Bisphenol AF type diglycidyl ether, its manufacturing method, and polycrystalline bisphenol AF type diglycidyl ether

By controlling the ratio of n≥1 and n=0 units in bisphenol AF diglycidyl ether, and combining a one-step reaction and crystallization process, a low-viscosity bisphenol AF diglycidyl ether with excellent crystallinity was prepared, solving the operability and viscosity problems in the prior art, and making it suitable for laminates used in electrical and electronic circuits.

CN116745274BActive Publication Date: 2026-11-17MITSUBISHI CHEM CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202180089444.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-01-07
Filing Date
2021-12-22
Publication Date
2026-11-17
Estimated Expiration
2041-12-22

AI Technical Summary

Technical Problem

Existing bisphenol AF type diglycidyl ethers are viscous and difficult to handle in liquid form, and have high viscosity when melted, which cannot meet the requirements of low viscosity and high filler content, affecting the stability of communication signals in electrical and electronic circuits.

Method used

By controlling the ratio of n≥1 and n=0 forms in bisphenol AF diglycidyl ether within a specific range, and combining a one-step reaction and crystallization process, a low-viscosity bisphenol AF diglycidyl ether with excellent crystallinity can be prepared.

Benefits of technology

It achieves rapid crystallization speed and high productivity of bisphenol AF type diglycidyl ether, with excellent operability and anti-blocking properties, and is suitable for laminates for electrical and electronic circuits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116745274B_ABST
    Figure CN116745274B_ABST
Patent Text Reader

Abstract

A bisphenol AF type diglycidyl ether represented by the following formula (1), wherein the proportion of bisphenol AF type diglycidyl ether containing n≥1 is less than 30% by mass. (In formula (1), R 1 ~R 8 Each can independently represent a hydrogen atom, a halogen atom, an alkyl group with 1 to 4 carbon atoms, or an aryl group with 5 to 14 carbon atoms. (n is an integer greater than or equal to 0).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a bisphenol AF type diglycidyl ether, its manufacturing method, curable composition, cured product, electrical and electronic components, insulating materials, laminates for electrical and electronic circuits, and polycrystalline bisphenol AF type diglycidyl ether. The bisphenol AF type diglycidyl ether has a fast crystallization rate and excellent productivity. In addition, it is a crystalline solid with excellent operability, and has low viscosity and excellent anti-blocking properties. Background Technology

[0002] Epoxy resins possess excellent adhesion, water resistance, mechanical strength, and electrical properties, making them widely used in various fields such as adhesives, coatings, civil engineering materials, and insulating materials for electrical and electronic components. In particular, they are extensively used in electrical and electronic fields for insulating injection molding, laminated materials, and sealing materials. In recent years, the development of multilayer circuit boards used in electrical and electronic machinery has trended towards miniaturization, lightweighting, and high functionality, demanding further improvements in multilayering, high density, thinness, lightweighting, reliability, and processability.

[0003] As epoxy resins have become increasingly popular in recent years as materials for electrical and electronic components such as laminates used in electrical and electronic circuits, bisphenol AF type epoxy resin (bisphenol AF type diglycidyl ether) was studied.

[0004] Patent Document 1 describes an epoxy resin composition containing bisphenol AF type diglycidyl ether as an epoxy resin composition for sealing colorless and transparent light-emitting elements that has excellent balance of moisture resistance, heat resistance and light resistance.

[0005] Patent document 2 discloses a bisphenol AF type epoxy resin, which is solid or semi-solid at room temperature, colorless and transparent with low water vapor permeability, and excellent bonding strength, moisture resistance, heat resistance and UV resistance.

[0006] Patent document 3 discloses an epoxy resin composition for laminates that has particularly excellent dielectric properties, low water absorption, and excellent heat resistance (high Tg), which is important when used as a laminate. The composition contains bisphenol AF type diglycidyl ether.

[0007] Patent Document 1: Japanese Patent Application Publication No. 2007-246819

[0008] Patent Document 2: Japanese Patent Application Publication No. 2013-155336

[0009] Patent Document 3: Japanese Patent Application Publication No. 2013-155337

[0010] As epoxy resins have become increasingly important materials for electrical and electronic components such as laminates used in electrical and electronic circuits in recent years, low viscosity (low melt viscosity) has become a growing requirement. This is because, compared to existing multilayer circuit boards, the content of particulate fillers such as silica has increased to improve dimensional stability associated with thinner designs and to suppress energy loss in communication signals due to increased information volume and communication speed. However, when high filler content is used to suppress energy loss in communication signals, the flowability of the epoxy resin composition is compromised; therefore, to improve this reduced flowability, a low viscosity epoxy resin is desirable.

[0011] Bisphenol AF type epoxy resin has excellent dielectric properties, and is therefore often used in laminates for electrical and electronic circuits. However, the bisphenol AF type diglycidyl ether described in Patent Documents 1 to 3 is viscous and difficult to handle when it is in liquid form. In addition, its solid form has a high viscosity when melted.

[0012] Bisphenol A type diglycidyl ethers have poor crystallinity, and as shown in Reference Example 1 described later, they cannot achieve low viscosity.

[0013] Based on the inventor's research, the following determinations are made.

[0014] In bisphenol A diglycidyl ethers, the bisphenol A structure repeating unit is crystalline when there is one repeating unit (n=0 units). However, when there are two or more repeating units (n≥1 units), it is resinous, and therefore its properties change to a viscous liquid at room temperature.

[0015] To further reduce the viscosity (low melt viscosity) and improve the operability (increased crystallization rate) of bisphenol AF type diglycidyl ether, the inventors focused on the content of the constituent components. The results showed that the content ratio of the constituent components not only affects the viscosity of bisphenol AF type diglycidyl ether, but also the adhesion of the resulting solid form of bisphenol AF type diglycidyl ether. Summary of the Invention

[0016] The problem that the invention aims to solve

[0017] The problem to be solved by the present invention is to provide a bisphenol AF type glycidyl ether and a method for manufacturing the same. The bisphenol AF type glycidyl ether has a fast crystallization rate and excellent productivity. In addition, it is a crystalline solid with excellent operability, and has low viscosity and excellent anti-blocking properties.

[0018] Technical solutions to the problem

[0019] The inventors have discovered that by controlling the proportion of the n≥1 form of bisphenol AF diglycidyl ether, preferably the proportion of the n=0 form and the n≥1 form of the constituent components within a specific range, the resulting bisphenol AF diglycidyl ether exhibits excellent anti-blocking properties and can further achieve a lower viscosity compared to existing bisphenol AF epoxy resins.

[0020] The key points of this invention are as follows.

[0021] [1] A bisphenol AF type diglycidyl ether, which is represented by the following formula (1), wherein the proportion of bisphenol AF type diglycidyl ether with n≥1 is less than 30% by mass.

[0022] [Chemistry 1]

[0023]

[0024] (In equation (1), R) 1 ~R 8 Each can independently represent a hydrogen atom, a halogen atom, an alkyl group with 1 to 4 carbon atoms, or an aryl group with 5 to 14 carbon atoms. n is an integer greater than or equal to 0.

[0025] [2] According to [1], the proportion of bisphenol AF type diglycidyl ether with n=0 in the bisphenol AF type diglycidyl ether represented by formula (1) is 70% by mass or more.

[0026] [3] The bisphenol AF type diglycidyl ether according to [1] or [2] has a melting point of 50 to 73°C.

[0027] [4] Bisphenol AF type diglycidyl ether according to any one of [1] to [3] has a melting enthalpy of 20 to 70 J / g.

[0028] [5] A curable composition comprising any one of [1] to [4] bisphenol AF type diglycidyl ether and a curing agent.

[0029] [6] The curable composition according to [5] contains 0.1 to 100 parts by weight of the curing agent relative to 100 parts by weight of the bisphenol AF type diglycidyl ether.

[0030] [7] The curable composition according to [5] or [6], wherein the curing agent is at least one selected from phenolic curing agents, amide curing agents, imidazole curing agents and reactive ester curing agents.

[0031] [8] A cured material formed by curing the curable composition described in any one of [5] to [7].

[0032] [9] An electrical and electronic component formed using any one of [5] to [7].

[0033]

[10] An insulating material containing the cured product described in [8].

[0034]

[11] A laminate for electrical and electronic circuits, comprising the insulating material described in

[10] .

[0035]

[12] A method for manufacturing bisphenol AF type diglycidyl ether, which has a crystallization step, wherein bisphenol AF is reacted with epihaloalcohol in the presence of alkali, and after obtaining supercooled liquid bisphenol AF type diglycidyl ether from the reaction solution, the supercooled molten bisphenol AF type diglycidyl ether is crystallized.

[0036]

[13] According to the method for manufacturing bisphenol AF type diglycidyl ether described in

[12] , the bisphenol AF type diglycidyl ether is a bisphenol AF type diglycidyl ether represented by the following formula (1), in which the proportion of bisphenol AF type diglycidyl ether with n≥1 is less than 30% by mass.

