Low shrinkage ultra-high performance concrete based on staged regulation and preparation method
By using CaO and CSA expansion agents and internal curing agents and plant fibers in ultra-high performance concrete, the debonding and cracking problems caused by self-contraction are solved, and the low shrinkage characteristics and efficient shrinkage control are achieved. For large-scale paving and infrastructure restoration.
Patent Information
- Application Number
- CN202310660681.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-02
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-06-02
AI Technical Summary
Due to the debonding or cracking caused by self-shrinkage during the repair process of ultra-high performance concrete, the single mechanism of action of the existing technology is difficult to effectively regulate the early shrinkage and the window of shrinkage, resulting in difficulty in controlling shrinkage.
Using a phased regulation method of expansion agents, internal curing agents and plant fibers including CaO and CSA, early reduction is achieved through the synergistic effect of CaO and internal curing agents, the continuous expansion of CSA and the physical constraints of plant fibers, and the synchronous control of ultra-high The shrinkage window period of performance concrete.
It effectively reduces the early shrinkage rate and long-term shrinkage value of ultra-high performance concrete, reduces the risk of cracking in the repair interface, and is suitable for large-area paving and the construction and life extension of major infrastructure.
Smart Images

Figure CN116675493B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of concrete materials, and in particular to low-shrinkage ultra-high performance concrete based on staged regulation and control and a preparation method thereof. Background Art
[0002] The statements in this section merely provide background information related to the present invention and do not necessarily constitute prior art.
[0003] Ultra-high performance concrete (UHPC) has ultra-high mechanical properties, toughness and excellent durability. UHPC is made of cement, water, filler, fine aggregate, silica fume and high-efficiency water reducer. In addition, the addition of fiber significantly improves the tensile, flexural and shear strength of UHPC, but the compressive strength may remain unchanged or slightly increase; UHPC is prepared at a lower water-cement ratio (about 0.2). The excellent mechanical properties and durability of UHPC give it a high potential to improve the durability of infrastructure and solve the problem of "repeated" repairs. Using UHPC to repair damaged concrete structures can not only enhance the bearing capacity, but also reduce the erosion of concrete by harmful media. In the splash zone of bridge piers and dams, ordinary concrete piers wrapped with UHPC repair materials can significantly improve the scour resistance of bridge piers. At present, domestic and foreign attempts to use UHPC to repair hydraulic concrete structures to solve the problem of threatening the safe service of hydraulic concrete structures due to insufficient mechanics or durability.
[0004] UHPC has a low water-binder ratio and a relatively low free water content inside, which is insufficient for the cement to be fully hydrated. As the hydration progresses, the free water content decreases, and the water in a large number of capillaries changes from a saturated state to an unsaturated state. The capillaries generate negative pressure that acts on the cement stone, causing shrinkage. In addition, the use of a high amount of silica fume in UHPC will also increase autogenous shrinkage. Silica fume can refine the pore size and increase the negative pressure of the capillaries. In addition, the volcanic ash reaction of silica fume will also promote the autogenous shrinkage of concrete.
[0005] The shrinkage of UHPC has a great impact on the repair interface, especially when UHPC is used as a repair material for large-scale paving. The stress generated by shrinkage may cause debonding of the repair interface or cracking of the repair material. Therefore, the shrinkage research of UHPC is particularly important. Traditional UHPC shrinkage reduction technology is mostly a single mechanism, such as controlling the hydration of cementitious materials, reducing capillary tension and physical constraints, and the shrinkage window period of this single mechanism is limited. The shrinkage of UHPC is a continuous process, and the shrinkage occurrence period and the shrinkage window period are not synchronized, which easily leads to the difficulty of shrinkage regulation and the phenomenon that early shrinkage is still large. Summary of the invention
[0006] In order to solve the above problems, the present invention proposes a low-shrinkage ultra-high performance concrete based on staged regulation and a preparation method. By adding expansion agents including CaO and CSA, internal curing agents and plant fibers, staged regulation of the early shrinkage of high-performance concrete is achieved to obtain low-shrinkage ultra-high performance concrete.
[0007] To achieve the above object, the present invention adopts the following technical solution:
[0008] First, a low-shrinkage ultra-high performance concrete based on phased regulation is proposed, including water, cement, silica fume, sand, steel fiber, expansive agent, plant fiber, internal curing agent and water reducing agent, and the expansive agent includes CaO and CSA.
