Method for modifying lignin with sodium borohydride, and method for preparing cellulose composite membrane
Through the combination of sodium borohydride modified lignin and nanocellulose, the problem of poor film formation toughness of traditional lignin and cellulose is solved, the mechanical properties and biodegradability of cellulose films are improved, and the low-carbon cycle and cost are achieved Reduced effect.
Patent Information
- Application Number
- CN202310773617.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-28
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-06-28
Smart Images

Figure CN116693879B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cellulose membranes, and in particular to a method for modifying lignin with sodium borohydride and a method for preparing a cellulose composite membrane. Background Art
[0002] Traditional polyethylene materials are difficult to degrade in the environment and cause great harm to the environment. Biodegradable polymers will replace fossil-based polymers as they are less harmful to the environment. Lignin and cellulose come from plants and have aroused great interest because of their biodegradability, non-toxicity, biocompatibility and relatively low cost. However, the tensile toughness of the direct combination of cellulose and lignin is poor and does not meet the practical application conditions, which to a certain extent restricts its comprehensive application in the field of life.
[0003] Based on the structure of traditional wood, lignin acts as a cellulose adhesive that gives wood solid strength. Under experimental conditions, the direct film strength of lignin and cellulose is very low, and there are few hydrogen bonds between them. The produced film has no practical application conditions.
[0004] Based on the current defects of directly forming films from lignin and cellulose, it is necessary to improve this. Summary of the invention
[0005] In view of this, the present invention provides a method for modifying lignin with sodium borohydride and a method for preparing a cellulose composite membrane to solve the defects in the prior art.
[0006] In a first aspect, the present invention provides a method for modifying lignin with sodium borohydride, comprising the following steps:
[0007] adding lignin into an alcohol solvent to obtain a lignin solution;
[0008] adding sodium silicate to the lignin solution to obtain a mixed solution;
[0009] The pH of the mixed solution is adjusted to 10-13, and then sodium borohydride is added. After the reaction, the solution is filtered and dried to obtain modified lignin.
[0010] Preferably, in the method of modifying lignin with sodium borohydride, the lignin includes alkali lignin and / or ethanol lignin;
[0011] The alcohol solvent includes at least one of ethanol, methanol and glycerol.
[0012] Preferably, in the method of modifying lignin with sodium borohydride, the mass ratio of lignin, alcohol solvent, sodium silicate and sodium borohydride is (0.25-1):(10-20):(0.5-2):(0.25-1).
[0013] Preferably, the method for modifying lignin with sodium borohydride and the method for preparing ethanol lignin comprise the following steps:
[0014] Crush the straw and dry it;
[0015] The dried straw is placed in a reactor and an ethanol aqueous solution is added;
[0016] Pass oxygen into the reactor, and after the air above the material is completely replaced by oxygen, seal the reactor and keep passing oxygen; heat to 70-90°C; keep warm for 2-3 hours to react; keep passing oxygen during the reaction, and when the pressure in the reactor reaches 0.8-1.3MPa, the pressure in the reactor is balanced with the pressure at the air inlet pipe, and oxygen no longer enters the reactor;
[0017] After the reaction is completed, the pressure is released and filtered to separate the straw from the liquid;
[0018] Distilling the liquid to remove ethanol and obtain a lignin mixture;
[0019] The lignin mixture is hydrolyzed with sulfuric acid to cause the lignin to flocculate and precipitate, and then centrifuged. The lower precipitate is freeze-dried to obtain lignin, which is ethanol lignin.
[0020] Preferably, in the method of modifying lignin with sodium borohydride, the pH of the mixed solution is adjusted to 10-13, sodium borohydride is added, reacted at 20-30° C. for 1-7 minutes, and then dried to obtain modified lignin.
[0021] In a second aspect, the present invention also provides a modified lignin obtained by the treatment method.
[0022] In a third aspect, the present invention further provides a method for preparing a cellulose composite film, comprising the following steps:
[0023] adding nanocellulose to water to obtain a cellulose solution;
[0024] adding the modified lignin to a cellulose solution to obtain a film-forming solution;
[0025] The film-forming liquid is poured into a mold and solidified to obtain a cellulose composite film.