[0037] [Chemistry 2]

[0038]

[0039] (In equation (1), R) 1 ~R 8 Each can independently represent a hydrogen atom, a halogen atom, an alkyl group with 1 to 4 carbon atoms, or an aryl group with 5 to 14 carbon atoms. n is an integer greater than or equal to 0.

[0040]

[14] According to the method for manufacturing bisphenol AF type diglycidyl ether as described in

[13] , the proportion of bisphenol AF type diglycidyl ether with n=0 in the bisphenol AF type diglycidyl ether represented by formula (1) is 70% by mass or more.

[0041]

[15] In the method for manufacturing bisphenol AF type diglycidyl ether according to any one of

[12] to

[14] , in the crystallization process, crystal nuclei are mixed and crystallized at a temperature of 0 to 50°C.

[0042]

[16] According to the method for manufacturing bisphenol AF type diglycidyl ether as described in

[15] , the amount of the crystal nucleus is 0.01 to 5 by mass relative to the molten bisphenol AF type diglycidyl ether.

[0043]

[17] In the method for manufacturing bisphenol AF type diglycidyl ether according to any one of

[12] to

[16] , in the crystallization step, an external force is applied to the molten bisphenol AF type diglycidyl ether to crystallize it.

[0044]

[18] A bisphenol type diglycidyl ether polycrystalline material having a crystallite size of more than 10 Å and less than 100,000 Å, calculated from the X-ray diffraction pattern determined by CuKα rays.

[0045]

[19] The bisphenol type diglycidyl ether polycrystalline according to

[18] has a crystallinity of more than 1% and less than 100%.

[0046]

[20] According to

[18] or

[19] , the bisphenol type diglycidyl ether polycrystal has diffraction peaks at diffraction angles (2θ) of 7.9, 16.3, 18.5, 22.3 and 26.0 degrees in the powder X-ray diffraction pattern determined by CuKα rays.

[0047] Invention Effects

[0048] The bisphenol AF type diglycidyl ether of the present invention has a fast crystallization rate and excellent productivity. In addition, it is a crystalline solid with excellent operability, and has low viscosity and excellent anti-blocking properties.

[0049] In the manufacture of the bisphenol AF type diglycidyl ether of the present invention, there is no need to perform advanced distillation purification or recrystallization operations to improve the purity of the n=0 body, and the bisphenol AF type diglycidyl ether can be manufactured in an industrially advantageous manner with good operability.

[0050] In the bisphenol AF type diglycidyl ether of the present invention, by controlling the proportion of the n≥1 body, preferably the proportion of the n=0 body and the n≥1 body within the range specified in the present invention, the crystallization rate can be accelerated and controlled to an appropriate rate, and it is expected that the production efficiency of the bisphenol AF type diglycidyl ether can be further improved. Attached Figure Description

[0051] Figure 1 This is the X-ray diffraction pattern of the bisphenol AF type diglycidyl ether polycrystal obtained in Example 1.

[0052] Figure 2 The image shows the X-ray diffraction pattern of the amorphous (non-crystalline) bisphenol AF type diglycidyl ether obtained in Comparative Example 1. Detailed Implementation

[0053] The embodiments of the present invention will now be described in detail. The following description is one example of an embodiment of the present invention, and the present invention is not limited to the following description as long as it does not deviate from its spirit.

[0054] When “~” is used in this specification, it is used as a description including the numerical or physical property values ​​before and after it.

[0055] [Bisphenol AF type diglycidyl ether]

[0056] The bisphenol AF type diglycidyl ether of the present invention is a bisphenol AF type diglycidyl ether (bisphenol AF type epoxy resin) represented by the following formula (1), characterized in that, in the following formula (1), the proportion of bisphenol AF type diglycidyl ether (hereinafter, sometimes simply referred to as "n≥1 body") containing n≥1 is less than 30% by mass.

[0057] The bisphenol AF type diglycidyl ether of the present invention preferably contains 70% by mass or more of the bisphenol AF type diglycidyl ether with n=0 (hereinafter, sometimes simply referred to as "n=0 body").

[0058] In this invention, by controlling the proportion of n≥1 particles, preferably n=0 particles, and n≥1 particles within a specific range, a balance of physical properties such as productivity, operability, low viscosity, and anti-blocking properties can be achieved.

[0059] [Chemistry 3]

[0060]

[0061] (In equation (1), R) 1 ~R 8 Each can independently represent a hydrogen atom, a halogen atom, an alkyl group with 1 to 4 carbon atoms, or an aryl group with 5 to 14 carbon atoms. n is an integer greater than or equal to 0.

[0062] The bisphenol AF type diglycidyl ether of the present invention is crystalline, and preferably becomes polycrystalline through crystallization. The polycrystalline of the present invention refers to a state in which the low molecular weight components (e.g., n=0 volume) of the bisphenol AF type diglycidyl ether, as an internal structure, are oriented and positioned to form long-range ordered microcrystals, and such microcrystals are aggregated together.

[0063] In the presence of high molecular weight components of bisphenol AF type diglycidyl ether (e.g., n≥1 volume), by controlling their presence ratio within a certain range, some or all of them are miscible with the low molecular weight component, thus becoming a state in which they are contained within the microcrystals while maintaining long-range order.

[0064] As a polycrystalline material, it can exist as long as it is composed of aggregates of microcrystals. Alternatively, it can be a phase-separated structure in which the low-molecular-weight component of bisphenol AF type diglycidyl ether or the high-molecular-weight component of bisphenol AF type diglycidyl ether is contained in the microcrystals in an amorphous solid or semi-solid form during crystallization.

[0065] Existing solid bisphenol AF type diglycidyl ethers (e.g., the solid bisphenol AF type diglycidyl ether described in Patent Document 3) are amorphous solids, and the molecules they constitute do not have an ordered structure; their molecular motion is simply frozen. Amorphous solids do not have a melting point. Although the viscosity decreases at temperatures above the glass transition point, there are also cases where the molecular weight is relatively large. In most cases, the decrease in viscosity with increasing temperature is smaller, and the solid surface becomes sticky at high temperatures, thus significantly reducing its anti-blocking properties.

[0066] Due to the structural characteristics described above, the bisphenol AF type diglycidyl ether of the present invention, as described below, has a melting point and its constituent components have a small molecular weight. Therefore, when the bisphenol AF type diglycidyl ether of the present invention is heated or otherwise heated, it melts, and the viscosity is immediately suppressed to a low level after melting. Furthermore, at room temperature, the surface of the bisphenol AF type diglycidyl ether of the present invention is dry, thus exhibiting excellent anti-blocking properties.

[0067] In the bisphenol AF type diglycidyl ether of the present invention, from the perspective of improving crystallinity and maintaining a low viscosity, the proportion of the n=0 body is preferably 70% by mass or more, more preferably 73% by mass or more, further preferably 76% by mass or more, and particularly preferably 80% by mass or more. On the other hand, if the n=0 body is 100% by mass, the crystallization rate increases, but this leads to a higher load on purification processes such as distillation when manufacturing bisphenol AF type diglycidyl ether on an industrial scale. Therefore, from the perspective of reducing such a load and improving productivity, the proportion of the n=0 body is preferably 99% by mass or less, more preferably 98% by mass or less, further preferably 97% by mass or less, and particularly preferably 95% by mass or less.

[0068] In the bisphenol AF type diglycidyl ether of the present invention, the proportion of n≥1 is less than 30% by mass, but the proportion of n=1 is preferably less than 30% by mass. Furthermore, from the perspective of improving the lattice disorder of the crystalline composition, obtaining an appropriate time until complete crystallization, and improving productivity, the proportion of n≥1, and n=1, is preferably 2% by mass or more, more preferably 5% by mass or more, and even more preferably 6% by mass or more. In addition, in order to suppress viscosity within an appropriate range, the proportion of n≥1, and n=1, is preferably 25% by mass or less, more preferably 20% by mass or less, and even more preferably 18% by mass or less.

[0069] The bisphenol AF type diglycidyl ether of the present invention can be controlled by the method described later to achieve the presence ratio of n≥1, preferably n=0, and more preferably n≥1, n=1 in the range described above.

[0070] The proportions of n=0, n≥1, specifically n=1 and n=2 or higher components in bisphenol AF diglycidyl ether are shown in the examples described below and can be determined by analysis using gel permeation chromatography (GPC).

[0071] The melting point of the bisphenol AF type diglycidyl ether of the present invention is preferably 50-73°C. From the perspective of maintaining good anti-blocking properties and good crystallinity, the melting point of the bisphenol AF type diglycidyl ether of the present invention is more preferably 52°C or higher, further preferably 54°C or higher, and particularly preferably 56°C or higher. From the perspective of moderately disrupting crystallinity and improving productivity, the melting point of the bisphenol AF type diglycidyl ether of the present invention is more preferably 72°C or lower, further preferably 70°C or lower, and particularly preferably 69°C or lower.

[0072] The melting point of the bisphenol AF type diglycidyl ether of the present invention refers to the melting point determined using differential scanning calorimetry (DSC).

