Aramid nanofiber and carbonyl iron powder composite aerogel and its preparation method and application
The composite aerogel material prepared by combining aramid nanofibers with carbonyl iron powder has solved the shortcomings of existing microwave absorbing materials in broadband, low density and low matching thickness, and achieved high-performance microwave absorption effect. In the fields of aerospace, microwave darkrooms, etc.
Patent Information
- Application Number
- CN202310668288.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-07
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-06-07
AI Technical Summary
Existing microwave absorbing materials do not perform well in broadband, low density and low matching thickness, making it difficult to meet the demand for high-performance absorbing materials in military fields, especially materials such as carbon nanotubes and graphene. , magnetic metals and oxides have narrow bandwidth and large density.
Using the preparation method of aramid nanofiber and carbonyl iron powder composite aerogel, aramid and dimethyl sulfoxide are dispersed in potassium hydroxide solution and stirred in a potassium hydroxide solution, and then filtration is carried out with carbonyl iron powder in ethanol solution. Ultrasonic liquid phase peeling and freeze-drying were prepared to produce porous aerogels with a density of 25-60 mg/cm3.
The effective absorption bandwidth of electromagnetic waves reaches 11.2GHz when the thickness is 1.6mm, the maximum reflection loss is -14.7dB, and the maximum reflection loss is -42.6dB when the thickness is 2.4mm, and it has a wide microwave absorption frequency band and strong microwave absorption capacity. Low density and low matching thickness have expanded the application field of wave absorbing materials.
Smart Images

Figure CN116655997B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of microwave absorbing materials, and more specifically, relates to an aramid nanofiber and carbonyl iron powder composite aerogel and a preparation method and application thereof. Background Art
[0002] With the widespread use of electronic devices, electromagnetic technology has been applied to all walks of life. Although the application of many electronic products has brought many conveniences to people, electromagnetic radiation pollution is difficult to avoid and has threatened the production and living environment of human beings. Therefore, it is urgent to design ideal high-quality microwave absorbing materials, especially microwave absorbing materials with wide microwave absorption band, strong microwave absorption ability, low density and low matching thickness. In recent years, porous aerogels have attracted widespread attention due to their lightweight and porous properties.
[0003] Reference 1 "Ma, Y.; Li, Y.; Zhao, X.; Zhang, L.; Wang, B.; Nie, A.; Mu, C.; Xiang, J.; Zhai, K.; Xue, T.; Wen, F. Lightweight and multifunctional super-hydrophobic aramidnanofiber / multiwalled carbon nanotubes / Fe3O4aerogel for microwave ab-sorption, thermal insulation and pollutants adsorption. Journal of Alloys and Com-pounds. 2022, 919." reported the carbon nanotube / Fe3O4 nanoparticle composite aerogel modified with trimethoxymethylsilane prepared by vacuum assisted filtration, freeze drying and vapor deposition method. The results showed that at a microwave frequency of 5.46 GHz, the minimum reflection loss can reach -45.83 dB, and at a thickness of
[0004] At 1.4mm, the maximum effective absorption bandwidth is 4.0GHz.
[0005] Reference 2 "Hao C.; Wang B.; Wen F S.; Mu, C.; Xiang, J.; Li, L.; Liu, Z. Superior microwave absorption properties of ultralight reduced graphene oxide / blackphos-phorus aerogel. Nanotechnology, 2018, 29 (23)" reported a successful preparation of ultralight reduced graphene oxide / black phosphorus (rGO / BP) composite aerogel by self-assembly process. With a thickness of 2.53 mm, the minimum reflection loss value of -46.9 dB was obtained, and a wide absorption band of 6.1 GHz was achieved.