[0026] Preferably, in the method for preparing the cellulose composite membrane, the mass concentration of the cellulose solution is 0.5-2%.
[0027] Preferably, in the method for preparing the cellulose composite membrane, the mass of the modified lignin is 10-30% of the mass of the nanocellulose.
[0028] Preferably, in the method for preparing the cellulose composite membrane, the membrane-forming liquid is poured into a mold and cured at room temperature for 60 to 80 hours to obtain the cellulose composite membrane.
[0029] The method for modifying lignin with sodium borohydride and the method for preparing a cellulose composite film of the present invention have the following beneficial effects compared with the prior art:
[0030] 1. The method of modifying lignin with sodium borohydride of the present invention is to reduce and modify lignin with sodium borohydride in an alkaline alcohol system. The sodium borohydride reduction efficiency is higher in the alcohol system. At the same time, sodium silicate is used as a reaction catalyst to shorten the reaction time to 3 minutes, thereby improving the utilization rate of sodium borohydride and increasing the hydroxyl content in lignin, so that more hydrogen bonds are generated between lignin and cellulose, thereby improving the mechanical properties of the membrane itself. At the same time, the raw materials used come from crop straw, which is itself a clean energy source, and the cost of production is low, thus realizing a low-carbon cycle;
[0031] 2. The preparation method of the cellulose composite film of the present invention modifies the alkali / ethanol lignin by sodium borohydride to increase the hydrogen bond between cellulose, and at the same time, the lignin can give the composite film good anti-ultraviolet, antioxidant and antibacterial properties; the nanocellulose (CNF) and alkali / ethanol lignin composite film can be fully biodegradable. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the prior art descriptions. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0033] Figure 1 is a graph showing the hydroxyl content of the modified lignin prepared in Examples 1 to 4;
[0034] Figure 2 is a graph showing the hydroxyl content of the modified lignin prepared in Examples 1, 5 to 6;
[0035] Figure 3 is a graph showing the hydroxyl content of the modified lignin prepared in Examples 7 to 10;
[0036] Figure 4 is a graph showing the hydroxyl content of the modified lignin prepared in Examples 7, 11-12;
[0037] Figure 5 The macroscopic photographs of the cellulose films prepared in Comparative Example 2 when the mass of lignin is 10%, 20%, and 30% of the mass of nanocellulose (CNF) respectively;
[0038] Figure 6 This is a macroscopic photograph of the cellulose composite film prepared when the mass of the modified alkali lignin in Example 13 is 10%, 20%, and 30% of the mass of the nanocellulose (CNF) (from left to right in the figure, 10%, 20%, and 30%, respectively);
[0039] Figure 7 Graphs showing stress-strain curves of the cellulose film prepared in Comparative Example 1, the cellulose composite film prepared in Example 13, and the cellulose film prepared in Comparative Example 2;
[0040] Figure 8 These are stress-strain curves of the cellulose film prepared in Comparative Example 1, the cellulose composite film prepared in Example 14, and the cellulose film prepared in Comparative Example 3. DETAILED DESCRIPTION
[0041] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] It should be noted that the order of description of the following embodiments is not intended to limit the preferred order of the embodiments. In addition, in the description of the present application, the term "including" means "including but not limited to". Various embodiments of the present invention may be in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity and should not be understood as a rigid limitation on the scope of the present invention; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values within the range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the numbered ranges, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated in this article, it is meant to include any cited numbers (fractions or integers) within the indicated range.
[0043] The present application embodiment provides a method for modifying lignin with sodium borohydride, comprising the following steps:
[0044] S1, adding lignin to an alcohol solvent to obtain a lignin solution;
[0045] S2, adding sodium silicate to the lignin solution to obtain a mixed solution;
[0046] S3, adjusting the pH of the mixed solution to 10-13, then adding sodium borohydride, filtering after the reaction, and drying to obtain modified lignin.