[0073] Specifically, in DSC, in the measured spectrum when the temperature is increased from 30℃ to 150℃ at a rate of 10℃ / min, the temperature corresponding to the intersection of the tangent line at the maximum value of the DDSC (the spectrum obtained by taking the differential value of the DSC spectrum) at the endothermic peak of the melting point and the parallel line of the spectrum before the endothermic peak is defined as the melting point.

[0074] From the perspective of maintaining good anti-blocking properties and good crystallinity, the melting enthalpy of the bisphenol AF type diglycidyl ether of the present invention is preferably 20 J / g or more, more preferably 23 J / g or more, even more preferably 25 J / g or more, particularly preferably 30 J / g or more, and most preferably 40 J / g or more. From the perspective of moderately disrupting crystallinity and improving productivity, the melting enthalpy of the bisphenol AF type diglycidyl ether of the present invention is preferably 70 J / g or less, more preferably 67 J / g or less, and even more preferably 65 J / g or less.

[0075] The melting enthalpy of the bisphenol AF type diglycidyl ether of the present invention refers to the melting enthalpy measured using DSC.

[0076] Specifically, in DSC, the enthalpy of fusion can be determined from the area of ​​the endothermic peak at the melting point in the measured spectrum when the temperature is increased from 30°C to 150°C at a rate of 10°C / min.

[0077] In the bisphenol AF type diglycidyl ether of the present invention, the substituent R in the above formula (1) 1 ~R 8 Each is independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 4 carbon atoms, or an aryl group having 5 to 14 carbon atoms.

[0078] Examples of halogen atoms include: fluorine, chlorine, bromine, and iodine.

[0079] Examples of alkyl groups having 1 to 4 carbon atoms include methyl, ethyl, propyl, and isopropyl. They may also have substituents.

[0080] Aryl groups with 5 to 14 carbon atoms are broadly categorized as including heteroaryl groups with heterocyclic structures. Examples of aryl groups with 5 to 14 carbon atoms include phenyl, biphenyl, naphthyl, and anthracene aryl groups; and furanyl and phenylthioyl heteroaryl groups. They may also have substituents.

[0081] As the substituent R in the above formula (1) 1 ~R 8 From the perspective of maintaining good crystallinity and suppressing viscosity within an appropriate range, hydrogen atoms, methyl, phenyl or halogen atoms are preferred, hydrogen atoms or halogen atoms are more preferred, and hydrogen atoms are most preferred.

[0082] In the bisphenol AF type diglycidyl ether of the present invention, the presence ratio of alcohols having 1 to 2 carbon atoms, straight-chain, branched or cyclic ketones having 2 to 5 carbon atoms, straight-chain, branched or cyclic ethers having 2 to 6 carbon atoms, straight-chain, branched or cyclic amides having 1 to 4 carbon atoms, dimethyl sulfoxide, straight-chain, branched or cyclic alkanes having 5 to 20 carbon atoms, or benzene compounds that may have substituents is preferably 1000 ppm or less, more preferably 500 ppm or less, even more preferably 250 ppm or less, particularly preferably 100 ppm or less, and most preferably 0 ppm (excluding).

[0083] These compounds can be incorporated into bisphenol AF type diglycidyl ether via a one-step reaction process described later. However, when these compounds are present, the crystallization rate is slowed down, so their content is preferably low, and most preferably not present.

[0084] The proportions of these compounds in the bisphenol AF type diglycidyl ether of the present invention can be determined by gas chromatography.

[0085] [Method for manufacturing bisphenol AF type diglycidyl ether]

[0086] The method for manufacturing bisphenol AF type diglycidyl ether of the present invention is characterized in that bisphenol AF is reacted with epihaloalcohol in the presence of alkali, and after obtaining supercooled liquid bisphenol AF type diglycidyl ether from the reaction solution, the supercooled molten bisphenol AF type diglycidyl ether is crystallized to obtain bisphenol AF type diglycidyl ether.

[0087] Bisphenol AF, used as a raw material, is a bisphenol compound represented by the following formula (2). In this invention, the structure represented by the following formula (2) is defined as "bisphenol AF".

[0088] [Chemistry 4]

[0089]

[0090] (In equation (2), R) 9 ~R 16 respectively with R in equation (1) 1 ~R 8 (Same meaning.)

[0091] The reaction process of reacting the bisphenol compound represented by formula (2) with the epihaloalcohol in the presence of a base is not particularly limited, but it is preferred to react the bisphenol compound represented by formula (2) with the epihaloalcohol in a one-step reaction process.

[0092] The reaction process using this one-step method will be described in detail below.

[0093] [A reaction process using a one-step method]

[0094] As a specific example of a one-step manufacturing method, one can cite a method in which a bisphenol compound represented by formula (2) is manufactured by using a monohalogenated alcohol in a ratio of typically 1.00 to 20 moles, preferably 3.00 to 15.0 moles, more preferably 3.5 to 12.0 moles, and even more preferably 4.5 to 10.0 moles, relative to 1 mole of the hydroxyl group. When the amount of monohalogenated alcohol used is small, a high molecular weight phase is formed, resulting in increased viscosity and deterioration of crystallinity. When the amount of monohalogenated alcohol is excessive, in addition to excessive crystallinity, economic efficiency deteriorates.

[0095] More specifically, the bisphenol compound represented by formula (2) is mixed with epichlorohydrin or other epihaloalcohols and reacted in the presence of a base. The base is preferably an alkali metal hydroxide, either in solid or aqueous solution. The reaction can be carried out under normal or reduced pressure. The reaction temperature is typically 20–150°C under normal pressure and 30–80°C under reduced pressure. If necessary, the reaction can be carried out azeotropically while maintaining the specified temperature. The condensate obtained by cooling the volatilized vapor is then subjected to oil / water separation, allowing the oil fraction after water removal to return to the reaction system. This method allows for dehydration while simultaneously carrying out the reaction. To suppress vigorous reactions, the alkali metal hydroxide is preferably added to the reaction system in small, intermittent or continuous increments of 0.1–10 hours. The total reaction time is typically 1–15 hours.

[0096] After the reaction is complete, the insoluble byproduct salt is filtered out from the reaction solution containing the target product, bisphenol AF type diglycidyl ether, or removed by washing with water. Unreacted epihaloalcohol is then removed by vacuum distillation to obtain the target bisphenol AF type diglycidyl ether.

[0097] The obtained bisphenol AF type diglycidyl ether is a mixture of various values ​​of n from 0 to 5 in the above formula (1). Hereinafter, the bisphenol AF type diglycidyl ether obtained by this reaction is sometimes referred to as "bisphenol AF type epoxy resin composition".

[0098] Epichlorohydrin or epibromohydrin are preferred as the epihaloalcohol in this reaction. Sodium hydroxide or potassium hydroxide are preferred as the alkali metal hydroxide.

[0099] In this reaction, quaternary ammonium salts such as tetramethylammonium chloride and tetraethylammonium bromide; tertiary amines such as benzyldimethylamine and 2,4,6-tris(dimethylaminomethyl)phenol; imidazoles such as 2-ethyl-4-methylimidazolium and 2-phenylimidazolium; phosphonium salts such as ethyltriphenylphosphonium iodide; and phosphine catalysts such as triphenylphosphine can also be used.

[0100] In this reaction, inert organic solvents such as alcohols (ethanol, isopropanol, etc.), ketones (acetone, methyl ethyl ketone, etc.), ethers (dioxane, ethylene glycol, etc.), glycol ethers (methoxypropanol, etc.), and nonprotic polar solvents (dimethyl sulfoxide, dimethylformamide, etc.) can be used.

[0101] If the bisphenol AF type diglycidyl ether obtained as described above has an excessive amount of saponifiable halogens, further processing can yield purified bisphenol AF type diglycidyl ether with a sufficiently reduced amount of saponifiable halogens. In this case, the crude bisphenol AF type diglycidyl ether obtained through the reaction is redissolved in an inert organic solvent such as isopropanol, methyl ethyl ketone, methyl isobutyl ketone, toluene, xylene, dioxane, methoxypropanol, or dimethyl sulfoxide. An alkali metal hydroxide is added in solid or aqueous solution, and a ring-closing reaction is carried out at a temperature of approximately 20–120°C for 0.5–8 hours. Then, excess alkali metal hydroxide and byproduct salts are removed by washing with water, and the organic solvent is further removed by vacuum distillation. Thus, purified bisphenol AF type diglycidyl ether can be obtained in one step.

[0102] In the case of manufacturing the bisphenol AF type diglycidyl ether represented by formula (1) by a one-step method, at least the bisphenol compound represented by formula (2) is used as a raw material. However, it is also possible to manufacture the bisphenol AF type diglycidyl ether of formula (1) as a mixture of the bisphenol AF type diglycidyl ether and other epoxy resins using polyhydroxy compounds other than the bisphenol compound represented by formula (2) (sometimes referred to as "other polyhydroxy compounds" in this invention). However, from the perspective of improving the effect of this invention, the proportion of the bisphenol compound represented by formula (2) is preferably 72 mol% or more, more preferably 80 mol% or more, further preferably 90 mol% or more, and particularly preferably 95 mol% or more, relative to the total amount of all polyhydroxy compounds used as raw materials. The upper limit is 100 mol%, and the most preferred is 100 mol%. In this invention, "polyhydroxy compound" is a general term for phenolic compounds with two or more components and alcohols with two or more components.

