A method for introducing trace sulfur into smelting process materials
By first melting the ingot pre-alloy and pyrite powder during the smelting process, multiple analyzes and adjustments were made to solve the problem of difficult to accurately control the introduction of trace amounts of sulfur, achieve efficient sulfur content control, and reduce volatilization and costs. .
Patent Information
- Application Number
- CN202310722661.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-19
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-06-19
AI Technical Summary
In special scenarios such as copper anodes and nickel anodes for electroplating, the introduction of trace amounts of sulfur is difficult to accurately control. Existing methods are difficult to effectively solve when the PPM level of sulfur content is required, especially in a narrow range within tens of PPM. Conventional methods Difficult to control precisely.
By first melting the ingot pre-alloy to determine the proportion of sulfur element burning, grind the raw pyrite into powder, vibrate it evenly and then add the material a second time. Combined with the high-frequency furnace and smelting aids, multiple analyzes and adjustments are made to ensure that the sulfur element is lost. The precise elemental content reaches the target.
It achieves precise control of the introduction of trace sulfur elements into the smelting process materials, reduces the volatilization and cost of sulfide, and improves the accuracy and efficiency of production.
Smart Images

Figure CN116770121B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of target material manufacturing, and in particular to a method for introducing trace sulfur elements into smelting process materials. Background Art
[0002] In some special use scenarios, such as copper anodes and nickel anodes for electroplating, the materials are often required to contain trace amounts of sulfur, usually 10 to 1000 ppm (parts per million). However, the melting point of sulfur is only 112.8°C, which is thousands of degrees Celsius higher than the melting points of copper (1803.4°C) and nickel (1453°C). When the metal melts, the sulfur has already volatilized severely, resulting in exceeding the target specifications.
[0003] During the production process, volatile elements are often added at the batching stage, that is, volatile elements are compensated, and then smelted together with other metal materials. However, this method is only applicable to conditions with high volatile element content (at%>0.5%). When the sulfur content is required to be at the PPM level, especially in a very narrow range of tens of PPM, it is difficult to control it with conventional methods. Summary of the invention
[0004] In view of the problems mentioned in the background technology, the purpose of the present invention is to provide a method for introducing trace sulfur elements into smelting process materials to solve the problems mentioned in the background technology.
[0005] The above technical objectives of the present invention are achieved through the following technical solutions:
[0006] A method for introducing trace sulfur into smelting process materials comprises the following steps: firstly, smelting an ingot pre-alloy to determine the sulfur burnout ratio, grinding and powdering the pyrite raw material, vibrating it evenly, taking a certain weight of the powder, mixing it with a certain amount of single material or alloy material, smelting it, analyzing the sulfur content of the obtained ingot to determine the sulfur content of the first smelting; in the smelting process, the powder is fed for a second time, and then, according to the sulfur content of the pre-alloy, the weight of the single material or alloy material required by the target material is mixed for smelting, and then the sulfur content is analyzed again to confirm.
[0007] Preferably, the method comprises the following steps:
[0008] S1. Primary batching: prepare 10-20 kg of pyrite and grind it into powder. After vibration and homogenization, take 4-8 g of powder, and then prepare 10-20 kg of single material or alloy material for standby use;
[0009] S2. Melting pre-alloy: Put the single material or alloy material into the crucible for melting, put the pyrite powder into the secondary feeding device, wait for the single material or alloy material to form a molten soup and then feed it, and melt to obtain the pre-alloy;
[0010] S3. Sulfur element detection: Pre-alloy sampling is performed to analyze the sulfur content and confirm that the sulfur content is 0.01wt%;
[0011] S4. Secondary batching: prepare 40-60g of pyrite powder, 100-120kg of single material or alloy material, and the surface of the raw materials must be clean;
[0012] S5. Smelting the target alloy: putting the raw single substance material or alloy material into the crucible for smelting, putting the pyrite powder into the secondary feeding device, and then feeding the single substance material or alloy material into the secondary feeding device after the single substance material or alloy material forms a molten soup, and smelting to obtain the target alloy;
[0013] S6. Sulfur element detection and confirmation: Component analysis was performed and the sulfur content was found to be 0.01 wt%.
[0014] Preferably, the surface of the single substance or alloy material in S1 needs to be cleaned before use.
[0015] Preferably, when smelting S2, the selected melting furnace is a high frequency furnace, and a smelting aid is added during smelting.
[0016] Preferably, when detecting sulfur element, S3 uses a sampling gun to take samples, so that the sampling end of the sampling gun is immersed in the molten metal, the molten metal enters the inner cavity of the sampling gun through the sampling end and flows into the condensation end, and then the piston rod of the oil cylinder is started to press down the mold frame and drive the contour cutter to cut and sample.
