A non-rebound self-adhesive butyl adhesive and its preparation method and application, a high-elongation flexible sealing tape and its preparation method and application
Through the combination of non-rebound self-adhesive butyl glue and high-elongation flexible sealing tape, the problem of poor aging resistance of existing sealing materials at multiple corners and irregular surfaces is solved, achieving good waterproof, high and low temperature resistance and Environmentally friendly, suitable for sealing applications in a variety of special scenarios.
Patent Information
- Application Number
- CN202310842236.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-11
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-07-11
AI Technical Summary
Existing sealing materials have poor aging resistance and are prone to cracking when used on multiple corners and irregular surfaces. Moreover, traditional waterproof sealing methods will release harmful substances to pollute the environment and have poor resistance to high and low temperatures.
Using non-rebound self-adhesive butyl glue and high-elongation flexible sealing tape, through a combination of medium-molecular polyisobutylene, low-molecular polyisobutylene, tackifying resin and other materials, a rubber material with good waterproof, high and low temperature resistance and aging resistance is prepared , and set irregular wrinkles on the adhesive layer and surface layer to improve the sealing effect.
It achieves firm fit and long-term waterproofing effect in special-shaped places, avoids deformation and warping, is environmentally friendly, extensible and permanently self-adhesive, and is suitable for sealing in special places such as multiple corners and irregular surfaces.
Smart Images

Figure CN116751538B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sealing materials, and in particular to a non-rebound self-adhesive butyl rubber and a preparation method and application thereof, and a high-elongation flexible sealing tape and a preparation method and application thereof. Background Art
[0002] At present, the sealing and waterproofing of special places such as corners and irregular surfaces mostly adopt traditional waterproof sealing methods. Traditional sealants can be sealed for a short time, but they have poor aging resistance and will crack after a period of time when exposed to use, thus losing the sealing and waterproofing effect.
[0003] Modified asphalt waterproofing membranes and sealing pastes are mainly made of SBS or random polypropylene modified asphalt, which have certain weather resistance and sealing properties, but they will continue to release harmful substances to pollute the environment during use, and have poor high and low temperature resistance, especially in winter, they will crack and flow in summer. Other membranes with good sealing and waterproofing effects and aging resistance have poor ductility, tracking and aging resistance, and are not good in sealing and waterproofing effects in special places such as corners. Summary of the invention
[0004] The purpose of the present invention is to provide a non-rebound self-adhesive butyl rubber and a preparation method and application thereof, a high-elongation flexible sealing tape and a preparation method and application thereof. The non-rebound self-adhesive butyl rubber provided by the present invention has good waterproof effect, high and low temperature resistance effect and excellent aging resistance effect, and can be more firmly bonded to special-shaped parts without defects such as deformation and warping after bonding.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a non-resilient self-adhesive butyl rubber, which comprises the following preparation raw materials in parts by weight:
[0007] 40 to 60 parts of medium molecular weight polyisobutylene; the number average molecular weight of the medium molecular weight polyisobutylene is 55,000 to 65,000;
[0008] 100 to 130 parts of low molecular weight polyisobutylene; the number average molecular weight of the low molecular weight polyisobutylene is 1300 to 2400;
[0009]
[0010]
[0011] Preferably, the tackifying resin comprises C5 petroleum resin and / or terpene resin; the softening point of the tackifying resin is 100-105°C.
[0012] The present invention provides a method for preparing the non-resilient self-adhesive butyl rubber described in the above technical solution, comprising the following steps:
[0013] The raw materials for preparing the non-resilient self-adhesive butyl rubber are mixed to obtain the non-resilient self-adhesive butyl rubber.
[0014] The present invention provides the use of the non-resilient self-adhesive butyl rubber described in the above technical solution or the non-resilient self-adhesive butyl rubber prepared by the preparation method described in the above technical solution in an adhesive tape.
[0015] The present invention provides a high-elongation flexible sealing tape, comprising an adhesive layer and a surface layer which are stacked in sequence; the adhesive layer is formed by coating the non-resilient self-adhesive butyl rubber described in the above technical solution or the non-resilient self-adhesive butyl rubber prepared by the preparation method described in the above technical solution; the surface layer is a substrate provided with irregular wrinkles.