[0047] It should be noted that the method for modifying lignin with sodium borohydride of the present invention is to reduce and modify lignin with sodium borohydride in an alkaline alcohol system, and the sodium borohydride reduction efficiency is higher in the alcohol system. At the same time, sodium silicate is used as a reaction catalyst to shorten the reaction time to 1 to 7 minutes, thereby improving the utilization rate of sodium borohydride and increasing the hydroxyl content in lignin, so that more hydrogen bonds are generated between lignin and cellulose, thereby improving the mechanical properties of the film itself. At the same time, the raw materials used come from crop straw, which is itself a clean energy source, and the cost of production is low, realizing a low-carbon cycle.
[0048] In some embodiments, 1 mol / L sodium hydroxide solution is added dropwise to the mixed solution to adjust the pH of the solution to 10-13. In a strong alkaline environment, the decomposition rate of sodium borohydride is reduced, while its reducing ability is further improved.
[0049] In some embodiments, lignin includes alkali lignin and / or ethanol lignin; specifically, alkali lignin is obtained by spray-drying caustic soda pulping waste liquid through the latest production process, and is an industrial by-product.
[0050] In some embodiments, the alcohol solvent includes at least one of ethanol, methanol, and glycerol, preferably anhydrous ethanol.
[0051] In some embodiments, the mass ratio of lignin, alcohol solvent, sodium silicate, and sodium borohydride is (0.25-1):(10-20):(0.5-2):(0.25-1).
[0052] In some embodiments, the method for preparing ethanol lignin comprises the following steps:
[0053] S1, crushing the straw and drying it;
[0054] S2, placing the dried straw in a reactor and adding ethanol aqueous solution; the ethanol aqueous solution is an ethanol aqueous solution with an ethanol mass concentration of 70-90%; the solid-liquid ratio of the straw to the ethanol aqueous solution is 1:10-30;
[0055] S3, oxygen is passed into the reactor, and after the air above the material is completely replaced by oxygen, the reactor is sealed and oxygen is kept passing;
[0056] S4, heating, keeping warm for reaction; heating to 70-90°C; keeping warm for 2-3h for reaction; keeping oxygen flowing during the reaction, when the pressure in the reactor reaches 0.8-1.3MPa, the pressure in the reactor is balanced with the pressure at the air inlet pipe, and oxygen no longer enters the reactor;
[0057] S5. After the reaction is completed, open the reactor valve to release the pressure;
[0058] S6. After the pressure relief is completed, filter immediately to separate the straw from the liquid;
[0059] S7, distilling the liquid to remove ethanol and obtain a lignin mixture;
[0060] S8. The lignin mixture is hydrolyzed with 3% sulfuric acid to cause lignin flocculation and precipitation, followed by centrifugation. The lower precipitate is freeze-dried to obtain lignin, namely ethanol lignin.
[0061] Preferably, a 250-mesh filter is used for filtration in step S6.
[0062] Specifically, in the above embodiment, the solid-liquid ratio of straw to ethanol aqueous solution is 1:10-30, that is, 10-30 mL of ethanol aqueous solution is added per gram of straw.
[0063] In some embodiments, the pH of the mixed solution is adjusted to 10-13, and then sodium borohydride is added, and the mixture is reacted at 20-30°C for 1-7 minutes, and then dried to obtain modified lignin. Preferably, the mixture is reacted at 25°C (room temperature) for 1-7 minutes. Due to the instability of the properties of sodium borohydride itself, the reaction is carried out at room temperature to reduce the loss of sodium borohydride itself due to decomposition; at the same time, lignin itself will condense under high temperature conditions, and the reaction rate is reduced due to the steric hindrance effect. Under low temperature conditions, the steric hindrance effect of lignin is reduced, and the hydroxylation efficiency of lignin is improved.
[0064] Based on the same inventive concept, the present invention also provides a modified lignin obtained by the above-mentioned treatment method.
[0065] Based on the same inventive concept, the present invention also provides a method for preparing a cellulose composite film, comprising the following steps:
[0066] S1, adding nanocellulose (CNF) to water to obtain a cellulose solution;
[0067] S2, adding the modified lignin mentioned above to the cellulose solution to obtain a film-forming solution;
[0068] S3, pouring the film-forming liquid into the mold and solidifying it to obtain a cellulose composite film.