[0103] Other examples of polyhydroxy compounds include: bisphenol A, bisphenol F, bisphenol S, bisphenol AD, hydroquinone, resorcinol, methyl resorcinol, biphenol, tetramethyl biphenol, dihydroxynaphthalene, dihydroxydiphenyl ether, thiodiphenols, phenolic varnish resins, cresol phenolic varnish resins, phenol aralkyl resins, biphenyl aralkyl resins, naphthol aralkyl resins, terpene phenol resins, dicyclopentadienol resins, bisphenol A phenolic varnish resins, naphthol phenolic varnish resins, brominated bisphenol A, brominated phenolic varnish resins, and various other polyphenols; various phenols in combination with benzaldehyde, hydroxybenzaldehyde, crotonaldehyde, etc. Polyphenolic resins obtained from the condensation reaction of various aldehydes such as dialdehyde; polyphenolic resins obtained from the condensation reaction of xylene resin and phenols; various phenolic resins such as co-condensation resins of heavy oil or asphalt with phenols and formaldehyde; chain aliphatic diols such as ethylene glycol, 1,3-propanediol, propylene glycol, 1,3-butanediol, 1,4-butanediol, 1,3-pentanediol, 1,4-pentanediol, 1,5-pentanediol, and 1,6-hexanediol; cyclic aliphatic diols such as cyclohexanediol and cyclodecanediol; polyalkylene ether diols such as polyvinyl ether diol, polyoxymethylene ether diol, and polypropylene ether diol. Preferred compounds among these include: phenolic varnish resins, phenolic aralkyl resins, polyphenolic resins obtained from the condensation reaction of phenol and hydroxybenzaldehyde, biphenyl aralkyl resins, naphthol aralkyl resins; chain aliphatic diols such as ethylene glycol, 1,3-propanediol, propylene glycol, 1,3-butanediol, 1,4-butanediol, 1,3-pentanediol, 1,4-pentanediol, 1,5-pentanediol, and 1,6-hexanediol; cyclic aliphatic diols such as cyclohexanediol and cyclodecanediol; and polyalkylene ether diols such as polyoxymethylene ether diol, polyoxymethylene ether diol, and polypropylene ether diol.

[0104] [Crystallization process of bisphenol AF type diglycidyl ether]

[0105] When obtaining the bisphenol AF type diglycidyl ether of the present invention, the bisphenol AF type epoxy resin composition obtained in the above reaction step is crystallized.

[0106] In this invention, during the crystallization of the bisphenol AF type epoxy resin composition, firstly, after obtaining the supercooled liquid bisphenol AF type epoxy resin composition from the reaction solution, the supercooled molten bisphenol AF type epoxy resin composition is crystallized to obtain the bisphenol AF type diglycidyl ether of this invention.

[0107] In the context of this invention, "supercooled liquid" refers to a state in which the substance retains its liquid-like fluidity below its melting point. Typically, during a phase transition, the state of a substance remains unchanged even below the temperature at which the phase change occurs (metastable state). The bisphenol AF type epoxy resin composition of this invention crystallizes slowly and can maintain its molten state even when cooled from a molten state above its melting point to below its melting point, thus enabling processing while maintaining its liquid-like fluidity.

[0108] As a method for crystallization, it is preferable that, before and after obtaining the supercooled liquid bisphenol AF type epoxy resin composition in the above reaction step, the n=0 component in the above formula (1) is 70 to 100% by mass, and the n≥1 component is less than 30% by mass. As a method for controlling the amount of the n=0 component and the n≥1 component, the following methods can be cited as examples.

[0109] <1> A method for adjusting the feed molar ratio of the bisphenol compound represented by formula (2) to the epihaloalcohol and the amount of alkali used in the above reaction process;

[0110] <2> A method for controlling the amount of bisphenol AF type epoxy resin composition from a reaction solution containing such composition by purification and distillation during the process of obtaining a supercooled liquid bisphenol AF type epoxy resin composition.

[0111] <3> A method for adding crystal nuclei to a bisphenol AF type epoxy resin composition in a supercooled molten state;

[0112] <4> A method for crystallizing a bisphenol AF type epoxy resin composition in a supercooled molten state by applying external force;

[0113] <5> A method for crystallizing a supercooled molten bisphenol AF type epoxy resin composition by dripping it onto a metal plate, wherein the metal plate is controlled at a melting point below 49°C, for example, 10–40°C.

[0114] These methods are preferred to be implemented individually or in combination.

[0115] In the method of adding crystal nuclei, the amount of crystal nuclei added is preferably 0.01 to 5% by mass relative to the supercooled bisphenol AF type epoxy resin composition. From the perspective of maintaining good crystallinity, the amount of crystal nuclei added is more preferably 0.05% by mass or more, further preferably 0.2% by mass or more, particularly preferably 0.5% by mass or more, and most preferably 1% by mass or more. From the perspective of economy, the amount of crystal nuclei added is more preferably 3% by mass or less, further preferably 2% by mass or less.

[0116] As the crystal nucleus, bisphenol AF type diglycidyl ether polycrystals are preferred, and in particular, polycrystals containing more than 70% by mass of n=0 are preferred. The particle size of the crystal nucleus is not specifically specified, but from the perspective of accelerating the crystallization rate, the particle size (diameter) is preferably 10 mm or less, and more preferably 8 mm or less.

[0117] The crystallite of bisphenol AF type diglycidyl ether used herein, calculated based on the powder X-ray diffraction pattern determined by CuKα rays, is preferably 10 Å or more and 100,000 Å or less. More preferably, it is 50 Å or more, further preferably 100 Å or more, and particularly preferably 150 Å or more. On the other hand, more preferably, it is 50,000 Å or less, further preferably 10,000 Å or less, and particularly preferably 5,000 Å or less.

[0118] In powder X-ray diffraction patterns determined by CuKα rays, the crystallite size is preferably calculated based on the presence of a peak at the diffraction angle (2θ) at 26 degrees.

[0119] For the polycrystal used as the crystal nucleus, the full width at half maximum (FWHM) of the peak at 2θ=26° in the X-ray diffraction pattern determined by CuKα rays is preferably 0.01° to 1.0°, more preferably 0.1° to 0.7°, and even more preferably 0.2° to 0.5°.

[0120] As a polycrystalline nucleus, the crystallinity is preferably 1% or more and 100% or less, more preferably 20% or more, even more preferably 40% or more, and particularly preferably 60% or more.

[0121] The preferred holding temperature for promoting crystallization after adding crystal nuclei is 0 to 50°C. From the perspective of increasing the crystallization rate, this holding temperature is more preferably 5°C or higher, and even more preferably 10°C or higher. From an economic perspective, it is more preferably 45°C or lower, and even more preferably 40°C or lower.

[0122] In methods of crystallizing bisphenol A diglycidyl ether by applying external force in a supercooled molten state, the external force orients the crystalline sites while maintaining molecular mobility, thus promoting crystal growth. The temperature is not particularly limited as long as it falls within the aforementioned temperature range, but as a lower limit, a temperature at which an industrially usable viscosity is achieved for applying external force is preferred. As a general standard, this viscosity is approximately 10,000 pF or lower. Above this viscosity, applying external force requires a large amount of energy and is impractical. The upper limit temperature is preferably about 10°C lower than the melting point of bisphenol A diglycidyl ether. At temperatures infinitely close to the melting point, the cohesive forces of the molecules decrease, making crystallization less likely.

[0123] The state of crystal nucleus growth or the state of promoting crystallization mentioned here refers to the state in which the resin becomes opaque and loses its adhesiveness, or exhibits sufficient hardness.

[0124] Examples of external forces applied in this invention include shearing force, vibration, and stirring. Methods of applying this external force include electric motors, mixers, vibrators, ultrasonic devices, and extruders.

[0125] Examples of metal plates that can be used in the method of dripping a bisphenol AF type epoxy resin composition onto a metal plate to crystallize it include stainless steel (SUS) plates, iron plates, and aluminum plates. However, stainless steel (SUS) plates are preferred from the perspective of rust prevention and preventing foreign matter from entering during manufacturing.

[0126] [Bisphenol diglycidyl ether polycrystalline]

[0127] The crystallite size of the bisphenol-type diglycidyl ether polycrystalline material of the present invention, calculated from the powder X-ray diffraction pattern determined by CuKα rays, is 10 Å or more and 100,000 Å or less.