[0016] Preferably, the irregular wrinkles in the surface layer have a depth of 0.5 to 0.7 mm and a width of 0.7 to 1 mm.
[0017] Preferably, the high-elongation flexible sealing tape further comprises double silicon kraft paper; the double silicon kraft paper and the surface layer are respectively arranged on two sides of the adhesive layer.
[0018] The present invention provides a method for preparing the high-elongation flexible sealing tape described in the above technical solution, comprising the following steps:
[0019] The non-resilient self-adhesive butyl adhesive is coated on double silicon kraft paper, and a surface layer is covered on the surface of the coated non-resilient self-adhesive butyl adhesive layer to obtain a high-elongation flexible sealing tape.
[0020] Preferably, the method for preparing the surface layer includes: using three unequal speed brush rollers to process the substrate into irregular wrinkles; the speed ratio of the three unequal speed brush rollers is 2.4-2.6: 0.9-1.1: 0.8-1.0; the linear speed of the brush roller with a ratio of 0.8-1.0 is 5-10 m / min.
[0021] The present invention provides the use of the high-elongation flexible sealing tape described in the above technical solution or the high-elongation flexible sealing tape prepared by the preparation method described in the above technical solution in wall joints.
[0022] The present invention provides a non-rebound self-adhesive butyl adhesive, in which medium molecular polyisobutylene gives it good waterproof effect and aging resistance effect, low molecular polyisobutylene and cyclohexane oil give it good low temperature resistance effect, and low density polyethylene and polyethylene wax give it good high temperature resistance effect. The non-rebound self-adhesive butyl adhesive provided by the present invention has good waterproof effect, high and low temperature resistance effect and excellent aging resistance effect, and is more firmly attached to special-shaped parts and has no defects such as deformation and warping after attachment.
[0023] The present invention also provides a high-elongation flexible sealing tape, which is an environmentally friendly, elongated, and permanently self-adhesive flexible sealing waterproof tape, and can be used for sealing and waterproofing special-shaped places such as wall joints, around vents, pipe roots, around skylights, and window corners. The results of the embodiment show that the maximum elongation of the high-elongation flexible sealing tape is 200%, and it can be bent and fitted at will, and is particularly suitable for waterproofing special places such as corners and irregular surfaces. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a physical picture of the high elongation flexible sealing tape prepared in Application Example 1;
[0025] Figure 2 This is a schematic diagram of the sealing between the drain pipe and the wall;
[0026] Figure 3 This is a physical picture of the seal between the drain pipe and the wall. DETAILED DESCRIPTION
[0027] The present invention provides a non-resilient self-adhesive butyl rubber, which comprises the following preparation raw materials in parts by weight:
[0028] 40 to 60 parts of medium molecular weight polyisobutylene; the number average molecular weight of the medium molecular weight polyisobutylene is 55,000 to 65,000;
[0029] 100 to 130 parts of low molecular weight polyisobutylene; the number average molecular weight of the low molecular weight polyisobutylene is 1300 to 2400;
[0030]
[0031] In parts by weight, the non-resilient self-adhesive butyl rubber provided by the present invention comprises 40 to 60 parts of medium molecular weight polyisobutylene, preferably 50 parts. In the present invention, the number average molecular weight of the medium molecular weight polyisobutylene is 55,000 to 65,000. In the present invention, the medium molecular weight polyisobutylene can improve the waterproof effect and aging resistance of the non-resilient self-adhesive butyl rubber.
[0032] Based on the weight percentage of the medium molecular weight polyisobutylene, the non-rebound self-adhesive butyl rubber provided by the present invention includes 100 to 130 parts of low molecular weight polyisobutylene, preferably 110 to 120 parts. In the present invention, the number average molecular weight of the low molecular weight polyisobutylene is 1300 to 2400. In the present invention, the low molecular weight polyisobutylene can improve the low temperature resistance and adhesion of the non-rebound self-adhesive butyl rubber.
[0033] Based on the weight of the medium molecular weight polyisobutylene, the non-resilient self-adhesive butyl rubber provided by the present invention includes 20 to 30 parts of naphthenic oil, preferably 20 to 25 parts. In the present invention, the naphthenic oil can improve the low temperature resistance and softness of the non-resilient self-adhesive butyl rubber.