[0069] In some embodiments, the mass concentration of the cellulose solution is 0.5-2%.
[0070] In some embodiments, the mass of modified lignin is 10-30% of the mass of nanocellulose.
[0071] In some embodiments, the film-forming liquid is poured into a mold and cured at room temperature for 60 to 80 hours to obtain a cellulose composite film.
[0072] In some embodiments, modified lignin is added to a cellulose solution and ultrasonically dispersed to obtain a film-forming solution; 10 to 30 mL of the film-forming solution is poured into a polytetrafluoroethylene mold with a diameter of 5 to 10 cm and cured at room temperature to obtain a cellulose composite membrane.
[0073] The preparation method of the cellulose composite film of the present invention modifies alkali / ethanol lignin by sodium borohydride to increase the hydrogen bond between cellulose, and the lignin can give the composite film good anti-ultraviolet, anti-oxidation and antibacterial properties; the nanocellulose (CNF) and alkali / ethanol lignin composite film can be fully biodegraded.
[0074] The following further describes the method for modifying lignin with sodium borohydride and the method for preparing a cellulose composite film of the present application with specific examples. This section further describes the content of the present invention in conjunction with specific examples, but should not be construed as limiting the present invention. Unless otherwise specified, the technical means used in the examples are conventional means known to those skilled in the art. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0075] In the following examples, alkali lignin was purchased from Shanghai MacLean Biochemical Technology Co., Ltd.; nanocellulose (CNF), with a diameter of 50 nm and a length of 1 to 3 μm, was purchased from Shanghai MacLean Biochemical Technology Co., Ltd.
[0076] Example 1
[0077] The present application embodiment provides a method for modifying lignin with sodium borohydride, comprising the following steps:
[0078] S1, 0.5 g of alkali lignin was added to 20 mL of anhydrous ethanol and ultrasonically dispersed for 10 min to obtain a lignin solution;
[0079] S2, adding 1 g of sodium silicate to the lignin solution, and ultrasonically dispersing for 2 min to obtain a mixed solution;
[0080] S3. Add 1 mol / L sodium hydroxide solution to the mixed solution, adjust the pH of the mixed solution to 13, then add 0.5 g sodium borohydride, react at room temperature (25°C) for 3 min, filter the mixed solution after the reaction at room temperature, place the filtrate in a vacuum drying oven at 40°C, dry the water, and obtain modified lignin.
[0081] Example 2
[0082] The method for modifying lignin with sodium borohydride provided in the embodiment of the present application is the same as that in embodiment 1, except that in step S3, the reaction is carried out at room temperature (25° C.) for 1 minute.
[0083] Example 3
[0084] The method for modifying lignin with sodium borohydride provided in the embodiment of the present application is the same as that in embodiment 1, except that in step S3, the reaction is carried out at room temperature (25° C.) for 5 minutes.
[0085] Example 4
[0086] The method for modifying lignin with sodium borohydride provided in the embodiment of the present application is the same as that in embodiment 1, except that in step S3, the reaction is carried out at room temperature (25° C.) for 7 minutes.
[0087] Example 5
[0088] The method for modifying lignin with sodium borohydride provided in the embodiment of the present application is the same as that in Example 1, except that 0.25 g of sodium borohydride is added in step S3.
[0089] Example 6
[0090] The method for modifying lignin with sodium borohydride provided in the embodiment of the present application is the same as that in embodiment 1, except that 1 g of sodium borohydride is added in step S3.