[0128] There are no particular limitations on the types of bisphenol diglycidyl ethers, but examples include: bisphenol A type diglycidyl ether, bisphenol AD ​​type diglycidyl ether, bisphenol AF type diglycidyl ether, bisphenol AP type diglycidyl ether, bisphenol B type diglycidyl ether, bisphenol BP type diglycidyl ether, bisphenol E type diglycidyl ether, bisphenol F type diglycidyl ether, bisphenol G type diglycidyl ether, bisphenol M type diglycidyl ether, bisphenol S type diglycidyl ether, bisphenol P type diglycidyl ether, bisphenol PH type diglycidyl ether, bisphenol TMC type diglycidyl ether, bisphenol Z type diglycidyl ether, etc.

[0129] The bisphenol-type diglycidyl ether polycrystalline of the present invention is particularly preferably bisphenol AF type diglycidyl ether, and more preferably the bisphenol AF type diglycidyl ether of the present invention.

[0130] The crystallite size is preferably 50 Å or more, more preferably 100 Å or more, and particularly preferably 150 Å or more. On the other hand, the crystallite size is preferably 50,000 Å or less, more preferably 10,000 Å or less, and even more preferably 5,000 Å or less.

[0131] In powder X-ray diffraction patterns determined by CuKα rays, the crystallite size is preferably calculated based on the presence of a peak at the diffraction angle (2θ) at 26 degrees.

[0132] The bisphenol-type diglycidyl ether polycrystalline material of the present invention preferably has a half-width of 0.01° to 1.0° for the peak at 2θ=26.0deg in the X-ray diffraction pattern determined by CuKα rays, more preferably 0.1° to 0.7°, and even more preferably 0.2° to 0.5°.

[0133] The bisphenol diglycidyl ether polycrystalline of the present invention preferably has a crystallinity of 1% or more and 100% or less, more preferably 20% or more, even more preferably 40% or more, and particularly preferably 60% or more.

[0134] The bisphenol-type diglycidyl ether polycrystal of the present invention preferably has diffraction peaks at diffraction angles (2θ) of 7.9, 16.3, 18.5, 22.3 and 26.0 degrees in the powder X-ray diffraction pattern determined by CuKα rays.

[0135] [Curing composition]

[0136] The curable composition of the present invention contains at least the aforementioned bisphenol AF type diglycidyl ether and curing agent. Furthermore, other epoxy resins, inorganic fillers, coupling agents, antioxidants, and other additives besides the bisphenol AF type diglycidyl ether of the present invention may be appropriately incorporated into the curable composition of the present invention, as needed.

[0137] The curable composition of the present invention achieves low viscosity by incorporating the bisphenol AF type diglycidyl ether of the present invention, thereby enabling an increase in the amount of filler added and an improvement in impregnation in glass cloth, which is beneficial for the micro-wiring, multi-layering, and high-density of electronic components.

[0138] [Curing agent]

[0139] In this invention, a curing agent refers to a substance that facilitates the crosslinking reaction and / or chain growth reaction between the epoxy groups of an epoxy resin. In this invention, even if referred to as a "curing accelerator," any substance that facilitates the crosslinking reaction and / or chain growth reaction between the epoxy groups of an epoxy resin is generally considered a curing agent.

[0140] Compared to 100 parts by weight of the solid content of the bisphenol AF type diglycidyl ether of the present invention, the content of the curing agent in the curable composition of the present invention is preferably 0.1 to 100 parts by weight, more preferably 90 parts by weight or less, and even more preferably 80 parts by weight or less, based on the solid content.

[0141] When the curable composition of the present invention contains other epoxy resins described later, the mass ratio of the solid components of the bisphenol AF type diglycidyl ether of the present invention to other epoxy resins is preferably 99 / 1 to 1 / 99.

[0142] In this case, relative to the total solids content of the bisphenol AF type diglycidyl ether and other epoxy resins of the present invention, the content of the curing agent in the curable composition of the present invention is preferably 0.1 to 100 parts by weight, more preferably 90 parts by weight or less, and even more preferably 80 parts by weight or less, based on the solids content.

[0143] In this invention, "solid components" refers to components other than the solvent, including not only solid epoxy resins but also semi-solid and viscous liquid components. "Total epoxy resin components" refers to the sum of the bisphenol AF type diglycidyl ether of this invention and other epoxy resins described later.

[0144] There are no particular limitations on the curing agent used in the curable composition of the present invention; generally known epoxy resin curing agents can be used. From the perspective of improving heat resistance, preferred curing agents include phenolic curing agents, amide curing agents, imidazole curing agents, and reactive ester curing agents. Examples of phenolic curing agents, amide curing agents, imidazole curing agents, reactive ester curing agents, and other usable curing agents are given below.

[0145] <Phenolic curing agent>

[0146] From the perspective of improving the workability of the obtained curable composition and the heat resistance after curing, phenolic curing agents are preferred as curing agents.

[0147] Specific examples of phenolic curing agents include: bisphenol A, bisphenol F, 4,4'-dihydroxydiphenylmethane, 4,4'-dihydroxydiphenyl ether, 1,4-bis(4-hydroxyphenoxy)benzene, 1,3-bis(4-hydroxyphenoxy)benzene, 4,4'-dihydroxydiphenyl sulfide, 4,4'-dihydroxydiphenyl ketone, 4,4'-dihydroxydiphenyl sulfone, 4,4'-dihydroxybiphenyl, 2,2'-dihydroxybiphenyl, 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, phenolic varnish, bisphenol A phenolic varnish, o-cresol phenolic varnish, m-cresol phenolic varnish, p-cresol phenolic varnish, xylenol phenolic varnish, poly(p-hydroxystyrene), hydroquinone, resorcinol, and catechol. Tert-butylcatechol, tert-butylhydroquinone, phloroglucinol, phloroglucinol, tert-butylcatechol, allylated phloroglucinol, polyallylated phloroglucinol, 1,2,4-phenylpyroglucinol, 2,3,4-trihydroxybenzophenone, 1,2-dihydroxynaphthalene, 1,3-dihydroxynaphthalene, 1,4-dihydroxynaphthalene, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 1,7-dihydroxynaphthalene, 1,8-dihydroxynaphthalene, 2,3-dihydroxynaphthalene, 2,4-dihydroxynaphthalene, 2,5-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, 2,7-dihydroxynaphthalene, 2,8-dihydroxynaphthalene, allylated or polyallylated derivatives of the above dihydroxynaphthalenes, allylated bisphenol A, allylated bisphenol F, allylated phenolic varnish, allylated phloroglucinol, etc.

[0148] The phenolic curing agents mentioned above can be used alone, or two or more can be mixed in any combination and ratio.

[0149] When using a phenolic curing agent, it is preferable to use it in a manner where the equivalent ratio of the functional groups in the curing agent to the epoxy groups in all epoxy resin components of the curable composition is in the range of 0.8 to 1.5. Within this range, unreacted epoxy groups and functional groups of the curing agent are less likely to remain, which is therefore preferable.

[0150] <Amide-based curing agents>

[0151] From the perspective of improving the heat resistance of the obtained curable composition, it is preferable to use an amide-based curing agent as the curing agent.

[0152] Examples of amide-based curing agents include dicyandiamine and its derivatives, and polyamide resins.

[0153] The amide-based curing agents mentioned above can be used alone, or two or more can be mixed in any combination and ratio.

[0154] The amide-based curing agent is preferably used in the range of 0.1% to 20% by mass relative to the total amount of all epoxy resin components and the amide-based curing agent as solid components in the curable composition.

[0155] <Imidazoles>

[0156] From the perspective of ensuring the curing reaction proceeds fully and improving heat resistance, imidazole-based curing agents are preferred.

[0157] Examples of imidazoles include: 2-phenylimidazolium, 2-ethyl-4(5)-methylimidazolium, 2-phenyl-4-methylimidazolium, 1-benzyl-2-methylimidazolium, 1-benzyl-2-phenylimidazolium, 1-cyanoethyl-2-undecylimidazolium, 1-cyano-2-phenylimidazolium, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, and 2,4-diamino-6-[2'-methylimidazolium-(1')] [Ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazolyl isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazolium, 2-phenyl-4-methyl-5-hydroxymethylimidazolium, and epoxy resin adducts of the above imidazoles, etc.

[0158] Because imidazoles have catalytic ability, they are usually classified as curing accelerators as described later, but in this invention they are classified as curing agents.

[0159] The imidazoles mentioned above can be used alone, or two or more can be used in any combination and ratio.

[0160] Imidazoles are preferably used in a range of 0.1 to 20% by mass relative to the total amount of the epoxy resin component and the imidazoles as solid components in the curable composition.

[0161] <Active Ester-Based Curing Agent>

[0162] From the perspective of ensuring that the cured product exhibits low water absorption and low dielectric properties, it is preferable to use an active ester-based curing agent.

[0163] As reactive ester-based curing agents, compounds having two or more highly reactive ester groups in one molecule, such as phenolic esters, thiophenolic esters, N-hydroxyamine esters, and esters of heterocyclic hydroxyl compounds, are preferred. Phenolic esters formed by reacting carboxylic acid compounds with aromatic compounds having phenolic hydroxyl groups are more preferred. Examples of carboxylic acid compounds include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyromellitic acid. Examples of aromatic compounds having phenolic hydroxyl groups include catechol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucinol, pyroglucinol, dicyclopentadienyldiol, and phenolic varnish. Polyarylates can also be used as similar curing agents.