[0034] Based on the weight percentage of the medium molecular weight polyisobutylene, the non-rebound self-adhesive butyl rubber provided by the present invention includes 80 to 100 parts of tackifying resin, preferably 90 to 95 parts. In the present invention, the tackifying resin preferably includes C5 petroleum resin and / or terpene resin; the softening point of the tackifying resin is preferably 100 to 105°C. In the present invention, the tackifying resin can improve the adhesion of the non-rebound self-adhesive butyl rubber.
[0035] Based on the weight percentage of the medium molecular weight polyisobutylene, the non-rebound self-adhesive butyl rubber provided by the present invention includes 300 to 400 parts of filler, preferably 300 to 350 parts. In the present invention, the filler preferably includes one or more of calcium carbonate powder, talcum powder, kaolin, white carbon black and carbon black. In the present invention, the filler can improve the plasticity of the non-rebound self-adhesive butyl rubber and reduce the cost.
[0036] Based on the weight percentage of the medium molecular weight polyisobutylene, the non-rebound self-adhesive butyl rubber provided by the present invention includes 5 to 8 parts of low-density polyethylene (LDPE), preferably 6 to 7 parts. In the present invention, the density of the low-density polyethylene is preferably 0.91 to 0.93 g / cm 3 In the present invention, the low-density polyethylene can improve the high temperature resistance of the non-resilient self-adhesive butyl rubber.
[0037] Based on the weight percentage of the medium molecular weight polyisobutylene, the non-rebound self-adhesive butyl rubber provided by the present invention includes 6 to 10 parts of polyethylene wax, preferably 7 to 8 parts. In the present invention, the melting point of the polyethylene wax is preferably 90 to 110°C; the number average molecular weight of the polyethylene wax is preferably 1500 to 4000. In the present invention, the polyethylene wax can improve the plasticity of the non-rebound self-adhesive butyl rubber.
[0038] Based on the weight percentage of the medium molecular weight polyisobutylene, the non-resilient self-adhesive butyl rubber provided by the present invention includes 1.5 to 2 parts of an antioxidant, preferably 1.5 to 1.8 parts. In the present invention, the antioxidant preferably includes antioxidant 264 and / or antioxidant 1010. In the present invention, the antioxidant can improve the aging resistance and antioxidant properties of the non-resilient self-adhesive butyl rubber.
[0039] The present invention provides a method for preparing the non-resilient self-adhesive butyl rubber described in the above technical solution, comprising the following steps:
[0040] The raw materials for preparing the non-resilient self-adhesive butyl rubber are mixed to obtain the non-resilient self-adhesive butyl rubber.
[0041] In the present invention, the mixing is preferably carried out in a kneader. In the present invention, the mixing is preferably carried out under stirring conditions; the stirring speed is preferably 40 to 50 r / min.
[0042] In the present invention, the mixing preferably includes: first mixing medium molecular polyisobutylene, LDPE, part of filler and part of low molecular polyisobutylene to obtain a first mixture; second mixing the first mixture and polyethylene wax to obtain a second mixture; third mixing the second mixture and tackifying resin to obtain a third mixture; fourth mixing the third mixture and remaining low molecular polyisobutylene and cyclohexane oil to obtain a fourth mixture; fifth mixing the fourth mixture and remaining filler to obtain a fifth mixture; sixth mixing the fifth mixture and antioxidant. In the present invention, the mass of the part of filler is preferably 1 / 4 to 1 / 5 of the total mass of filler, more preferably 1 / 5. In the present invention, the mass of the part of low molecular polyisobutylene is preferably 10% to 15% of the total mass of low molecular polyisobutylene, more preferably 14 to 15%. The temperature of the first mixing is preferably 150 to 170°C, more preferably 160°C; the time of the first mixing is preferably 1 to 1.5h, more preferably 1h. In the present invention, the temperature of the second mixing is preferably 150-160°C; the time of the second mixing is preferably 40-60min, more preferably 40min. In the present invention, the third mixing of the second mixture and the tackifying resin preferably includes: adding the tackifying resin to the second mixture twice on average, each time with an interval of 15min. In the present invention, the temperature of the third mixing is preferably 140-150°C, more preferably 140°C; the present invention preferably stirs for 30min after the tackifying resin is added. In the present invention, the fourth mixing of the third mixture and the remaining low molecular weight polyisobutylene and cyclohexane oil preferably includes: adding the remaining low molecular weight polyisobutylene and cyclohexane oil to the third mixture in sequence. In the present invention, the remaining low molecular weight polyisobutylene and cyclohexane oil are preferably added to the third mixture within 30min. In the present invention, the temperature of the fourth mixing is preferably 110-120°C, more preferably 110°C; the time of the fourth mixing is preferably 1-1.5h, more preferably 1h. In the present invention, the temperature of the fifth mixing is preferably 110-120°C, more preferably 110°C; the time of the fifth mixing is preferably 40-60 min, more preferably 40 min. In the present invention, the temperature of the sixth mixing is preferably 110-120°C; the time of the sixth mixing is preferably 1-1.5 h, more preferably 1 h. The present invention adopts the above mixing method to make the raw materials mixed more uniformly and prevent some materials from being denatured and decomposed during the mixing process, such as polyethylene wax.