[0006] Reference 3 “Xu, J.; Zhang, X.; Zhao, Z.; Hu, H.; Li, B.; Zhu, C.; Zhang, X.; Chen, Y. Lightweight, Fire-Retardant, and Anti-Compressed Honeycombed-Like Carbon Aerogels for Thermal Management and High-Efficiency Electromagnetic Absorb-ing Properties. Small 2021, 17(33), e2102032.” reported that carbon aerogels (0.017 g cm) containing Co@C nanoparticles were prepared by directional freeze casting and carbonization. -3 ), showing excellent performance, with a maximum reflection loss of -45.02dB at 1.5mm and an effective absorption bandwidth of 4.02GHz.
[0007] Reference 4 "Liang, L.; Li, Q.; Yan, X.; Feng, Y.; Wang, Y.; Zhang, HB; Zhou, X.; Liu, C.; Shen, C.; Xie, X. Multifunctional Magnetic Ti3C2Tx MXene / Graphene Aerogel with Superior Electromagnetic Wave Absorption Performance. ACS Nano 2021, 15(4), 6622-6632." reported that a three-dimensional MXene / reduced graphene oxide (RGO) aerogel anchored by magnetic nickel nanochains was constructed by directional freezing method and hydrazine vapor reduction process. The minimum reflection loss at 2.15 mm was -75.2 dB, and the effective absorption bandwidth was 5.4 GHz; its widest effective absorption bandwidth was 7.3 GHz.
[0008] Reference 5 "Yang, J.; Wang, J.; Li, H.; Wu, Z.; Xing, Y.; Chen, Y.; Liu, L. MoS2 / MXeneAerogel with Conformal Heterogeneous Interfaces Tailored by Atomic LayerDeposition for Tunable Microwave Absorption. Adv Sci (Weinh) 2022, 9 (7), e2101988." reported that a three-dimensional porous MoS2 / MXene hybrid aerogel structure with conformal heterogeneous interfaces was constructed by atomic layer deposition (ALD) method, and its microwave absorption performance was fully optimized. The MoS2 / MXene hybrid aerogel prepared under 300 ALD cycles had the lowest reflection loss of -61.65 dB at a thickness of 4.53 mm.
[0009] The above documents have prepared some composite aerogels with wave-absorbing properties. Although these aerogels have good reflection loss performance, they cannot be light in weight and thin in thickness at the same time, and the effective absorption bandwidth is limited (less than 10GHz), which greatly limits the further application of such materials in the field of wave absorption. For example, in the military field, in order to prevent radar monitoring, the performance requirements of wave-absorbing materials are very high, and existing materials are often difficult to meet the requirements. Carbon materials such as carbon nanotubes and graphene have too high conductivity, resulting in impedance mismatch; materials such as magnetic metals and oxides have narrow bandwidths and high densities, which are difficult to meet practical applications.
[0010] In view of this, the present application proposes a new composite material to solve the above problems. Summary of the invention
[0011] The purpose of the present invention is to provide an aramid nanofiber and carbonyl iron powder composite aerogel and a preparation method and application thereof.
[0012] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0013] In the first aspect, the present application proposes a method for preparing a composite aerogel of aramid nanofibers and carbonyl iron powder, which comprises:
[0014] Dispersing aramid and dimethyl sulfoxide in a potassium hydroxide solution with a concentration of 2-5 mg / ml, stirring at room temperature for 3-5 hours, vacuum filtering and washing to obtain aramid nanofibers;
[0015] Aramid nanofibers and carbonyl iron powder are dispersed in an ethanol solution at a mass ratio of 1:3-7, ultrasonic liquid phase stripping is performed for 0.5-2h, and vacuum filtration is performed to obtain a composite hydrogel of aramid nanofibers and carbonyl iron powder;
[0016] The aramid nanofiber and carbonyl iron powder composite hydrogel is freeze-dried under vacuum conditions to obtain the aramid nanofiber and carbonyl iron powder composite aerogel.
[0017] Furthermore, in a preferred embodiment of the present invention, the aramid nanofiber is prepared by the following method:
[0018] Disperse aramid and dimethyl sulfoxide in potassium hydroxide solution, stir at room temperature for 3-5 hours, and vacuum filter and wash.