[0009] Secondly, a method for preparing low shrinkage ultra-high performance concrete based on staged regulation is proposed, including:
[0010] Mix cement, silica fume and sand to obtain dry material;
[0011] adding water and a water reducing agent to the dry material and stirring to obtain a mixture;
[0012] adding plant fiber to the mixture and stirring to obtain a mixture with plant fiber;
[0013] adding steel fiber to the mixture with plant fiber and stirring to obtain a mixture with steel fiber;
[0014] adding an expansion agent to the mixture with steel fibers and stirring the mixture to obtain a mixture with the expansion agent;
[0015] An internal curing agent is added to the mixture with the expansion agent and stirred to obtain low shrinkage ultra-high performance concrete.
[0016] On the third aspect, the application of the above-mentioned low shrinkage ultra-high performance concrete based on phased control in the field of road and bridge engineering is proposed.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] The expansion agent of the present invention comprises CaO and CSA, the action window time of the CaO expansion agent is 24h, the action window time of the CSA expansion agent is 3d, CaO reacts with water to generate Ca(OH)2, the apparent volume expands, the expansion product of CSA is calcium sulfate, based on the early shrinkage characteristics of ultra-high performance concrete, CaO and internal curing agent are selected to synergistically realize early shrinkage reduction, realize the unification of the CaO expansion agent window and the internal curing agent water release window, realize the synchronization of the shrinkage window period of ultra-high performance concrete, the early expansion of the CSA expansion agent needs to consume more water to show the expansion effect, and the duration is longer, the cavity plant fiber is used to release the cavity free water, and the CSA is assisted to play the expansion effect, the expansion effect compensates for the shrinkage caused by the capillary negative pressure caused by the early water loss, and the whole presents expansion, after the age exceeds 3d, the early shrinkage of the ultra-high performance concrete accounts for more than half of the 28d shrinkage, and the early shrinkage rate is relatively high, the shrinkage control after 3d relies on physical constraint regulation, and the plant fiber and steel fiber after the free water are released have a shrinkage constraint effect to achieve efficient shrinkage reduction.
[0019] Advantages of additional aspects of the present invention will be given in part in the following description, and in part will become obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The drawings in the specification, which constitute a part of the present application, are used to provide further understanding of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute improper limitations on the present application.
[0021] Figure 1 This is the result of monitoring the long-term shrinkage performance of concrete;
[0022] Figure 2 This is the microscopic observation diagram of internal curing of ZH1 group ultra-high performance concrete;
[0023] Figure 3 This is the microscopic observation picture of ettringite in ZH1 ultra-high performance concrete;
[0024] Figure 4 This is the microscopic observation picture of the cement matrix of the ZH1 group ultra-high performance concrete;
[0025] Figure 5 This is the microscopic observation picture of cellulose fibers in ultra-high performance concrete of group ZH1;
[0026] Figure 6 Schematic diagram of regulating UHPC shrinkage in stages. DETAILED DESCRIPTION
[0027] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.
[0028] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.
[0029] As introduced in the background technology, in the prior art, UHPC shrinkage technology is mostly a single action mechanism, and the shrinkage window period of the single action mechanism is limited. The shrinkage of UHPC is a continuous process, which makes the shrinkage occurrence period and the shrinkage window period not synchronized, which easily leads to difficulty in shrinkage regulation, and early shrinkage is still a big problem.
[0030] In view of this, in a specific embodiment of the present invention, a low shrinkage ultra-high performance concrete based on staged regulation is provided, including water, cement, silica fume, sand, steel fiber, an expansive agent, plant fiber, an internal curing agent and a water reducing agent, wherein the expansive agent includes calcium oxide (CaO) and calcium sulfoaluminate (CSA).
[0031] In some embodiments of this implementation mode, the low shrinkage ultra-high performance concrete based on staged regulation includes, by weight: 156-240 parts of water, 800-920 parts of cement, 150-280 parts of silica fume, 800-1200 parts of sand, 126-160 parts of steel fiber, 72-120 parts of expansion agent, 1-13 parts of plant fiber, 100-200 parts of internal curing agent and 20-36 parts of water reducer.
[0032] In some examples of this embodiment, the expansion agent includes CaO and CSA; the weight ratio of CaO to CSA in the expansion agent is 0.5 to 0.75.
[0033] In some examples of this embodiment, the water is tap water or deionized water.
[0034] In some examples of this embodiment, the cement is ordinary Portland cement.
[0035] In some examples of this embodiment, the sand is river sand or quartz sand.
[0036] In some examples of this embodiment, the steel fiber is a straight, hook-ended or wavy steel fiber with a tensile strength of 2800-2900 MPa, a length of 12-14 mm, and a diameter of 0.15-0.25 mm.