[0091] Example 7
[0092] The present application embodiment provides a method for modifying lignin with sodium borohydride, comprising the following steps:
[0093] S1, 0.5 g ethanol lignin was added into 20 mL anhydrous ethanol and ultrasonically dispersed for 10 min to obtain a lignin solution;
[0094] S2, adding 1 g of sodium silicate to the lignin solution, and ultrasonically dispersing for 2 min to obtain a mixed solution;
[0095] S3, adding 1 mol / L sodium hydroxide solution to the mixed solution, adjusting the pH of the mixed solution to 13, and then adding 0.5 g sodium borohydride, reacting at room temperature (25° C.) for 3 min, filtering the mixed solution after the reaction at room temperature, placing the filtrate in a vacuum drying oven at 40° C., drying the water, and obtaining modified lignin;
[0096] Wherein, the preparation method of ethanol lignin comprises the following steps:
[0097] S11, crushing the straw: cutting the wheat straw into about 5 cm, putting it into a crusher, running it for 30 seconds to obtain powdered straw, and drying it at 105° C. for 4 hours to obtain absolutely dry powdered straw;
[0098] S12, accurately weigh 10g of absolutely dry powdered straw, place it in a 250mL reactor, prepare an ethanol aqueous solution with a mass concentration of 70% with distilled water, and add it to the reactor at a material-liquid ratio of 1:10 (i.e., 10g of absolutely dry powdered straw, add 100mL of ethanol aqueous solution with a mass concentration of 70%);
[0099] S13, start the stirring rotor to stir, seal the reactor, open the gas inlet and outlet valves, and then pass oxygen into the reactor for 5 minutes. After the air above the material is completely replaced by oxygen, close the gas outlet valve;
[0100] S14, start the reactor, heat it to 70°C, keep it warm for 2h to react, keep oxygen flowing during the reaction, and when the pressure in the reactor reaches about 0.8-1.3Mpa, the pressure in the reactor is balanced with the pressure at the air inlet pipe, and oxygen no longer enters the reactor;
[0101] S15. After the reaction is completed, close the gas inlet valve and open the reactor outlet valve to release the pressure;
[0102] S16, after the reactor is free of pressure, open the reactor, and filter with a 250-mesh filter while it is still hot to separate the straw from the black liquid to reduce the ineffective residual lignin; and wash the separated straw several times with 500 mL of 70% ethanol aqueous solution at 70° C. to reduce the residual lignin in the straw as much as possible, and mix the washing liquid with the black liquid obtained above to carry out the next distillation;
[0103] S17, placing the black liquid in step S16 in a 250 mL round-bottom flask, and using a rotary evaporator to distill at 40° C. and 80 rpm to remove ethanol; when only 10 mL of black liquid is left in the round-bottom flask, the distillation is completed, and all the distilled ethanol is recovered for secondary use.
[0104] S18. Slowly add the concentrated black liquor obtained by distillation to 2000 mL of 3% sulfuric acid solution to make the lignin flocculate and precipitate under acidic conditions, then centrifuge at 5000 rpm for 10 minutes, pour out the supernatant, freeze the lower precipitate at -18°C for 8 hours, and then freeze-dry to obtain lignin, namely ethanol lignin.
[0105] Example 8
[0106] The method for modifying lignin with sodium borohydride provided in the embodiment of the present application is the same as that in Example 7, except that in step S3, the reaction is carried out at room temperature (25° C.) for 1 minute.
[0107] Example 9
[0108] The method for modifying lignin with sodium borohydride provided in the embodiment of the present application is the same as that in embodiment 7, except that in step S3, the reaction is carried out at room temperature (25° C.) for 5 minutes.
[0109] Example 10
[0110] The method for modifying lignin with sodium borohydride provided in the embodiment of the present application is the same as that in embodiment 7, except that in step S3, the reaction is carried out at room temperature (25° C.) for 7 minutes.
[0111] Embodiment 11
[0112] The method for modifying lignin with sodium borohydride provided in the embodiment of the present application is the same as that in Example 7, except that 0.25 g of sodium borohydride is added in step S3.
[0113] Example 12
[0114] The method for modifying lignin with sodium borohydride provided in the embodiment of the present application is the same as that in embodiment 1, except that 1 g of sodium borohydride is added in step S3.