[0043] In the present invention, after the raw materials for preparing the non-resilient self-adhesive butyl rubber are mixed, the obtained mixture is preferably extruded through a kneader screw discharge system to obtain the non-resilient self-adhesive butyl rubber. In the present invention, the discharge temperature of the mixture is preferably 110-120°C.
[0044] The present invention provides the use of the non-resilient self-adhesive butyl rubber described in the above technical solution or the non-resilient self-adhesive butyl rubber prepared by the preparation method described in the above technical solution in an adhesive tape.
[0045] The present invention provides a high-elongation flexible sealing tape, comprising an adhesive layer and a surface layer stacked in sequence; the adhesive layer is formed by coating the non-resilient self-adhesive butyl rubber described in the above technical solution or the non-resilient self-adhesive butyl rubber prepared by the preparation method described in the above technical solution; the surface layer is a substrate provided with irregular wrinkles. In the present invention, the substrate is preferably an aluminum foil film, a HDPE film or a polypropylene non-woven fabric. In the present invention, the thickness of the adhesive layer is preferably 0.8 to 1 mm. In the present invention, the thickness of the substrate is preferably 0.05 to 0.15 mm. In the present invention, the depth of the irregular wrinkles in the surface layer is preferably 0.5 to 0.7 mm, and the width is preferably 0.7 to 1 mm. The present invention provides irregular wrinkles on the surface layer, which has a better sealing effect than regular wrinkles.
[0046] In the present invention, the surface layer has good air tightness and UV resistance and aging resistance; the bonding layer has high initial adhesion and is easy to construct, and the non-rebound self-adhesive butyl rubber has good waterproof effect and excellent aging resistance. The non-rebound self-adhesive butyl rubber is more firmly bonded to special-shaped parts and has no deformation, warping, etc. after bonding.
[0047] In the present invention, the high elongation flexible sealing tape preferably further comprises double silicon kraft paper; the double silicon kraft paper and the surface layer are respectively arranged on both sides of the adhesive layer. In a specific embodiment of the present invention, the high elongation flexible sealing tape comprises double silicon kraft paper, an adhesive layer and a surface layer which are stacked in sequence.
[0048] The present invention also provides a method for preparing the high-elongation flexible sealing tape described in the above technical solution, comprising the following steps:
[0049] The non-resilient self-adhesive butyl adhesive is coated on double silicon kraft paper, and a surface layer is covered on the surface of the coated non-resilient self-adhesive butyl adhesive layer to obtain a high-elongation flexible sealing tape.
[0050] In the present invention, the coating thickness of the non-resilient self-adhesive butyl rubber is preferably 0.8-1 mm. In the present invention, the coating temperature is preferably 120-130°C. In the present invention, the surface layer is a substrate provided with irregular wrinkles; the preparation method of the surface layer preferably includes: processing the substrate into irregular wrinkles using three unequal speed brush rollers. In the present invention, the speed ratio of the three unequal speed brush rollers is preferably 2.4-2.6:0.9-1.1:0.8-1.0, more preferably 2.5:1:0.9; the linear speed of the brush roller with a ratio of 0.8-1.0 is preferably 5-10 m / min.