[0037] In some examples of this embodiment, the plant fiber is a plant fiber with a hollow structure, such as cellulose fiber or sisal fiber, and has a diameter less than 0.1 mm.
[0038] In some examples of this implementation mode, the internal curing agent is pottery sand or waste bricks with a rich cavity structure, the internal curing agent is pre-absorbed with water for more than 24 hours, and the porosity is greater than 10%.
[0039] In some examples of this embodiment, the water reducing agent is a polycarboxylate water reducing agent, the water reducing efficiency is more than 30%, and the solid content is close to 40%.
[0040] The early shrinkage mechanism of low shrinkage ultra-high performance concrete based on staged regulation proposed in the present invention is: the expansion agent includes CaO and CSA, CaO and CSA can be used as expansion agents, the CaO expansion agent action window time is 24h, the CSA expansion agent action window time is 3d, CaO reacts with water to generate Ca(OH)2, the apparent volume expands, and the expansion product of CSA is calcium aluminate. Based on the early shrinkage characteristics of ultra-high performance concrete, CaO and internal curing agent are selected to work together to achieve early shrinkage reduction, and the CaO expansion agent window and the internal curing agent water release window are unified to achieve ultra-high performance concrete. The shrinkage window period of the concrete can be synchronized. The early expansion of CSA expansive agent consumes more water to show the expansion effect, which lasts for a long time. The cavity plant fiber is used to release the cavity free water to assist CSA to play the expansion effect. The expansion effect compensates for the shrinkage caused by the capillary negative pressure caused by the early water loss. The overall expansion is presented. After the age exceeds 3d, the early shrinkage of ultra-high performance concrete accounts for more than half of the 28d shrinkage, and the early shrinkage rate is high. The shrinkage control after 3d relies on physical constraint regulation. The plant fiber and steel fiber after releasing free water have a shrinkage constraint effect to achieve efficient shrinkage reduction, such as Figure 6 shown.
[0041] The present invention uses a variety of regulatory mechanisms to regulate concrete in stages in sequence through internal compensation, delaying the decline of internal humidity, reducing capillary negative pressure and physical constraints, effectively reducing the autogenous shrinkage of ultra-high performance concrete in the first 3 days, and greatly reducing the shrinkage of ultra-high performance concrete in the long term; the UHPC autogenous shrinkage value of the present invention is relatively small, with an autogenous shrinkage of 0 μm / m in 3 days, or even slight expansion, an autogenous shrinkage of less than 190 μm / m in 7 days, and an autogenous shrinkage of less than 240 μm / m in 28 days; different from the window period using a single mechanism, the present invention uses a variety of shrinkage reduction mechanisms to work in synergy, achieving the whole process of shrinkage reduction and ultra-high performance concrete body shrinkage in the same window, thereby efficiently regulating the early shrinkage of ultra-high performance concrete.
[0042] The ultra-high performance concrete of the present invention has the characteristic of low shrinkage, which can effectively reduce the risk of cracking caused by large-area paving and repair of ultra-high performance concrete, and can be used for the construction and life extension of various major infrastructures with the goal of serving for a hundred years, such as dam spillways and submarine tunnel joints.
[0043] In a specific embodiment of the present invention, a method for preparing the above-mentioned low shrinkage ultra-high performance concrete based on staged regulation is also provided, comprising:
[0044] Mix cement, silica fume and sand to obtain dry material;
[0045] adding water and a water reducing agent to the dry material and stirring to obtain a mixture;
[0046] adding plant fiber to the mixture and stirring to obtain a mixture with plant fiber;
[0047] adding steel fiber to the mixture with plant fiber and stirring to obtain a mixture with steel fiber;
[0048] adding an expansion agent to the mixture with steel fibers and stirring the mixture to obtain a mixture with the expansion agent;
[0049] An internal curing agent is added to the mixture with the expansion agent and stirred to obtain low shrinkage ultra-high performance concrete.
[0050] In some examples of this implementation mode, cement, silica fume and sand are mixed and stirred for 3 minutes to obtain dry material; water and water reducing agent are added to the dry material and stirred for 5 minutes to obtain a mixture; plant fiber is added to the mixture and stirred for 3 minutes to obtain a mixture with plant fiber; steel fiber is added to the mixture with plant fiber and stirred for 3 minutes to obtain a mixture with steel fiber; an expansion agent is added to the mixture with steel fiber and stirred for 3 minutes to obtain a mixture with an expansion agent; an internal curing agent is added to the mixture with the expansion agent and stirred for 3 minutes to obtain low shrinkage ultra-high performance concrete.