[0019] Furthermore, in a preferred embodiment of the present invention, the concentration of the potassium hydroxide solution is 2-5 mg / ml.
[0020] Furthermore, in a preferred embodiment of the present invention, the mass volume ratio of the aramid fiber to the dimethyl sulfoxide is 1g:450-500ml.
[0021] Furthermore, in a preferred embodiment of the present invention, the ultrasonic power in the ultrasonic liquid phase stripping is 500-700w.
[0022] Furthermore, in a preferred embodiment of the present invention, the ethanol solution is an ethanol-water solution with a volume fraction of 60-90%.
[0023] Furthermore, in a preferred embodiment of the present invention, in the vacuum filtration step, an organic microporous micromembrane with a diameter of 0.45 μm is used.
[0024] In the second aspect, the present application provides an aramid nanofiber and carbonyl iron powder composite aerogel, which is prepared by the above preparation method, and the density of the aramid nanofiber and carbonyl iron powder composite aerogel is: 25-60 mg / cm 3 .
[0025] In a third aspect, the present application provides a microwave absorbing material comprising the above-mentioned aramid nanofiber and carbonyl iron powder composite aerogel.
[0026] Furthermore, in a preferred embodiment of the present invention, the aramid nanofiber and carbonyl iron powder composite aerogel has the following properties:
[0027] When the thickness is 1.6mm, the effective absorption bandwidth of electromagnetic waves reaches 11.2GHz, and the maximum reflection loss is -14.7dB;
[0028] When the thickness is 2.4mm, the effective absorption bandwidth of electromagnetic waves reaches 3.63GHz, and the maximum reflection loss is -42.6dB.
[0029] The design concept of the present invention is as follows:
[0030] Carbonyl iron powder is suitable as a magnetic loss material in the field of microwave absorption due to its strong ferromagnetism. However, carbonyl iron powder also has many disadvantages, such as low dielectric loss, narrow absorption bandwidth, high density, etc., so its practical application value is not good. At present, many researchers have controlled carbonyl iron powder through morphology control, composite of multiple materials and other means to obtain better microwave performance. Usually, morphology control requires high temperature, high pressure, etc., and the preparation process is relatively complex and energy-consuming; composite with other materials will increase costs, and the performance of the introduced material itself also needs to be considered.
[0031] In the prior art, carbon nanofiber aerogel is obtained by calcining aramid nanofibers at high temperature and applied in the field of microwave absorption. However, the microwave absorption performance of this aerogel is poor. For example, the maximum absorption bandwidth is 7-8 GHz when the thickness is about 4 mm. When the thickness decreases to about 2 mm, the maximum absorption bandwidth is reduced by several times.
[0032] Here, after unremitting theoretical research and practical exploration, the inventor creatively combined carbonyl iron powder with aramid nanofibers to prepare porous aerogel, which not only achieved the lightweight application of carbonyl iron powder (the density of pure carbonyl iron powder is 1490mg / cm 3 , and the density of the composite aerogel of the present application is 25-60 mg / cm 3 ); moreover, since a large amount of electromagnetic waves enter the interior of the composite aerogel, multiple reflections can be increased, thereby obtaining a high-performance microwave absorbing material.
[0033] Even when the thickness is only 1.6mm, the microwave absorbing material has an effective absorption bandwidth of 11.2GHz for electromagnetic waves, which truly realizes that the absorbing material is light and thin while the absorbing performance can be further improved to above 10GHz, thereby expanding the application areas of absorbing materials, such as in aerospace, microwave darkrooms, electromagnetic protection and other aspects.
[0034] The effects of the present invention are as follows:
[0035] The present invention obtains a composite aerogel of aramid nanofibers and carbonyl iron powder by uniformly compounding aramid nanofibers and carbonyl iron powder, and applies it to the field of microwave absorption. It has the following advantages:
[0036] 1. The present invention can obtain aramid nanofibers by mixing aramid with a protonated solvent, dimethyl sulfoxide, and dispersing the mixture in an alkaline potassium hydroxide solution of a certain concentration, which is conducive to the fusion of aramid nanofibers with carbonyl iron powder to prepare porous aerogel.