[0017] Preferably, when the S6 is used to detect and confirm the sulfur element, the method for component analysis is as follows: the sample is melted by high-frequency induction heating under a flux and an oxygen flow to generate sulfur dioxide, and a manned infrared detector is used to measure the mass of carbon and sulfur based on the change in the infrared light energy of a specific wavelength absorbed by the measured gas.
[0018] In summary, the present invention mainly has the following beneficial effects:
[0019] The purpose of the present invention is to provide a method for introducing trace sulfur into smelting process materials. The principle is as follows: first, a small ingot is smelted to pre-alloy and determine the sulfur burn-out ratio. The pyrite raw material is ground and powdered, and after vibrating evenly, a certain weight of powder is taken, and a certain amount of single material or alloy material is mixed for smelting. The obtained ingot is analyzed for sulfur content to determine the content of sulfur in the first smelting. In this smelting process, the powder needs to be fed twice. Then, according to the pre-alloy sulfur content, the weight of single material or alloy material required by the target material is mixed for smelting. Then analyze and confirm the sulfur content again. This is due to the high melting point of pyrite ore, which is not easy to volatilize. Secondly, the secondary feeding shortens the smelting time of sulfide and reduces the volatilization amount. Therefore, the sulfur content of the obtained target material is very accurate. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION
[0021] The present invention is described in detail below in conjunction with the accompanying drawings and embodiments.
[0022] Example 1
[0023] A method for introducing trace sulfur into smelting process materials comprises the following steps: firstly, smelting a small ingot pre-alloy to determine the sulfur burnout ratio, grinding and powdering the pyrite raw material, vibrating it evenly, taking a certain weight of the powder, mixing it with a certain amount of single material or alloy material, smelting it, analyzing the sulfur content of the obtained ingot to determine the sulfur content of the first smelting; in the smelting process, the powder is fed for a second time, and then, according to the sulfur content of the pre-alloy, the weight of the single material or alloy material required by the target material is mixed for smelting, and then the sulfur content is analyzed again to confirm.
[0024] Specifically, the following steps are included:
[0025] S1. Primary batching: prepare 10-20 kg of pyrite and grind it into powder. After vibration and homogenization, take 4-8 g of powder, and then prepare 10-20 kg of single material or alloy material for standby use;
[0026] S2. Melting pre-alloy: Put the single material or alloy material into the crucible for melting, put the pyrite powder into the secondary feeding device, wait for the single material or alloy material to form a molten soup and then feed it, and melt to obtain the pre-alloy;
[0027] S3. Sulfur element detection: Pre-alloy sampling is performed to analyze the sulfur content and confirm that the sulfur content is 0.01wt%;
[0028] S4. Secondary batching: prepare 40-60g of pyrite powder, 100-120kg of single material or alloy material, and the surface of the raw materials must be clean;
[0029] S5. Smelting the target alloy: putting the raw single substance material or alloy material into the crucible for smelting, putting the pyrite powder into the secondary feeding device, and then feeding the single substance material or alloy material into the secondary feeding device after the single substance material or alloy material forms a molten soup, and smelting to obtain the target alloy;
[0030] S6. Sulfur element detection and confirmation: Component analysis was performed and the sulfur content was 0.01 wt%.
[0031] The surface of the single substance or alloy material in S1 needs to be cleaned before use.
[0032] Among them, when S2 is smelted, the selected melting furnace is a high-frequency furnace, and a smelting aid is added during smelting.
[0033] Among them, when S3 detects sulfur elements, a sampling gun is used for sampling, and the sampling end of the sampling gun is immersed in the molten metal. The molten metal enters the inner cavity of the sampling gun through the sampling end and flows into the condensation end. Then the piston rod of the oil cylinder is started to press down the mold frame and drive the contour cutter to cut and sample.
[0034] Among them, the method used for component analysis of S6 when confirming the sulfur element detection is: the sample is melted by high-frequency induction heating under a flux and oxygen flow to generate sulfur dioxide, and a manned infrared detector is used to measure the mass of carbon and sulfur based on the change in the infrared light energy of a specific wavelength absorbed by the measured gas.
[0035] The purpose of the present invention is to provide a method for introducing trace sulfur into smelting process materials, based on the following principles. First, a small ingot is smelted to pre-alloy and determine the sulfur burn-out ratio. The pyrite raw material is ground and powdered, and after vibrating evenly, a certain weight of powder is taken, and a certain amount of single material or alloy material is mixed for smelting. The obtained ingot is analyzed for sulfur content to determine the sulfur content of the first smelting. In this smelting process, the powder needs to be fed twice. Based on the pre-alloyed sulfur content, the weight of single material or alloy material required by the target material is mixed for smelting. Then analyze and confirm the sulfur content again. This is due to the high melting point of pyrite ore, which is not easy to volatilize. Secondly, the secondary feeding shortens the smelting time of the sulfide and reduces the volatilization amount. Therefore, the sulfur content of the obtained target material is very accurate.