[0051] In a specific embodiment of the present invention, there is also provided application of the above-mentioned low shrinkage ultra-high performance concrete based on staged regulation in the field of road and bridge engineering.
[0052] Example 1
[0053] This embodiment discloses a low shrinkage ultra-high performance concrete based on staged regulation, comprising: 800.4 parts of cement, 276 parts of silica fume, 860.2 parts of sand, 156 parts of steel fiber, 220.2 parts of water, 22 parts of water reducer, 151.8 parts of internal curing agent, 119.6 parts of expansion agent and 3.4 parts of plant fiber. The concrete is named ZH1 group.
[0054] Among them, cement is ordinary Portland cement.
[0055] The water is tap water.
[0056] The sand is river sand.
[0057] The expansion agent is a composite of CaO and CSA, and the ratio between the two is 0.7.
[0058] The internal curing agent is ceramic sand with a rich cavity structure. The internal curing agent has been pre-absorbed with water for more than 24 hours and has a porosity of more than 10%.
[0059] Plant fibers are cellulose fibers with a hollow structure and a diameter of less than 0.1 mm.
[0060] The steel fiber is a straight steel fiber with a tensile strength of 2850 MPa, a length of 13 mm and a diameter of 0.2 mm.
[0061] The water reducer is a polycarboxylic acid water reducer with a water reduction efficiency of more than 30% and a solid content of nearly 40%.
[0062] The preparation method of concrete in this embodiment is: pre-mix cement, silica fume and sand and stir for 3 minutes, then add water and water reducing agent and stir for 5 minutes, then add cellulose fiber and stir for 3 minutes, then add steel fiber and stir for 3 minutes, then add expansion agent and stir for 3 minutes, and finally add pottery sand and stir for 2 minutes to obtain the low shrinkage ultra-high performance concrete based on staged regulation disclosed in this embodiment.
[0063] Example 2
[0064] This embodiment discloses a low shrinkage ultra-high performance concrete based on staged regulation, including: 848 parts of cement, 276 parts of silica fume, 911.8 parts of sand, 156 parts of steel fiber, 220.2 parts of water, 20 parts of water reducer, 100 parts of internal curing agent, 72 parts of expansion agent and 1 part of plant fiber. The concrete is named ZH2 group.
[0065] Among them, cement is ordinary Portland cement.
[0066] The water is deionized water.
[0067] The sand is quartz sand.
[0068] The expansion agent is a composite of CaO and CSA, and the ratio between the two is 0.5.
[0069] The internal curing agent is waste bricks with rich cavity structure. The internal curing agent has been pre-absorbed with water for more than 24 hours and has a porosity of more than 10%.
[0070] The plant fiber is sisal fiber with a hollow structure and a diameter of less than 0.1 mm.
[0071] The steel fiber is an end hook steel fiber with a tensile strength of 2850 MPa, a length of 13 mm and a diameter of 0.2 mm.
[0072] The water reducer is a polycarboxylic acid water reducer with a water reduction efficiency of more than 30% and a solid content of nearly 40%.
[0073] The preparation method of concrete in this embodiment is: pre-mix cement, silica fume and sand and stir for 3 minutes, then add water and water reducing agent and stir for 5 minutes, then add sisal fiber and stir for 3 minutes, then add steel fiber and stir for 3 minutes, then add expansion agent and stir for 3 minutes, and finally add waste bricks and stir for 2 minutes to obtain the low shrinkage ultra-high performance concrete based on staged regulation disclosed in this embodiment.
[0074] Example 3
[0075] This embodiment discloses a low shrinkage ultra-high performance concrete based on staged regulation, including: 810.4 parts of cement, 276 parts of silica fume, 810.2 parts of sand, 160 parts of steel fiber, 220.2 parts of water, 24 parts of water reducer, 200 parts of internal curing agent, 120 parts of expansion agent and 13 parts of plant fiber. The concrete is named ZH3 group.
[0076] Among them, cement is ordinary Portland cement.
[0077] The water is tap water.
[0078] The sand is quartz sand.
[0079] The expansion agent is a composite of CaO and CSA, and the ratio between the two is 0.75.
[0080] The internal curing agent is ceramic sand with a rich cavity structure. The internal curing agent has been pre-absorbed with water for more than 24 hours and has a porosity of more than 10%.
[0081] Plant fibers are cellulose fibers with a hollow structure and a diameter of less than 0.1 mm.