[0037] 2. The present invention further obtains a dispersion containing both carbonyl iron powder and aramid nanofibers through ultrasonic liquid phase stripping technology.
[0038] 3. In the vacuum filtration technology adopted by the present invention, the organic microporous micromembrane used has a diameter of 0.45 μm. The filtration process ensures that the sample is cleaned and the sample will not be lost through the tiny micropores with alcohol or water.
[0039] 4. The prepared aramid nanofiber and carbonyl iron powder composite aerogel has an effective absorption of electromagnetic waves up to 11.2GHz when the thickness is only 1.6mm, and a maximum reflection loss of -42.6dB when the thickness is 2.4mm. This shows that the composite aerogel material can be used as a high-quality microwave absorbing material, which has a wide microwave absorption band, strong microwave absorption capacity, low density and low matching thickness, and can meet the high demand for absorbing materials in some special fields, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 This is a schematic diagram of the preparation process of Example 1;
[0041] Figure 2 is the XRD pattern of the composite material in Example 1;
[0042] Figure 3a is the reflection loss of the composite aerogel with a mass ratio of aramid nanofiber (ANF) to carbonyl iron powder (CIP) of 1:3 in Example 1;
[0043] Figure 3b is the reflection loss of the composite aerogel with a mass ratio of ANF to CIP of 1:5 in Example 2;
[0044] Figure 3c is the reflection loss of the composite aerogel with a mass ratio of ANF to CIP of 1:7 in Example 3;
[0045] Figure 4 This is a comparison chart of the microwave absorption performance of the composite aerogel prepared in Example 1 and related aerogel materials in the prior art. DETAILED DESCRIPTION
[0046] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0047] Embodiment 1:
[0048] This embodiment provides a composite material of aramid nanofiber and carbonyl iron powder, and the preparation method thereof is as follows: Figure 1 As shown, the specific steps include:
[0049] (1) 1.5 g of potassium hydroxide was first dissolved in 20 ml of water, and then 1 g of aramid (AF) and 480 ml of dimethyl sulfoxide were added. The mixture was stirred at room temperature for 4 h to obtain a dark red aramid nanofiber / dimethyl sulfoxide suspension (2 mg / mL).
[0050] (2) washing with alcohol and deionized water to obtain an aramid nanofiber aqueous solution by vacuum filtration;
[0051] (3) the aramid nanofibers and the carbonyl iron powder were uniformly mixed in a mass ratio of 1:3, 20 ml of alcohol was added, and liquid phase ultrasonic dissociation was performed for 1 hour, thereby obtaining a dispersion of the aramid nanofibers and the carbonyl iron powder uniformly mixed;
[0052] (4) The uniformly mixed suspension was taken and vacuum filtered using an organic microporous micromembrane with a diameter of 0.45 μm. After washing with deionized water, a composite aerogel in which aramid nanofibers and carbonyl iron powder were uniformly mixed was obtained after freeze-drying.
[0053] Example 2
[0054] This embodiment provides a composite material of aramid nanofiber and carbonyl iron powder, and the preparation method thereof is as follows: Figure 1 As shown, the specific steps include:
[0055] (1) 1.5 g potassium hydroxide was first dissolved in 20 ml water, and then 1 g aramid and 480 ml dimethyl sulfoxide were added. The mixture was stirred at room temperature for 4 h to obtain a dark red aramid nanofiber / dimethyl sulfoxide suspension (2 mg / mL).
[0056] (2) washing with deionized water to obtain an aramid nanofiber aqueous solution by vacuum filtration;
[0057] (3) the aramid nanofibers and the carbonyl iron powder were uniformly mixed in a mass ratio of 1:5, 20 ml of alcohol was added, and ultrasonic liquid phase dissociation was performed for 1 hour, thereby obtaining a dispersion of the aramid nanofibers and the carbonyl iron powder uniformly mixed;
[0058] (4) The uniformly mixed suspension was taken and vacuum filtered using an organic microporous micromembrane with a diameter of 0.45 μm. After washing with deionized water, a composite aerogel in which aramid nanofibers and carbonyl iron powder were uniformly mixed was obtained after freeze-drying.