[0115] Example 13
[0116] The present invention provides a method for preparing a cellulose composite film, comprising the following steps:
[0117] S1, adding nanocellulose (CNF) to water to obtain a cellulose solution, wherein the mass concentration of the cellulose solution is 1%;
[0118] S2, adding the modified lignin prepared in Example 1 (i.e., the prepared modified alkali lignin) to the cellulose solution to obtain a film-forming solution; wherein the mass of the modified lignin is 10%, 20%, and 30% of the mass of the nanocellulose (CNF), respectively;
[0119] S3. Pour the film-forming liquid into a mold and solidify it at room temperature (25° C.) for 72 hours to obtain a cellulose composite film.
[0120] Embodiment 14
[0121] The present invention provides a method for preparing a cellulose composite film, comprising the following steps:
[0122] S1, adding nanocellulose (CNF) to water to obtain a cellulose solution, wherein the mass concentration of the cellulose solution is 1%;
[0123] S2, adding the modified lignin prepared in Example 7 (i.e., the prepared modified ethanol lignin) to the cellulose solution to obtain a film-forming solution; wherein the mass of the modified lignin is 10%, 20%, and 30% of the mass of the nanocellulose (CNF), respectively;
[0124] S3. Pour the film-forming liquid into a mold and solidify it at room temperature (25° C.) for 72 hours to obtain a cellulose composite film.
[0125] Comparative Example 1
[0126] This comparative example provides a method for preparing a cellulose film, comprising the following steps:
[0127] S1, adding nanocellulose (CNF) to water to obtain a cellulose solution, wherein the mass concentration of the cellulose solution is 1%;
[0128] S2. Pour the cellulose solution into a mold and solidify it at room temperature (25° C.) for 72 hours to obtain a cellulose film.
[0129] Comparative Example 2
[0130] This comparative example provides a method for preparing a cellulose film, comprising the following steps:
[0131] S1, adding nanocellulose (CNF) to water to obtain a cellulose solution, wherein the mass concentration of the cellulose solution is 1%;
[0132] S2, adding alkali lignin to the cellulose solution to obtain a film-forming solution; wherein the mass of the alkali lignin is 10%, 20%, and 30% of the mass of the nanocellulose (CNF), respectively;
[0133] S3. Pour the film-forming liquid into a mold and solidify it at room temperature (25° C.) for 72 hours to obtain a cellulose composite film.
[0134] Comparative Example 3
[0135] This comparative example provides a method for preparing a cellulose film, comprising the following steps:
[0136] S1, adding nanocellulose (CNF) to water to obtain a cellulose solution, wherein the mass concentration of the cellulose solution is 1%;
[0137] S2, adding ethanol lignin (prepared by the same method as in Example 7) to the cellulose solution to obtain a film-forming solution; wherein the mass of the ethanol lignin is 10%, 20%, and 30% of the mass of the nanocellulose (CNF), respectively;
[0138] S3. Pour the film-forming liquid into a mold and solidify it at room temperature (25° C.) for 72 hours to obtain a cellulose composite film.
[0139] Performance Testing
[0140] The hydroxyl content of the modified lignin prepared in Examples 1 to 4 was tested. The results are as follows: Figure 1As shown; the hydroxyl content of the modified lignin prepared in Examples 1, 5 to 6 was tested, and the results were as follows Figure 2 shown. Figure 1 The reaction time of medium alkali lignin is 3 min corresponding to Example 1, the reaction time of alkali lignin is 1 min corresponding to Example 2, the reaction time of alkali lignin is 5 min corresponding to Example 3, and the reaction time of alkali lignin is 7 min corresponding to Example 4; Figure 2 The mass ratio of sodium borohydride to alkali lignin is 1:2, corresponding to Example 5, the mass ratio of sodium borohydride to alkali lignin is 1:1, corresponding to Example 1, and the mass ratio of sodium borohydride to alkali lignin is 2:1, corresponding to Example 6.