[0082] The steel fiber is a corrugated steel fiber with a tensile strength of 2850 MPa, a length of 13 mm and a diameter of 0.2 mm.
[0083] The water reducer is a polycarboxylic acid water reducer with a water reduction efficiency of more than 30% and a solid content of nearly 40%.
[0084] The preparation method of concrete in this embodiment is: pre-mix cement, silica fume and sand and stir for 3 minutes, then add water and water reducing agent and stir for 5 minutes, then add cellulose fiber and stir for 3 minutes, then add steel fiber and stir for 3 minutes, then add expansion agent and stir for 3 minutes, and finally add pottery sand and stir for 2 minutes to obtain the low shrinkage ultra-high performance concrete based on staged regulation disclosed in this embodiment.
[0085] Experimental Group 1
[0086] The experimental group is the basic group 0. The concrete of group 0 includes, by mass, 800.4 parts of cement, 276 parts of silica fume, 860.2 parts of sand, 156 parts of steel fiber, 220.2 parts of water and 20 parts of water reducing agent.
[0087] Among them, cement is ordinary Portland cement.
[0088] The water is tap water.
[0089] The sand is river sand.
[0090] The steel fiber is a straight steel fiber with a tensile strength of 2850 MPa, a length of 13 mm and a diameter of 0.2 mm.
[0091] The water reducer is a polycarboxylic acid water reducer with a water reduction efficiency of more than 30% and a solid content of nearly 40%.
[0092] The preparation method of the concrete is: pre-mixing cement, silica fume and sand for 3 minutes, then adding water and a water reducing agent and stirring for 5 minutes, and finally adding steel fiber and stirring for 3 minutes to obtain the concrete of this experimental group.
[0093] Experimental Group 2
[0094] The experimental group is group T. The concrete of group T, calculated by mass, includes: 800.4 parts of cement, 276 parts of silica fume, 860.2 parts of sand, 156 parts of steel fiber, 220.2 parts of water, 23 parts of water reducer and 151.8 parts of internal curing agent.
[0095] Among them, cement is ordinary Portland cement.
[0096] The water is tap water.
[0097] The sand is river sand.
[0098] The internal curing agent is ceramic sand with a rich cavity structure. The internal curing agent has been pre-absorbed with water for more than 24 hours and has a porosity of more than 10%.
[0099] The steel fiber is a straight steel fiber with a tensile strength of 2850 MPa, a length of 13 mm and a diameter of 0.2 mm.
[0100] The water reducer is a polycarboxylic acid water reducer with a water reduction efficiency of more than 30% and a solid content of nearly 40%.
[0101] The preparation method of concrete in this embodiment is: pre-mix cement, silica fume and sand and stir for 3 minutes, then add water and water reducing agent and stir for 5 minutes, then add steel fiber and stir for 3 minutes, and finally add pottery sand and stir for 2 minutes to obtain the concrete of this experimental group.
[0102] Experimental Group 3
[0103] The experimental group is Group P. The concrete of Group P includes: 800.4 parts of cement, 276 parts of silica fume, 860.2 parts of sand, 156 parts of steel fiber, 220.2 parts of water, 20 parts of water reducing agent and 119.6 parts of expansion agent.
[0104] Among them, cement is ordinary Portland cement.
[0105] The water is tap water.
[0106] The sand is river sand.
[0107] The expansion agent is a composite of CaO and CSA, and the ratio between the two is between 0.5 and 0.75.
[0108] The steel fiber is a straight steel fiber with a tensile strength of 2850 MPa, a length of 13 mm and a diameter of 0.2 mm.
[0109] The water reducer is a polycarboxylic acid water reducer with a water reduction efficiency of more than 30% and a solid content of nearly 40%.
[0110] The preparation method of concrete in this embodiment is: pre-mix cement, silica fume and sand and stir for 3 minutes, then add water and water reducing agent and stir for 5 minutes, then add steel fiber and stir for 3 minutes, and then add expansion agent and stir for 3 minutes to obtain the low shrinkage ultra-high performance concrete based on staged regulation of this experimental group.