[0059] Example 3
[0060] This embodiment provides a composite material of aramid nanofiber and carbonyl iron powder, and the preparation method thereof is as follows: Figure 1 As shown, the specific steps include:
[0061] (1) 1.5 g potassium hydroxide was first dissolved in 20 ml water, and then 1 g aramid and 480 ml dimethyl sulfoxide were added. The mixture was stirred at room temperature for 4 h to obtain a dark red aramid nanofiber / dimethyl sulfoxide suspension (2 mg / mL).
[0062] (2) washing with deionized water to obtain an aramid nanofiber aqueous solution by vacuum filtration;
[0063] (3) the aramid nanofibers and the carbonyl iron powder were uniformly mixed in a mass ratio of 1:7, 20 ml of alcohol was added, and ultrasonic liquid phase dissociation was performed for 1 hour, thereby obtaining a dispersion of the aramid nanofibers and the carbonyl iron powder uniformly mixed;
[0064] (4) The uniformly mixed suspension was taken and vacuum filtered using an organic microporous micromembrane with a diameter of 0.45 μm. After washing with deionized water, a composite aerogel in which aramid nanofibers and carbonyl iron powder were uniformly mixed was obtained after freeze-drying.
[0065] The materials prepared in Examples 1-3 were characterized and tested:
[0066] Material Characterization:
[0067] Figure 2 This is the XRD pattern of the composite material in Example 1. By comparing with the standard pdf card, the successful preparation of the aramid nanofiber and carbonyl iron powder composite aerogel is proved.
[0068] Wave absorption performance test:
[0069] The composite material prepared in the embodiment of the present invention was subjected to microwave absorption experiment:
[0070] The three groups of samples obtained in the embodiment are pressed into a ring shape, with an inner diameter of 3 mm and an outer diameter of 7 mm. The real part and imaginary part of the dielectric constant and the real part and imaginary part of the magnetic permeability of the material are measured by a vector network analyzer. Finally, the wave absorption performance of the material is calculated based on the electromagnetic parameters.
[0071] The results are as follows:
[0072] Figure 3a-3c This is the relationship between the reflection loss of the composite material and the microwave frequency and the thickness of the absorbing material:
[0073] Figure 3a When the mass ratio of ANF to CIP is 1:3 (the density of the composite aerogel material is 28.39 mg / cm 3 ), the reflection loss value of the sample at 2.6mm can reach -52.2dB, and an effective absorption bandwidth of 8.91GHz can be obtained at 1.6mm.
[0074] Figure 3b When the mass ratio of ANF to CIP is 1:5 (the density of the composite aerogel material is 43.54 mg / cm 3 ), when the thickness is only 1.6mm, the effective absorption of electromagnetic waves reaches 11.2GHz, and when the thickness is 2.4mm, the maximum reflection loss is -42.6dB at 5.78GHz.
[0075] Figure 3c When the mass ratio of ANF to CIP is 1:7 (the density of the composite aerogel material is 58.15 mg / cm 3 ), when the thickness is only 1.3mm, the effective absorption of electromagnetic waves reaches 5.1GHz, and when the thickness is 2.5mm, the maximum reflection loss is -43.2dB.
[0076] The microwave absorption performance of the composite aerogel material prepared in Example 2 of the present application was compared with some materials in the prior art (as shown in Table 1). Figure 4 As shown, this illustrates that the present invention has the advantages of "thinner thickness" and "stronger electromagnetic wave absorption capability".