[0141] from Figure 1 It can be seen that the hydroxyl content of the modified lignin prepared when the reaction time is 1 min in Example 2 is 2.5 mmol / g, the hydroxyl content of the modified lignin prepared when the reaction time is 3 min in Example 1 is 4.7 mmol / g, the hydroxyl content of the modified lignin prepared when the reaction time is 5 min in Example 3 is 4.0 mmol / g, and the hydroxyl content of the modified lignin prepared when the reaction time is 7 min in Example 4 is 3.2 mmol / g; Figure 2 It can be seen that in Example 5, when the mass ratio of sodium borohydride to alkali lignin is 1:2, the hydroxyl content of the prepared modified lignin is 3.0 mmol / g; in Example 6, when the mass ratio of sodium borohydride to alkali lignin is 2:1, the hydroxyl content of the prepared modified lignin is 3.8 mmol / g; and the hydroxyl content of the unmodified lignin (i.e., alkali lignin) is 2.29 mmol / g. Compared with the unmodified lignin (i.e., alkali lignin), the modified alkali lignin of the present invention has an increased hydroxyl content in all modified alkali lignins.
[0142] The hydroxyl content of the modified lignin prepared in Examples 7 to 10 was tested. The results are as follows: Figure 3 As shown; the hydroxyl content of the modified lignin prepared in Examples 7, 11 to 12 was tested, and the results were as follows Figure 4 shown. Figure 3 The reaction time of ethanol lignin is 3 min corresponding to Example 7, the reaction time of ethanol lignin is 1 min corresponding to Example 8, the reaction time of ethanol lignin is 5 min corresponding to Example 9, and the reaction time of ethanol lignin is 7 min corresponding to Example 10; Figure 4 The mass ratio of sodium borohydride to ethanol lignin is 1:2, corresponding to Example 11, the mass ratio of sodium borohydride to ethanol lignin is 1:1, corresponding to Example 7, and the mass ratio of sodium borohydride to ethanol lignin is 2:1, corresponding to Example 12.
[0143] from Figure 3It can be seen that the hydroxyl content of the modified lignin prepared when the reaction time is 3 min in Example 7 is 7.9 mmol / g, the hydroxyl content of the modified lignin prepared when the reaction time is 1 min in Example 8 is 6.25 mmol / g, the hydroxyl content of the modified lignin prepared when the reaction time is 5 min in Example 9 is 7.5 mmol / g, and the hydroxyl content of the modified lignin prepared when the reaction time is 7 min in Example 10 is 7.0 mmol / g; Figure 4 It can be seen that in Example 11, when the mass ratio of sodium borohydride to ethanol lignin is 1:2, the hydroxyl content of the prepared modified lignin is 6.5 mmol / g; in Example 12, when the mass ratio of sodium borohydride to ethanol lignin is 2:1, the hydroxyl content of the prepared modified lignin is 7.3 mmol / g; and the hydroxyl content of the unmodified lignin (i.e., ethanol lignin) is 6.12 mmol / g. Compared with the unmodified lignin (i.e., ethanol lignin), the modified ethanol lignin of the present invention has an increased hydroxyl content in all modified ethanol lignins.
[0144] In Comparative Example 2, when the mass of lignin is 10%, 20%, and 30% of the mass of nanocellulose (CNF), respectively (from left to right in the figure, 10%, 20%, and 30%, respectively), the macroscopic photograph of the prepared cellulose film is as follows: Figure 5 shown.
[0145] In Example 13, when the mass of the modified alkali lignin is 10%, 20%, and 30% of the mass of the nanocellulose (CNF), respectively (from left to right in the figure, 10%, 20%, and 30%, respectively), the macroscopic photograph of the prepared cellulose composite film is as follows: Figure 6 shown.
[0146] The stress-strain curves of the cellulose film prepared in Comparative Example 1, the cellulose composite film prepared in Example 13, and the cellulose film prepared in Comparative Example 2 were tested. The results are as follows: Figure 7 shown.
[0147] Figure 7 Medium-pure CNF refers to the cellulose film prepared in Comparative Example 1, 10wt% alkali LNP-CNF, 20wt% alkali LNP-CNF, and 30wt% alkali LNP-CNF respectively represent the cellulose composite membranes prepared when the mass of the modified lignin in Example 13 is 10%, 20%, and 30% of the mass of nanocellulose (CNF), respectively, and 10wt% original alkali lignin-CNF, 20wt% original alkali lignin-CNF, and 30wt% original alkali lignin-CNF respectively represent the cellulose membranes prepared when the mass of the alkali lignin in Comparative Example 2 is 10%, 20%, and 30% of the mass of nanocellulose (CNF), respectively.