[0164] Commercially available reactive ester curing agents include: HPC-8000-65T (an reactive ester curing agent containing a dicyclopentadiene structure) and HPC-8150-60T (an reactive ester curing agent containing a naphthalene structure in its main skeleton) (both manufactured by DIC); W-575 and V-575 (both manufactured by UNITIKA, polyarylates with a bisphenol skeleton).

[0165] The above-mentioned active ester-based curing agents can be used alone, or two or more can be mixed in any combination and ratio.

[0166] The active ester-based curing agent is preferably used in a manner in which the equivalent ratio of the active ester group in the curing agent to the epoxy group in all the epoxy resins in the curable composition is in the range of 0.2 to 2.0.

[0167] <Other Curing Agents>

[0168] Other curing agents besides those described above that can be used in the curable compositions of the present invention include, for example: amine curing agents (excluding tertiary amines), acid anhydride curing agents, tertiary amines, organophosphorus compounds, phosphonium salts, tetraphenylboron salts, organic acid dihydrazides, boron halide amine complexes, polythiol curing agents, isocyanate curing agents, end-capped isocyanate curing agents, carbodiimides, etc.

[0169] The other curing agents mentioned above can be used alone, or two or more can be mixed in any combination and ratio.

[0170] [Other epoxy resins]

[0171] The curable composition of the present invention may contain other epoxy resins. By using other epoxy resins, deficiencies in physical properties can be compensated for, and various physical properties can be improved.

[0172] Other epoxy resins preferably have two or more epoxy groups within their molecules. Examples include bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, bisphenol Z type epoxy resin, naphthalene type epoxy resin, phenolic varnish type epoxy resin, cresol phenolic varnish type epoxy resin, phenolic alkyl type epoxy resin, biphenyl type epoxy resin, triphenylmethane type epoxy resin, dicyclopentadiene type epoxy resin, and many other epoxy resins. These can be used individually or as a mixture of two or more.

[0173] In the curable composition of the present invention, when using the bisphenol AF type diglycidyl ether and other epoxy resins of the present invention, the amount of other epoxy resins incorporated into 100% by mass of all epoxy resin components as solid components is preferably 1% by mass or more, more preferably 5% by mass or more, further preferably 10% by mass or more, preferably 99% by mass or less, more preferably 95% by mass or less, and further preferably 90% by mass or less. By making the proportion of other epoxy resins at or above the above-mentioned lower limit, the effect of improving physical properties obtained by incorporating other epoxy resins can be sufficiently obtained. By making the proportion of other epoxy resins at or below the above-mentioned upper limit, it is preferable from the perspective of fully utilizing the effect of the bisphenol AF type diglycidyl ether of the present invention and obtaining the effect of improving physical properties such as anti-blocking and low viscosity.

[0174] [solvent]

[0175] In order to adjust the viscosity of the curing composition appropriately during the coating process, a solvent may be added to dilute the curing composition of the present invention.

[0176] In the curable composition of the present invention, the solvent is used to ensure the operability and workability of the curable composition during molding, and there is no particular limitation on the amount used.

[0177] The term "solvent" in this invention is used differently from the aforementioned term "solvent medium" according to their usage, but they can be used independently in the same form or in different forms.

[0178] Examples of solvents that may be contained in the curable composition of the present invention include: ketones such as acetone, methyl ethyl ketone (MEK), methyl isobutyl ketone, and cyclohexanone; esters such as ethyl acetate; ethers such as ethylene glycol monomethyl ether; amides such as N,N-dimethylformamide and N,N-dimethylacetamide; alcohols such as methanol and ethanol; alkanes such as hexane and cyclohexane; and aromatics such as toluene and xylene.

[0179] The solvents listed above can be used alone, or two or more can be mixed in any combination and ratio.

[0180] [Other ingredients]

[0181] In order to further improve its functionality, the curable composition of the present invention may also contain components other than those listed above (sometimes referred to as "other components" in the present invention).

[0182] Other components include: thermosetting resins and photocurable resins other than epoxy resins, curing accelerators (excluding substances contained in "curing agents"), UV protectants, antioxidants, coupling agents, plasticizers, fluxes, flame retardants, colorants, dispersants, emulsifiers, low-elasticity agents, diluents, defoamers, ion scavengers, inorganic fillers, organic fillers, etc.

[0183] 〔Cured product〕

[0184] The cured product formed by curing the curable composition of the present invention, that is, the cured product formed by curing the bisphenol AF type diglycidyl ether of the present invention by curing agent, can increase the amount of filler added and improve the impregnation in glass cloth by reducing the viscosity of the curable composition, thus providing a cured product that is beneficial to the micro-wiring, multi-layering and high-density of electronic components.

[0185] The term "curing" here refers to the intentional curing of the curable composition by heat and / or light. The degree of curing is controlled according to the desired physical properties and application. The curing reaction can proceed to a fully cured or semi-cured state without particular limitation, but the reaction rate of the curing reaction between the epoxy group and the curing agent is typically 5-95%.

[0186] The curing method for the curable composition used to cure the curable composition of the present invention varies depending on the components and amounts incorporated into the curable composition, but generally, heating conditions of 80–280°C for 60–360 minutes are cited. This heating is preferably a two-stage process consisting of a primary heating at 80–160°C for 10–90 minutes and a secondary heating at 120–200°C for 60–150 minutes. In a mixed system where the glass transition temperature (Tg) is higher than the temperature of the secondary heating, a further tertiary heating at 150–280°C for 60–120 minutes is preferred. From the perspective of reducing poor curing and solvent residue, such secondary and tertiary heating is preferred.

[0187] When producing a resin semi-cured product, it is preferable to cure the curing composition by heating or other means until it can maintain its shape. If the curing composition contains solvent, most of the solvent is usually removed by methods such as heating, reducing pressure, or air drying; however, it is also permissible for up to 5% by mass of solvent to remain in the resin semi-cured product.

[0188] 〔use〕

[0189] The bisphenol AF type diglycidyl ether of the present invention exhibits excellent productivity and operability, and is characterized by low viscosity and excellent anti-blocking properties. The bisphenol AF type diglycidyl ether of the present invention can reduce the viscosity of the curable composition, thus enabling an increase in the amount of filler added and improved impregnation in glass cloth.

[0190] Therefore, the bisphenol AF type diglycidyl ether of the present invention can be applied to various fields such as adhesives, coatings, civil engineering materials, and insulating materials for electrical and electronic components, and is particularly useful as an insulating injection molding, laminate, and sealing material in the electrical and electronic field.

[0191] Examples of uses of the bisphenol AF type diglycidyl ether and curable compositions containing it according to the present invention include: multilayer printed circuit boards, electrical and electronic components such as laminates for electrical and electronic circuits such as capacitors, adhesives such as film adhesives and liquid adhesives, semiconductor sealing materials, underfill materials, inter-chip fillers for 3D-LSI, insulating materials such as insulating sheets, prepregs, heat dissipation substrates, etc., but are not limited to any of the above.

[0192] [Electrical and electronic components]

[0193] The curable composition of the present invention is suitable for use in electrical and electronic components such as laminates for electrical and electronic circuits, as described above.

[0194] In this invention, the "laminated board for electrical and electronic circuits" is formed by laminating an insulating layer containing the curable composition of this invention with a conductive metal layer. As long as it is formed by laminating an insulating layer containing the curable composition of this invention with a conductive metal layer, it can be used as a concept that includes, for example, a capacitor, even if it is not an electrical and electronic circuit.

[0195] In the laminated board for electrical and electronic circuits, an insulating layer composed of two or more curable compositions can be formed, provided that the curable composition of the present invention is used in at least one layer. Alternatively, two or more conductive metal layers can also be formed.

[0196] The thickness of the insulating layer formed by the curable composition of the present invention in the laminate for electrical and electronic circuits is typically about 10 to 200 μm. The thickness of the conductive metal layer is typically about 0.2 to 70 μm.

[0197] [Conductive metals]

[0198] Examples of conductive metals used in laminates for electrical and electronic circuits include copper, aluminum, and alloys containing these metals. In this invention, the conductive metal layer of the laminate for electrical and electronic circuits can be made of metal foils of these metals, or a metal layer formed by plating or sputtering.

[0199] [Manufacturing method of laminated boards for electrical and electronic circuits]

[0200] The following methods can be cited as examples of methods for manufacturing the laminated board for electrical and electronic circuits in this invention.

[0201] (1) A prepreg is prepared by impregnating the curable composition of the present invention into a nonwoven fabric or cloth made of inorganic and / or organic fiber materials such as glass fiber, polyester fiber, aramid fiber, cellulose, and nanofiber cellulose. After a conductive metal layer is formed by conductive metal foil and / or plating, a circuit is formed using a photoresist or the like. Such layers are stacked to the required number to form a laminate.

[0202] (2) Using the prepreg from (1) above as the core material, a layer composed of the curable composition of the present invention and a conductive metal layer are laminated on it (on one or both sides) (laminarization). The layer composed of the curable composition may contain organic and / or inorganic fillers.