[0077] Table 1. Aerogel microwave absorbing materials and their performance parameters in the prior art
[0078]
[0079]
[0080] In summary, the composite aerogel material provided by the present application, by creatively combining carbonyl iron powder with aramid nanofibers, not only realizes the lightweight application of carbonyl iron powder (the density of pure carbonyl iron powder is 1490 mg / cm 3 , and the density of the composite aerogel of the present application is 25-60 mg / cm 3 ); moreover, since a large amount of electromagnetic waves enter the interior of the composite aerogel, multiple reflections can be increased, thereby obtaining a high-performance microwave absorbing material. This microwave absorbing material, even when the thickness is only 1.6mm, has an effective absorption bandwidth of 11.2GHz for electromagnetic waves, truly realizing that the absorbing material is light and thin, and the absorbing performance can be further improved to more than 10GHz, which can meet the high demand for absorbing materials in certain special fields, thereby expanding the application field of absorbing materials, and has a very practical progressive significance.
[0081] The embodiments described above are only descriptions of the preferred implementation modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for preparing a composite aerogel of aramid nanofibers and carbonyl iron powder, characterized in that: It includes: Dispersing aramid and dimethyl sulfoxide in a potassium hydroxide solution with a concentration of 2-5 mg / ml, stirring at room temperature for 3-5 hours, vacuum filtering and washing to obtain aramid nanofibers; The aramid nanofibers and carbonyl iron powder are dispersed in an ethanol solution at a mass ratio of 1:3-7, and ultrasonic liquid phase stripping is performed for 0.5-2 hours. After vacuum filtration, a composite hydrogel of aramid nanofibers and carbonyl iron powder is obtained; freeze-drying the aramid nanofiber and carbonyl iron powder composite hydrogel under vacuum conditions to obtain the aramid nanofiber and carbonyl iron powder composite aerogel; When the mass ratio of aramid nanofibers to carbonyl iron powder is 1:3, the density of the composite aerogel is 28.39 mg / cm 3 , the reflection loss value reaches -52.2dB, and the effective absorption bandwidth is 8.91GHz; When the mass ratio of aramid nanofibers to carbonyl iron powder is 1:5, the density of the composite aerogel is 43.54 mg / cm 3 , an effective absorption bandwidth of 11.2 GHz is obtained, and the maximum reflection loss is -42.6 dB; When the mass ratio of aramid nanofibers to carbonyl iron powder is 1:7, the density of the composite aerogel is 58.15 mg / cm 3 , an effective absorption bandwidth of 5.1 GHz is obtained, and the maximum reflection loss is -43.2 dB.
2. The method for preparing the composite aerogel of aramid nanofiber and carbonyl iron powder according to claim 1, characterized in that: The mass volume ratio of the aramid fiber to the dimethyl sulfoxide is 1g:450-500ml.
3. The method for preparing the composite aerogel of aramid nanofiber and carbonyl iron powder according to claim 1, characterized in that: The ultrasonic power in the ultrasonic liquid phase stripping is 500-700w.
4. The method for preparing the composite aerogel of aramid nanofiber and carbonyl iron powder according to claim 1, characterized in that: The ethanol solution is an ethanol-water solution with a volume fraction of 60-90%.
5. The method for preparing the composite aerogel of aramid nanofiber and carbonyl iron powder according to claim 1, characterized in that: In the vacuum filtration step, an organic microporous micromembrane with a diameter of 0.45 μm is used.
6. A composite aerogel of aramid nanofiber and carbonyl iron powder, characterized in that: The compound is prepared by the preparation method as described in any one of claims 1 to 5.
7. A microwave absorbing material, characterized in that: It contains the composite aerogel of aramid nanofiber and carbonyl iron powder as claimed in claim 6.
8. The microwave absorbing material according to claim 7, characterized in that: When the thickness of the aramid nanofiber and carbonyl iron powder composite aerogel is 1.6 mm, the effective absorption bandwidth of electromagnetic waves reaches 11.2 GHz, and the maximum reflection loss is -14.7 dB; When the thickness is 2.4mm, the effective absorption bandwidth of electromagnetic waves reaches 3.63GHz, and the maximum reflection loss is -42.6dB.