[0036] Example 2
[0037] A method for introducing trace sulfur into smelting process materials comprises the following steps: firstly, smelting a small ingot pre-alloy to determine the sulfur burnout ratio, grinding and powdering the pyrite raw material, vibrating it evenly, taking a certain weight of the powder, mixing it with a certain amount of single material or alloy material, smelting it, analyzing the sulfur content of the obtained ingot to determine the sulfur content of the first smelting; in the smelting process, the powder is fed for a second time, and then, according to the sulfur content of the pre-alloy, the weight of the single material or alloy material required by the target material is mixed for smelting, and then the sulfur content is analyzed again to confirm.
[0038] Specifically, the following steps are included:
[0039] S1. Primary batching: prepare 10-20 kg of pyrite and grind it into powder. After vibration and homogenization, take 4-8 g of powder, and then prepare 10-20 kg of single material or alloy material for standby use;
[0040] S2. Melting pre-alloy: Put the single material or alloy material into the crucible for melting, put the pyrite powder into the secondary feeding device, wait for the single material or alloy material to form a molten soup and then feed it, and melt to obtain the pre-alloy;
[0041] S3. Sulfur element detection: Pre-alloy sampling is performed to analyze the sulfur content and confirm that the sulfur content is 0.01wt%;
[0042] S4. Secondary batching: prepare 40-60g of pyrite powder, 100-120kg of single material or alloy material, and the surface of the raw materials must be clean;
[0043] S5. Smelting the target alloy: putting the raw single substance material or alloy material into the crucible for smelting, putting the pyrite powder into the secondary feeding device, and then feeding the single substance material or alloy material into the secondary feeding device after the single substance material or alloy material forms a molten soup, and smelting to obtain the target alloy;
[0044] S6. Sulfur element detection and confirmation: Component analysis was performed and the sulfur content was 0.01 wt%.
[0045] The surface of the single substance material or alloy material in S1 needs to be cleaned before use.
[0046] Among them, when S2 is smelted, the selected melting furnace is a high-frequency furnace, and a smelting aid is added during smelting.
[0047] Among them, when S3 detects sulfur elements, a sampling gun is used for sampling, and the sampling end of the sampling gun is immersed in the molten metal. The molten metal enters the inner cavity of the sampling gun through the sampling end and flows into the condensation end. Then the piston rod of the oil cylinder is started to press down the mold frame and drive the contour cutter to cut and sample.
[0048] Among them, the method used for component analysis of S6 when confirming the sulfur element detection is: the sample is melted by high-frequency induction heating under a flux and oxygen flow to generate sulfur dioxide, and a manned infrared detector is used to measure the mass of carbon and sulfur based on the change in the infrared light energy of a specific wavelength absorbed by the measured gas.
[0049] Example 3
[0050] refer to Figure 1 A method for introducing trace sulfur into smelting process materials comprises the following steps: firstly, smelting a small ingot pre-alloy to determine the sulfur burnout ratio, grinding and powdering the pyrite raw material, vibrating it evenly, taking a certain weight of the powder, mixing it with a certain amount of single material or alloy material, smelting it, analyzing the sulfur content of the obtained ingot to determine the sulfur content of the first smelting; in the smelting process, the powder is fed for a second time, and then according to the sulfur content of the pre-alloy, the weight of the single material or alloy material required by the target material is mixed for smelting, and then the sulfur content is analyzed again.
[0051] Specifically, the following steps are included:
[0052] S1. Primary batching: prepare 10-20 kg of pyrite and grind it into powder. After vibration and homogenization, take 4-8 g of powder, and then prepare 10-20 kg of single material or alloy material for standby use;
[0053] S2. Melting pre-alloy: Put the single material or alloy material into the crucible for melting, put the pyrite powder into the secondary feeding device, wait for the single material or alloy material to form a molten soup and then feed it, and melt to obtain the pre-alloy;
[0054] S3. Sulfur element detection: Pre-alloy sampling is performed to analyze the sulfur content and confirm that the sulfur content is 0.01wt%;
[0055] S4. Secondary batching: prepare 40-60g of pyrite powder, 100-120kg of single material or alloy material, and the surface of the raw materials must be clean;
[0056] S5. Smelting the target alloy: putting the raw single substance material or alloy material into the crucible for smelting, putting the pyrite powder into the secondary feeding device, and then feeding the single substance material or alloy material into the secondary feeding device after the single substance material or alloy material forms a molten soup, and smelting to obtain the target alloy;
[0057] S6. Sulfur element detection and confirmation: Component analysis was performed and the sulfur content was 0.01 wt%.