[0203] (3) The layers are formed by stacking a layer of curable composition of the present invention and a conductive metal layer without using a core material.

[0204] Example

[0205] The present invention will now be described in more detail with reference to embodiments. However, the present invention is not limited to the following embodiments.

[0206] The values ​​of various manufacturing conditions and evaluation results in the following embodiments refer to preferred values ​​that are upper or lower limits in the embodiments of the present invention. The preferred range may be a range defined by a combination of the values ​​of the aforementioned upper or lower limits and the values ​​of the following embodiments or values ​​between embodiments.

[0207] [Methods for evaluating physical properties and characteristics]

[0208] In the following examples and comparative examples, the evaluation of physical properties and characteristics was carried out according to the methods described in (1) to (7) below.

[0209] (1) Composition ratio analysis of bisphenol AF type glycidyl ether

[0210] The separation was performed using the "HLC-8320GPC device" manufactured by Tosoh Corporation and the "TSKGELSuperHM-H+H5000+H4000+H3000+H2000" manufactured by Tosoh Corporation. The content ratios of the n=0, n=1, and n=2 compounds (the compounds with n=2) in the above formula (1) were determined from the analytical spectra.

[0211] Eluent: Tetrahydrofuran

[0212] Flow rate: 0.5 ml / min

[0213] Detection: RI

[0214] Temperature: 40℃

[0215] Sample concentration: 0.1–0.2% by mass

[0216] Sample loading volume: 10 μl

[0217] (2) Melting point

[0218] Using the "DSC7020" manufactured by SII Nanotechnology, the melting point was determined by heating from 0°C to 150°C at a rate of 10°C / min. In the measured spectrum, the temperature corresponding to the intersection of the tangent line at the maximum value of the DDSC (the spectrum obtained by taking the differential value of the DSC spectrum) at the endothermic peak of the melting point and the parallel line of the spectrum before the endothermic peak was taken as the melting point.

[0219] (3) Enthalpy of fusion

[0220] The enthalpy of fusion was calculated using the area of ​​the endothermic peak in the DSC spectrum when the temperature was increased from 0°C to 150°C at a rate of 10°C / min using the "DSC7020" manufactured by SII Nanotechnology.

[0221] (4) Crystallization rate

[0222] The crystallization time of molten bisphenol AF type epoxy resin composition samples was determined. For samples that did not crystallize after stirring for 15 minutes, stirring was stopped, and the samples were allowed to stand at 25°C to confirm the time until crystallization. Crystallization was determined when the sample became uniformly white and dry, and no liquid sample adhered to a bamboo stick. The operation after cooling was carried out in a constant temperature room at 25°C. The criteria for determining crystallinity are as follows.

[0223] A: Crystallization is completed within 15 minutes of stirring.

[0224] B: Crystallization is completed within 15 minutes of stirring and 24 hours of settling.

[0225] C: Stirring time exceeds 15 minutes and standing time exceeds 24 hours, which will take a long time to complete crystallization.

[0226] (5) Viscosity

[0227] A cone-plate viscometer (ICI viscometer) manufactured by Tokai Yagami Co., Ltd. was used. The sample was melted on the hot plate of the viscometer, which was adjusted to 100°C, and the viscosity was measured at 750 rpm. A viscosity of 1.5P or less is considered acceptable.

[0228] (6) Anti-adhesion

[0229] Crush 0.5g of the sample with a scraper to form particles with a diameter of 1mm square, then heat to 40℃ and maintain for 24 hours. Confirm the shape of the heated sample and determine its anti-blocking properties according to the following standards.

[0230] A: The shape of the sample did not change before and after heating.

[0231] B: After heating, the particles become sticky, but there is no evidence of them adhering to containers or changing in shape.

[0232] C: After heating, the particles become sticky, but it is also visible that the particles are combined with each other and attached to the container, etc.

[0233] (7) Powder X-ray diffraction (XRD)

[0234] XRD measurements of the powder samples were performed using an X'Pert Pro MPD manufactured by PANalytical, employing a concentrated CuKα ray optical system.

[0235] The crystallite size is calculated using the half-maximum width β, which is overcorrected for peak broadening from the device, and is given by Equation 1 (Scherrer formula).

[0236] D=Kλ / βcosθ (Equation 1)

[0237] In Equation 1, the symbols are shown below.

[0238] D: Crystalline size (Å)

[0239] K: Scherrer constant K = 0.9

[0240] λ: The wavelength of X-rays is λ = 1.54059 (Å).

[0241] β: Full width at half maximum (rad)

[0242] θ: Bragg angle (rad)

[0243] The X-ray diffraction peaks from CuKα rays used in the crystallite size calculations were 2θ = 26.0deg.

[0244] Here, β uses the measured full width at half maximum (FWHM) β0 and the FWHM β from the device. i Calculated using Equation 2 below. β i The full width at half maximum (FWHM) was calculated using the diffraction pattern of Si powder (NIST640c).

[0245] β 2 =β0 2 -β i 2 (Equation 2)

[0246] Crystallinity is determined by fitting the XRD pattern to the area (Q) of the crystalline region at 2θ = 5° to 50°. C ) and the area of ​​the amorphous portion (Q) A And calculate using Equation 3 below.

[0247] Crystallinity (%) = Q C / (Q) C +Q A (Equation 3)

[0248] [Raw materials, etc.]

[0249] The raw materials and their synthesis methods used in the following examples and comparative examples are shown below.

[0250] [Synthetic Example 1: Synthesis of Bisphenol AF Type Glycidyl Ether]

[0251] 200 g of 2,2-bis(4-hydroxyphenyl)hexafluoropropane, 661 g of epichlorohydrin, 258 g of isopropanol, and 275 g of pure water were added to a 2 L flask and stirred at 40 °C to form a homogeneous solution. Then, 114 g of 48.5% sodium hydroxide solution was added dropwise over 1.5 hours at a temperature ranging from 40 to 65 °C, and the mixture was maintained at 65 °C for 30 minutes to complete the epoxidation reaction. After the reaction was complete, the temperature was raised to 145 °C while distilling under reduced pressure to remove unreacted epichlorohydrin and isopropanol.

[0252] Next, 400g of methyl isobutyl ketone was added to the system and dissolved. The temperature was raised to 65°C, and 6g of 48.5% sodium hydroxide solution was added. The reaction was allowed to proceed for 1 hour. The resulting solution was washed four times with pure water, and the methyl isobutyl ketone was removed by distillation under reduced pressure at 100–150°C, yielding 266g of a bisphenol AF type epoxy resin composition composed of bisphenol AF type diglycidyl ether, which was a supercooled liquid at room temperature. The composition ratio (mass%) of the obtained bisphenol AF type epoxy resin composition, analyzed by GPC, showed that the n=0 fraction of bisphenol AF type diglycidyl ether was 91.1% by mass, the n=1 fraction was 6.2% by mass, and the n=2 fraction was 2.7% by mass.

[0253] The chemical structures of the n=0 to n=2 diglycidyl ethers of bisphenol AF are shown in the following formulas (3) to (5).

[0254] [Chemistry 5]

[0255]

[0256] [Example 1]

[0257] 5g of the bisphenol AF type epoxy resin composition obtained in Synthesis Example 1 was placed in a glass bottle and heated to 120°C to achieve a uniform molten state. After cooling the molten bisphenol AF type epoxy resin composition to a surface temperature of 40°C, 0.05g of crystal nuclei (bisphenol AF type diglycidyl ether of the above formula (3) with a diameter of 8mm or less, which was separately manufactured using the same method as in Example 8 described later) was added (1% by mass relative to the molten bisphenol AF type epoxy resin composition). The mixture was stirred at a speed of 1 rpm using a bamboo stick with a diameter of 2mm to obtain polycrystalline material.

[0258] The crystallization rate at this stage was evaluated, and the melting point, enthalpy of fusion, viscosity, anti-blocking properties, 2θ diffraction peak, full width at half maximum (FWHM), and crystallite size of the obtained polycrystals were also evaluated. The results are shown in Table 1. Furthermore, the powder X-ray diffraction pattern of the obtained polycrystals is shown in Table 1. Figure 1 .

[0259] [Examples 2-9, Comparative Example 1]

[0260] The bisphenol AF type epoxy resin composition obtained in Synthesis Example 1 was separated into n=0, n=1, and n=2 forms of bisphenol AF type diglycidyl ether using silica gel column chromatography. Bisphenol AF type epoxy resin compositions with the composition ratios (mass%) of each component as shown in Table 1 were prepared. It should be noted that the separability was confirmed by GPC.

[0261] 5g of the adjusted composition ratio of the bisphenol AF type epoxy resin composition was placed in a glass bottle and heated to 120°C to achieve a uniform molten state. After cooling the molten bisphenol AF type epoxy resin composition to a surface temperature of 40°C, 0.05g of crystal nuclei (bisphenol AF type diglycidyl ether of the above formula (3) with a diameter of less than 8mm) were added (1% by mass relative to the molten bisphenol AF type epoxy resin composition). The mixture was stirred at 1 rpm using a bamboo stick with a diameter of 2mm, and further allowed to stand at 25°C as needed to obtain polycrystalline material.