[0051] In a specific embodiment of the present invention, the non-resilient self-adhesive butyl rubber is coated on double silicon kraft paper, and a release film is covered on the surface of the coated non-resilient self-adhesive butyl rubber layer, and the non-resilient self-adhesive butyl rubber layer is rolled up; after removing the release film, the non-resilient self-adhesive butyl rubber layer is laminated to the surface layer using a composite roller to obtain a high elongation flexible sealing tape. In the present invention, the release film is preferably a PE release film; the thickness of the release film is preferably 4 to 4.5 filaments. In the present invention, the release film is relatively soft.
[0052] In the present invention, the high elongation flexible sealing tape is preferably cut and packaged as required, with a width of preferably 8 to 10 cm and a length of preferably 5 to 10 m.
[0053] The present invention also provides the use of the high elongation flexible sealing tape described in the above technical solution or the high elongation flexible sealing tape prepared by the preparation method described in the above technical solution in the wall joint, preferably used for sealing the joint between the pipe and the wall. In the present invention, the pipe preferably includes a ventilation pipe or a drainage pipe; the pipe preferably includes a plastic pipe, a cement pipe or a metal pipe. In the present invention, the composition of the wall preferably includes concrete or brick. In the present invention, the joint is preferably a corner.
[0054] The high-elongation flexible sealing tape provided by the present invention has the advantages of simple construction, environmental protection, and the ability to be bent and fitted at will, and is particularly suitable for waterproof sealing in special places such as multiple corners and irregular surfaces.
[0055] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0056] Example 1
[0057] By weight, 50 parts of medium molecular weight polyisobutylene (number average molecular weight of 65,000), 6 parts of LDPE (density of 0.93 g / cm 3), 70 parts of filler (calcium carbonate powder) and 15 parts of low molecular weight polyisobutylene (number average molecular weight of 1300) were added to the kneader, heated to 160°C, kneaded for 1 hour, then 8 parts of polyethylene wax (melting point of 90°C) were added, the temperature was maintained at 160°C, kneaded for 40 minutes, cooled to 140°C, 90 parts of tackifying resin (C5 petroleum resin) were added to the kneader twice, each time with an interval of 15 minutes, and 95 20 parts of low molecular weight polyisobutylene (number average molecular weight is 1300) and 20 parts of cyclohexane oil are added within 30 minutes and stirred for 1 hour. 280 parts of filler (calcium carbonate powder) are added to the kneader and stirred for 40 minutes, then cooled to 110°C. 1.5 parts of antioxidant 1010 are added to the kneader and stirred for 1 hour. The temperature is maintained at 110°C and extruded through the kneader screw discharge system to obtain non-rebound self-adhesive butyl rubber, which is packaged with double-sided anti-sticking PET film for standby use.
[0058] Application Example 1
[0059] The non-resilient self-adhesive butyl rubber prepared in Example 1 was coated onto double silicon kraft paper with a butyl rubber special coating machine to a thickness of 1 mm, and a PE anti-adhesive film (thickness of 0.04 mm) was covered on the non-resilient self-adhesive butyl rubber, and the coating machine temperature was controlled at 120° C. for standby use;
[0060] The substrate (non-woven fabric with a gram weight of 100 g) is processed into irregular wrinkles by three unequal speed brush rollers, the speed ratio of the three brush rollers is 2.5:1:0.9, and the linear speed of the brush roller with a ratio of 0.9 is 10 m / min to obtain a surface layer; the PE anti-sticking film on the non-resilient self-adhesive butyl rubber is removed, and the coated non-resilient self-adhesive butyl rubber layer is compounded to the surface layer by a compounding roller to obtain a high-elongation flexible sealing tape.
[0061] Test Case
[0062] (1) The high elongation flexible sealing tape prepared in Example 1 is as follows Figure 1 As shown, it is composed of double silicon kraft paper, an adhesive layer and a surface layer which are stacked in sequence; the adhesive layer is a non-rebound self-adhesive butyl rubber layer; and the surface layer is a substrate with irregular wrinkles.