[0058] The surface of the single substance material or alloy material in S1 needs to be cleaned before use.
[0059] Among them, when S2 is smelted, the selected melting furnace is a high-frequency furnace, and a smelting aid is added during smelting.
[0060] Among them, when S3 detects sulfur elements, a sampling gun is used for sampling, and the sampling end of the sampling gun is immersed in the molten metal. The molten metal enters the inner cavity of the sampling gun through the sampling end and flows into the condensation end. Then the piston rod of the oil cylinder is started to press down the mold frame and drive the contour cutter to cut and sample.
[0061] Among them, the method used for component analysis of S6 when confirming the sulfur element detection is: the sample is melted by high-frequency induction heating under a flux and oxygen flow to generate sulfur dioxide, and a manned infrared detector is used to measure the mass of carbon and sulfur based on the change in the infrared light energy of a specific wavelength absorbed by the measured gas.
[0062] In order to verify the superiority of the present invention, the following experiments were performed:
[0063] First, the comparative document and Example 1, Example 2, and Example 3 are selected for comparison. The comparative document is a conventional sulfur addition method; the experimental contents and results are as follows:
[0064]
[0065] Through various experiments, it can be found that Example 1, Example 2, and Example 3 are more convenient and quick when introducing trace sulfur elements into smelting process materials, and less sulfur is consumed and less sulfur escapes.
[0066] In addition, according to actual production statistics, the following results are obtained:
[0067] The experimental contents and results are shown in the following table:
[0068]
[0069] Through various experiments, it can be found that the production processes of Example 1, Example 2, Example 3, and Example 4 have lower various cost consumption and lower carbon emissions.
[0070] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. A method for introducing trace sulfur into smelting process materials, characterized in that: The following steps are involved: First, an ingot is smelted to pre-alloy and determine the sulfur burnout ratio. The pyrite raw material is ground and powdered. After vibrating evenly, a certain weight of powder is taken and mixed with a certain amount of single material or alloy material for smelting. The sulfur content of the obtained ingot is analyzed to determine the sulfur content of the first smelting. During the smelting process, the powder is fed a second time, and then according to the sulfur content of the pre-alloy, the weight of single material or alloy material required by the target material is mixed for smelting, and then the sulfur content is analyzed again. The specific steps include: S1. Primary batching: prepare 10-20 kg of pyrite and grind it into powder. After vibration and homogenization, take 4-8 g of powder, and then prepare 10-20 kg of single material or alloy material for standby use; S2. Melting pre-alloy: Put the single material or alloy material into the crucible for melting, put the pyrite powder into the secondary feeding device, wait for the single material or alloy material to form a molten soup and then feed it, and melt to obtain the pre-alloy; S3. Sulfur element detection: Pre-alloy sampling, sulfur element content analysis, confirm that the sulfur content is 0.01wt%; S4. Secondary batching: prepare 40-60g of pyrite powder, 100-120kg of single material or alloy material, and the surface of the raw materials must be clean; S5. Smelting the target alloy: putting the raw single substance material or alloy material into the crucible for smelting, putting the pyrite powder into the secondary feeding device, and then feeding the single substance material or alloy material into the secondary feeding device after the single substance material or alloy material forms a molten soup, and smelting to obtain the target alloy; S6. Sulfur element detection and confirmation: Component analysis was performed and the sulfur content was 0.01wt%.
2. A method for introducing trace sulfur into smelting process materials according to claim 1, characterized in that: The surface of the single substance material or alloy material in S1 needs to be cleaned before use.
3. A method for introducing trace sulfur into smelting process materials according to claim 1, characterized in that: When S2 is smelted, the selected melting furnace is a high frequency furnace, and a smelting aid is added during smelting.
4. The method for introducing trace sulfur into smelting process materials according to claim 1, characterized in that: When detecting sulfur element, S3 adopts sampling gun to take samples, immerses the sampling end of the sampling gun into molten metal, and the molten metal enters the inner cavity of the sampling gun through the sampling end and flows into the condensation end, then starts the piston rod of the oil cylinder to press down the die frame and drive the contour cutter to cut and take samples.
5. The method for introducing trace sulfur into smelting process materials according to claim 1, characterized in that: When the S6 is used to detect and confirm the sulfur element, the method used for component analysis is as follows: the sample is melted by high-frequency induction heating under a flux and an oxygen flow to generate sulfur dioxide, and an infrared detector is used to measure the mass of carbon and sulfur based on the change in the infrared light energy of a specific wavelength absorbed by the measured gas.