[0111] The long-term shrinkage performance of concrete in Example 1, Example 2, Example 3, Experimental Group 1, Experimental Group 2 and Experimental Group 3 was monitored. The monitored shrinkage results are as follows: Figure 1 As shown, when the contraction value is negative, it is expansion, and when the contraction value is positive, it is contraction. Figure 1 It can be seen that the shrinkage value in the first three days of shrinkage control by only a single mechanism is reduced, such as the T and P groups. The shrinkage control in the first three days of multiple mechanisms in stages is obvious, tending to be slightly expanded, such as the ZH group. Through long-term monitoring, it was found that the shrinkage of unregulated ultra-high performance concrete exceeded 700μm / m. If the shrinkage is not regulated, it will crack when used for bridge joints or bridge deck paving. After the coordinated action of multiple mechanisms in stages in the ZH group, the shrinkage of ultra-high performance concrete was reduced to below 240μm / m, effectively reducing the risk of cracking after bridge deck repair and paving.
[0112] The ZH1 group of ultra-high performance concrete was subjected to microscopic observation and analysis. The results are as follows Figure 2-Figure 5 As shown in the figure, it is observed that the water release of ceramic sand alleviates the decrease in humidity inside the ultra-high performance concrete. The interface between ceramic sand aggregate and cement stone is dense, without obvious interface transition zone, and hydration products are generated in the pores of ceramic sand, which proves that ceramic sand and cement matrix form a good combination. Figure 2 and Figure 3 The picture shows that the pore wall of ultra-high performance concrete is covered with calcium aluminate. Figure 4 Because there is a lot of strong calcium oxide in the cement matrix, volume expansion can effectively reduce shrinkage. Figure 5After the cellulose fiber cavity structure releases water, its volume shrinks, and the cement matrix around the fiber is maintained dense. The water released by the cellulose fiber alleviates the decrease in humidity inside the ultra-high performance concrete, provides a water source for the CSA reaction, and can assist CSA in exerting its effect. In addition, the constraint of the fiber on the deformation of the matrix is also beneficial to reducing the shrinkage of ultra-high performance concrete, thus illustrating the feasibility of the synergistic effect of multiple mechanisms and the stage-by-stage regulation of the shrinkage of ultra-high performance concrete.
[0113] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.
Claims
1. Low shrinkage ultra-high performance concrete based on staged regulation, characterized in that: It is composed of water, cement, silica fume, sand, steel fiber, expansion agent, plant fiber, internal curing agent and water reducing agent. The expansion agent is composed of CaO and CSA. By mass, water 156-240 parts, cement 800-920 parts, silica fume 150-280 parts, sand 800-1200 parts, steel fiber 126-160 parts, expansion agent 72-120 parts, plant fiber 1-13 parts, internal curing agent 100-200 parts and water reducing agent 20-36 parts; The weight ratio of CaO to CSA in the expansion agent is 0.5~0.75; Plant fibers are plant fibers with a hollow structure; The internal curing agent is ceramic sand or waste bricks with rich cavity structure, the internal curing agent has been pre-absorbed for more than 24 hours, and the porosity is greater than 10%; The low shrinkage ultra-high performance concrete based on staged regulation is prepared by the following preparation method: Mix cement, silica fume and sand according to proportion to obtain dry material; adding water and a water reducing agent to the dry material and stirring to obtain a mixture; adding plant fiber to the mixture and stirring to obtain a mixture with plant fiber; adding steel fiber to the mixture with plant fiber and stirring to obtain a mixture with steel fiber; adding an expansion agent to the mixture with steel fibers and stirring the mixture to obtain a mixture with the expansion agent; An internal curing agent is added to the mixture with the expansion agent and stirred to obtain low shrinkage ultra-high performance concrete.
2. The low shrinkage ultra-high performance concrete based on staged regulation according to claim 1, characterized in that: The steel fibers are straight, hooked or wavy.
3. The low shrinkage ultra-high performance concrete based on staged regulation according to claim 1, characterized in that: The water reducing agent is a polycarboxylic acid water reducing agent.
4. The method for preparing low shrinkage ultra-high performance concrete based on staged regulation according to any one of claims 1 to 3, comprising: Mix cement, silica fume and sand according to proportion to obtain dry material; adding water and a water reducing agent to the dry material and stirring to obtain a mixture; adding plant fiber to the mixture and stirring to obtain a mixture with plant fiber; adding steel fiber to the mixture with plant fiber and stirring to obtain a mixture with steel fiber; adding an expansion agent to the mixture with steel fibers and stirring the mixture to obtain a mixture with the expansion agent; An internal curing agent is added to the mixture with the expansion agent and stirred to obtain low shrinkage ultra-high performance concrete.
5. Application of the low shrinkage ultra-high performance concrete based on staged regulation according to any one of claims 1 to 3 and / or the low shrinkage ultra-high performance concrete obtained by the preparation method of claim 4 in the field of road and bridge engineering.