[0262] Comparative Example 1 is not polycrystalline, but remains in a liquid molten state (amorphous). The X-ray diffraction pattern of the bisphenol AF type diglycidyl ether obtained in Comparative Example 1 is shown in [image / image / description]. Figure 2 .

[0263] The crystallization rate at this stage was evaluated, and the melting point, enthalpy of fusion, viscosity, anti-adhesion, 2θ diffraction peak, half-maximum width, and crystallite size of the obtained polycrystalline or liquid melt were also evaluated. The results are shown in Table 1.

[0264]

[0265] As shown in Table 1, the bisphenol AF type diglycidyl ether of the present invention, with n≥1 and less than 30% by mass, is polycrystalline, exhibiting rapid crystallization and excellent productivity. Furthermore, it is a crystalline solid with excellent operability, low viscosity, and excellent anti-blocking properties. Additionally, the bisphenol AF type diglycidyl ether polycrystalline materials of Examples 1-9 have high crystallinity, with a full width at half maximum (FWHM) of less than 1.0 at 2θ=26°, thus exhibiting excellent operability, low viscosity, and excellent anti-blocking properties.

[0266] [Reference Example 1]

[0267] Using the bisphenol A type epoxy resin composition shown below, attempt to crystallize as follows.

[0268] <Bisphenol A type epoxy resin composition>

[0269] The substances with the chemical structures shown in formulas (6) to (8) below contain 90% by mass of formula (6) (n=0 units), 9% by mass of formula (7) (n=1 units), and 1% by mass of formula (8) (n=2 units) below, which are bisphenol A type epoxy resin compositions.

[0270] [Chemistry 6]

[0271]

[0272] Take 5g of the above-mentioned bisphenol A type epoxy resin composition into a glass bottle and heat it to 120°C to achieve a uniform molten state. After cooling the molten epoxy resin composition (B) to a surface temperature of 40°C, add 0.05g of crystal nuclei (the n=0 body of the bisphenol A type epoxy resin with the chemical structure of formula (6) above) (1% by mass relative to the molten bisphenol A type epoxy resin composition). Stir with a bamboo stick with a diameter of 2mm at a speed of 1 rpm. However, after stirring for 15 minutes, no crystallization occurred even after standing at 25°C for more than 1 week.

[0273] Although the invention has been described in detail using specific methods, it will be apparent to those skilled in the art that various modifications can be made without departing from the intent and scope of the invention.

[0274] This application is based on Japanese Patent Application 2021-001585, filed on January 7, 2021, the entire contents of which are incorporated herein by reference.

[0275] Industrial availability

[0276] According to the present invention, a bisphenol AF type diglycidyl ether can be provided, which is a crystalline solid with excellent productivity and operability, and has low viscosity and excellent anti-blocking properties.

[0277] The bisphenol AF type diglycidyl ether, curable composition and cured product of the present invention can be applied to various fields such as adhesives, coatings, civil engineering materials, insulating materials for electrical and electronic components, etc., and are particularly useful as insulating injection molding, laminated materials and sealing materials in the electrical and electronic field.

[0278] Examples of uses of the bisphenol AF type diglycidyl ether, curable composition and cured product of the present invention include: multilayer printed circuit boards, laminates for electrical and electronic circuits such as capacitors, adhesives such as film adhesives and liquid adhesives, semiconductor sealing materials, underfill materials, inter-chip fillers for 3D-LSI, insulating materials such as insulating sheets, prepregs, heat dissipation substrates, etc., but are not limited to any of the above.

Claims

1. A bisphenol AF type diglycidyl ether, which is a bisphenol AF type diglycidyl ether represented by the following formula (1), wherein, The proportion of bisphenol AF type diglycidyl ether with n≥1 is less than 30% by mass, and the bisphenol AF type diglycidyl ether is polycrystalline. [Chemistry 1] In equation (1), R 1 ~R 8 Each can independently represent a hydrogen atom, a halogen atom, an alkyl group with 1 to 4 carbon atoms, or an aryl group with 5 to 14 carbon atoms; n is an integer greater than or equal to 0. The melting enthalpy of the bisphenol AF type diglycidyl ether is 20–65 J / g.

2. The bisphenol AF type diglycidyl ether according to claim 1 has a melting point of 50-73°C.

3. The bisphenol AF type diglycidyl ether according to claim 1, wherein, In the bisphenol AF type diglycidyl ether represented by the formula (1), the proportion of bisphenol AF type diglycidyl ether with n=0 is 73% or more by mass and 95.6% or less by mass.

4. A curable composition comprising bisphenol AF type diglycidyl ether as described in any one of claims 1 to 3 and a curing agent.

5. The curable composition according to claim 4, wherein, The curing agent comprises 0.1 to 100 parts by weight of the bisphenol AF type diglycidyl ether relative to 100 parts by weight.

6. The curable composition according to claim 4 or 5, wherein, The curing agent is selected from at least one of phenolic curing agents, amide curing agents, imidazole curing agents, and reactive ester curing agents.

7. A cured product, which is formed by curing the curable composition according to any one of claims 4 to 6.

8. An electrical and electronic component formed using the curable composition according to any one of claims 4 to 6.

9. An insulating material comprising the cured product of claim 7.

10. A laminated board for electrical and electronic circuits, comprising the insulating material as described in claim 9.

11. A method for manufacturing bisphenol AF type diglycidyl ether, comprising a crystallization step, wherein bisphenol AF is reacted with epihaloalcohol in the presence of an alkali, and after obtaining supercooled liquid bisphenol AF type diglycidyl ether from the reaction solution, the supercooled molten bisphenol AF type diglycidyl ether is crystallized. The bisphenol AF type diglycidyl ether is a bisphenol AF type diglycidyl ether represented by the following formula (1), wherein, The proportion of bisphenol AF type diglycidyl ether with n≥1 is less than 30% by mass, and the bisphenol AF type diglycidyl ether is polycrystalline. [Chemistry 1] In equation (1), R 1 ~R 8 Each can independently represent a hydrogen atom, a halogen atom, an alkyl group with 1 to 4 carbon atoms, or an aryl group with 5 to 14 carbon atoms; n is an integer greater than or equal to 0. The melting enthalpy of the bisphenol AF type diglycidyl ether is 20–65 J / g.

12. The method for manufacturing bisphenol AF type diglycidyl ether according to claim 11, wherein, In the bisphenol AF type diglycidyl ether represented by the formula (1), the proportion of bisphenol AF type diglycidyl ether with n=0 is 73% or more by mass and 95.6% or less by mass.

13. The method for manufacturing bisphenol AF type diglycidyl ether according to claim 11 or 12, wherein in the crystallization step, crystal nuclei are mixed and crystallized at a temperature of 0 to 50°C.

14. The method for manufacturing bisphenol AF type diglycidyl ether according to claim 13, wherein, The amount of the crystal nuclei is 0.01 to 5% by mass relative to the molten bisphenol AF type diglycidyl ether.

15. The method for manufacturing bisphenol AF type diglycidyl ether according to claim 11 or 12, wherein in the crystallization step, an external force is applied to the molten bisphenol AF type diglycidyl ether to cause it to crystallize.

16. A bisphenol AF type diglycidyl ether polycrystalline material, wherein the crystallite size calculated from the X-ray diffraction pattern determined by CuKα rays is greater than 10 Å and less than 100,000 Å. The bisphenol AF type diglycidyl ether is a bisphenol AF type diglycidyl ether represented by the following formula (1), wherein, The proportion of bisphenol AF type diglycidyl ether with n≥1 is less than 30% by mass. [Chemistry 1] In equation (1), R 1 ~R 8 Each can independently represent a hydrogen atom, a halogen atom, an alkyl group with 1 to 4 carbon atoms, or an aryl group with 5 to 14 carbon atoms; n is an integer greater than or equal to 0. The melting enthalpy of the bisphenol diglycidyl ether polycrystalline material is 20–65 J / g.

17. The bisphenol AF type diglycidyl ether polycrystalline according to claim 16, wherein the crystallinity is more than 1% and less than 100%.

18. The bisphenol AF type diglycidyl ether polycrystalline material according to claim 16 or 17, having diffraction peaks at diffraction angles of 2θ at 7.9, 16.3, 18.5, 22.3 and 26.0 degrees in the powder X-ray diffraction pattern determined by CuKα rays.

Citation Information

Patent Citations

  • Epoxy resin, method for production thereof, and epoxy resin composition

    JP2013155336A

  • Epoxy resin composition for laminated board, laminated board, and integrated circuit

    JP2013155337A

  • Capacity-type reciprocation pump and cleaning method of capacity-type reciprocation pump

    JP2021001585A

  • Production of low viscosity crystalline epoxy resin

    JP1995179564A

  • Producing method for epoxy resin solid at ordinary temperature

    JP2004043829A