[0063] The surface layer of the present invention is made of irregular wrinkle substrate as the main material, so that it has high elongation, excellent weather resistance and aging resistance, and excellent sealing and waterproofing effect. The irregular wrinkle substrate has high ductility and extensibility, and has good tracking performance. The adhesive layer is made of non-rebound self-adhesive butyl rubber, which has excellent aging resistance, good waterproof sealing effect, permanent self-adhesion, firm bonding, and easy construction.
[0064] (2) The properties of the high elongation flexible sealing tape prepared in Application Example 1 are shown in Table 1.
[0065] Table 1 Properties of high elongation flexible sealing tape prepared in Application Example 1
[0066]
[0067]
[0068] It can be seen from Table 1 that the high elongation flexible sealing tape provided by the present invention has good heat resistance, low temperature bending property, long-lasting adhesion and high peel strength.
[0069] (3) Take the sealing of drainage pipe and wall as an example. Figures 2-3 As shown, the high-elongation flexible sealing tape prepared in Application Example 1 was used to seal the joints between drainage pipes of different diameters and walls, and the effects are shown in Table 2.
[0070] Table 2 The sealing effect of drainage pipe and wall
[0071]
[0072] In Table 2, × represents that the entire system cannot be sealed, and √ represents that the entire system can be sealed.
[0073] As can be seen from Table 2, the high elongation flexible sealing tape provided by the present invention has good ductility and can adapt to various arc-shaped or anisotropic component parts. The high elongation flexible sealing tape of the present invention is easy to construct and can be formed in one step, saving more than 50% of the construction time; it has good waterproofness and can adapt to different structures, and is effectively waterproof for a long time; it has good durability, and the non-rebound self-adhesive butyl adhesive has good weather resistance, and the product has excellent durability, is beautiful and pollution-free.
[0074] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A high-elongation flexible sealing tape, comprising an adhesive layer and a surface layer stacked in sequence; the adhesive layer is formed by coating a non-resilient self-adhesive butyl rubber; the surface layer is a substrate provided with irregular wrinkles; The non-resilient self-adhesive butyl rubber is prepared from the following raw materials in parts by weight: 40 to 60 parts of medium molecular weight polyisobutylene; the number average molecular weight of the medium molecular weight polyisobutylene is 55,000 to 65,000; 100 to 130 parts of low molecular weight polyisobutylene; the number average molecular weight of the low molecular weight polyisobutylene is 1300 to 2400; 2. The high elongation flexible sealing tape according to claim 1, characterized in that: The tackifying resin includes C5 petroleum resin and / or terpene resin; the softening point of the tackifying resin is 100-105°C.
3. The high elongation flexible sealing tape according to any one of claims 1 to 2, characterized in that: The preparation method of the non-resilient self-adhesive butyl rubber comprises the following steps: The raw materials for preparing the non-resilient self-adhesive butyl rubber are mixed to obtain the non-resilient self-adhesive butyl rubber.
4. The high elongation flexible sealing tape according to claim 1, characterized in that: The irregular wrinkles in the surface layer have a depth of 0.5 to 0.7 mm and a width of 0.7 to 1 mm.
5. The high elongation flexible sealing tape according to claim 1, characterized in that: The high-elongation flexible sealing tape also includes double silicon kraft paper; the double silicon kraft paper and the surface layer are respectively arranged on two sides of the adhesive layer.
6. The method for preparing the high elongation flexible sealing tape according to any one of claims 1 to 5, comprising the following steps: The non-resilient self-adhesive butyl adhesive is coated on double silicon kraft paper, and a surface layer is covered on the surface of the coated non-resilient self-adhesive butyl adhesive layer to obtain a high-elongation flexible sealing tape.
7. The preparation method according to claim 6, characterized in that: The preparation method of the surface layer comprises: processing the substrate into irregular wrinkles by using three unequal speed brush rollers; the speed ratio of the three unequal speed brush rollers is 2.4-2.6: 0.9-1.1: 0.8-1.0; the linear speed of the brush roller with a ratio of 0.8-1.0 is 5-10 m / min.
8. Use of the high elongation flexible sealing tape according to any one of claims 1 to 5 or the high elongation flexible sealing tape prepared by the preparation method according to any one of claims 6 to 7 in wall joints.