a solvent. The carbonyl-containing compound has the molecular formula represented by the following formula (I): (I) Among them, R1 and R2 may be the same or different each time they appear, and are independently hydrogen or monovalent organic groups, or R1 and R2 may be connected to form a ring, provided that R1 and R2 are not both hydrogen at the same time; The compound containing the terminal alkyne group is acetylene.

6. The method according to claim 5, characterized in that, The reaction temperature is 30-70℃, and the reaction time is 3-6 hours.

7. The method according to claim 5 or 6, characterized in that, The catalyst is either a newly prepared catalyst or a reused catalyst.

Citation Information

Patent Citations

  • Novel synthetic method preparing alkynol compound from acetylene

    CN102476978A

  • An alkynol preparing method

    CN104744211A

  • Novel process for synthesizing alkynol from acetylene and ketone compounds

    CN106117010A

  • Method for synthesizing propargyl alcohol

    CN107032956A

  • An acetylation method