[0148] from Figure 7 It can be seen that the tensile strength and elongation at break of the cellulose composite film prepared in Example 13 are significantly improved compared with the pure cellulose film prepared in Comparative Example 1. The performance is best when the addition amount of modified alkali lignin is 20wt%, with the yield strength and elongation at break being 27.4MPa and 6.15%, respectively, which are increased by 81.7% and 50.0%, respectively.
[0149] The stress-strain curves of the cellulose film prepared in Comparative Example 1, the cellulose composite film prepared in Example 14, and the cellulose film prepared in Comparative Example 3 were tested. The results are as follows: Figure 7 shown.
[0150] Figure 8 In the figure, pure CNF refers to the cellulose film prepared in Comparative Example 1, 10wt% ethanol LNP-CNF, 20wt% ethanol LNP-CNF and 30wt% ethanol LNP-CNF respectively represent the cellulose composite films prepared when the mass of the modified lignin in Example 14 is 10%, 20% and 30% of the mass of nanocellulose (CNF), and 10wt% raw ethanol lignin-CNF, 20wt% raw ethanol lignin-CNF and 30wt% raw ethanol lignin-CNF respectively represent the cellulose films prepared when the mass of the ethanol lignin in Comparative Example 3 is 10%, 20% and 30% of the mass of nanocellulose (CNF).
[0151] from Figure 8 It can be seen that the tensile strength and elongation at break of the cellulose composite film prepared in Example 14 are significantly improved compared with the pure cellulose film prepared in Comparative Example 1. When the addition amount of modified alkali lignin is 20wt%, the performance is the best, and the yield strength and elongation at break are 22.6MPa and 5.3%, respectively, which are increased by 50.7% and 29.3%, respectively.
[0152] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a cellulose composite film, characterized in that: The following steps are involved: adding nanocellulose to water to obtain a cellulose solution; adding modified lignin to a cellulose solution to obtain a film-forming solution; pouring the film-forming liquid into a mold and solidifying it to obtain a cellulose composite film; The mass concentration of the cellulose solution is 0.5-2%; The mass of the modified lignin is 20% of the mass of the nanocellulose; The preparation method of the modified lignin comprises the following steps: adding lignin into an alcohol solvent to obtain a lignin solution; adding sodium silicate to the lignin solution to obtain a mixed solution; The pH of the mixed solution is adjusted to 10-13, and then sodium borohydride is added, reacted at 20-30° C. for 1-7 minutes, filtered, and dried to obtain modified lignin; The lignin includes alkali lignin and / or ethanol lignin; The alcohol solvent includes at least one of ethanol, methanol and glycerol; The mass ratio of lignin, alcohol solvent, sodium silicate and sodium borohydride is (0.25-1):(10-20):(0.5-2):(0.25-1); The preparation method of the ethanol lignin comprises the following steps: Crush the straw and dry it; The dried straw is placed in a reactor and an ethanol aqueous solution is added; Pass oxygen into the reactor, and after the air above the material is completely replaced by oxygen, seal the reactor and keep passing oxygen; heat to 70-90°C; keep warm for 2-3 hours to react; keep passing oxygen during the reaction, and when the pressure in the reactor reaches 0.8-1.3MPa, the pressure in the reactor is balanced with the pressure at the air inlet pipe, and oxygen no longer enters the reactor; After the reaction is completed, the pressure is released and filtered to separate the straw from the liquid; Distilling the liquid to remove ethanol and obtain a lignin mixture; The lignin mixture is hydrolyzed with sulfuric acid to cause the lignin to flocculate and precipitate, and then centrifuged. The lower precipitate is freeze-dried to obtain lignin, which is ethanol lignin.
2. The method for preparing a cellulose composite film according to claim 1, characterized in that: The film-forming liquid is poured into a mold and cured at room temperature for 60 to 80 hours to obtain a cellulose composite film.