A composite negative electrode material and preparation method thereof and sodium ion battery

By using acid-base neutralization reaction in the hard carbon anode material of sodium ion battery, the problem of low efficiency of the hard carbon anode material of sodium ion battery is solved, and the energy density and Conductive performance reduces production costs.

CN116826003BActive Publication Date: 2024-11-26成都佰思格科技有限公司 +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310894973.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-20
Publication Date
2024-11-26
Estimated Expiration
2043-07-20

AI Technical Summary

Technical Problem

The first-time efficiency of the hard carbon anode material of sodium ion batteries is low, resulting in a small energy density and cannot be compared with lithium ion batteries.

Method used

Using a method of preparing composite negative electrode material, by mixing alkali metal sulfide with hard carbon precursor powder evenly in water, adding polymetallic acid to conduct acid-base neutralization reaction, to form polymetallic acid salt adhered to hard carbon material Inside, thereby improving sodium ion transport efficiency.

Benefits of technology

Through the three-dimensional pore structure of polyoxylate, the porosity and active sites of the composite anode material are improved, the first efficiency and conductive properties of the hard carbon anode material of sodium ion battery are significantly improved, and the production cost is reduced.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a composite negative electrode material and a preparation method thereof and a sodium ion battery, which relates to the technical field of sodium ion batteries. The preparation method comprises the following steps: uniformly mixing an alkali metal sulfide and a hard carbon precursor powder in water to obtain a mixed solution; adding a polyoxometalate to the mixed solution under stirring conditions to obtain a solid-liquid mixture; separating the solid matter in the solid-liquid mixture, vacuum drying and grinding the solid matter to obtain a precursor composite material; calcining the precursor composite material under an inert gas atmosphere to obtain a composite negative electrode material. The preparation method of the composite negative electrode material provided by the present invention generates a polyoxometalate in situ in a mixed solution containing a hard carbon precursor powder, so that the polyoxometalate is attached to the functional groups in the hard carbon precursor powder, and then utilizes the special three-dimensional pore structure of the polyoxometalate ions to facilitate the sodium ions to be deintercalated in the composite negative electrode material, thereby improving the initial efficiency of the composite negative electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a composite negative electrode material and a preparation method thereof, and a sodium ion battery. Background Art

[0002] Lithium-ion batteries are the representative of green electrochemical power sources, and are mainly divided into three categories: 3C batteries, power batteries, and energy storage batteries. However, due to the global shortage of lithium resources, the cost of lithium resources is relatively high. In this environment, sodium-ion batteries came into being. Sodium-ion batteries have received widespread attention in recent years because there are sufficient sodium resources in the world, there will be no price problem of lithium resources, and sodium-ion batteries are safer than lithium-ion batteries.

[0003] However, the negative electrode materials of sodium-ion batteries are not as abundant as those of lithium-ion batteries. The currently well-known and commercially available negative electrode material is hard carbon. Compared with traditional graphite negative electrode materials, the defects of hard carbon negative electrode materials are lower gram capacity, generally less than 300mAh / g, and lower first efficiency, generally around 85%. Compared with lithium-ion batteries, sodium-ion batteries prepared from hard carbon have lower energy density. Therefore, improving the first efficiency of hard carbon negative electrode materials for sodium-ion batteries has become a key issue in hard carbon research. Summary of the invention

[0004] The technical problem to be solved by the present invention is: in order to solve the problem of low initial efficiency of hard carbon negative electrode materials for sodium ion batteries in the prior art, the present invention provides a method for preparing a composite negative electrode material. The preparation method uses sodium sulfide, polyoxometalate and hard carbon precursor as raw materials to obtain a composite negative electrode material in which sodium polyoxometalate sodium salt is attached to the inside of the hard carbon material, so that sodium ions can be transported inside the polyoxometalate roots and in the hard carbon micropores, thereby improving the initial efficiency of the hard carbon negative electrode material for the sodium ion battery, and solving the problem of low initial efficiency of the hard carbon negative electrode material for the sodium ion battery in the prior art.

[0005] The technical solution adopted by the present invention to solve its technical problem is:

[0006] A method for preparing a composite negative electrode material comprises the following steps:

[0007] S1: uniformly mixing alkali metal sulfide and hard carbon precursor powder in water to obtain a mixed solution;

[0008] S2: adding polyoxometallic acid to the mixed solution under stirring conditions to obtain a solid-liquid mixture;

[0009] S3: separating the solid matter from the solid-liquid mixture, vacuum drying and grinding the solid matter to obtain a precursor composite material;

[0010] S4: calcining the precursor composite material under an inert gas atmosphere to obtain a composite negative electrode material.

[0011] Optionally, the polyoxometallic acid is selected from H3XY 12 O 40 、H4XY 12 O 40 At least one of; wherein X is selected from any one of P and Si; Y is selected from any one of Mo and W.

[0012] Optionally, the alkali metal sulfide is sodium sulfide.

[0013] Optionally, the hard carbon precursor is selected from at least one of bamboo, coconut shell, starch, walnut shell, anthracite, asphalt, and phenolic resin.

[0014] Optionally, the starch is selected from at least one of potato starch, corn starch, wheat starch, tapioca starch, pea starch and sweet potato starch.

[0015] Optionally, the molar ratio of the alkali metal sulfide to the polyoxometallic acid is 1:(2-3).

[0016] Optionally, the mass ratio of the alkali metal sulfide to the hard carbon precursor powder is 1:(8-10).

[0017] Optionally, calcining the precursor composite material under an inert gas atmosphere comprises: calcining the precursor composite material at 100-300° C. for 3-6 hours, and then calcining at 850-1400° C. for 4-6 hours under an inert gas atmosphere.

[0018] Another object of the present invention is to provide a composite negative electrode material prepared by the method for preparing the composite negative electrode material as described above.

[0019] Another object of the present invention is to provide a sodium ion battery comprising the composite negative electrode material as described above.

[0020] The beneficial effects of the present invention are:

[0021] The preparation method of the composite negative electrode material provided by the present invention generates polyoxometalates in situ in a mixed solution containing hard carbon precursor powder, so that the polyoxometalates are attached to functional groups in the hard carbon precursor powder, and then utilizes the special three-dimensional pore structure of the polyoxometalate ions to facilitate the embedding and deintercalation of sodium ions in the composite negative electrode material, thereby improving the initial efficiency of the composite negative electrode material. DETAILED DESCRIPTION

[0022] The present invention is now further described in detail. The embodiments described below are exemplary and intended to be used to explain the present invention, but cannot be understood as limiting the present invention. All other embodiments obtained by ordinary technicians in this field without creative work based on the embodiments of the present invention belong to the scope of protection of the present invention.

[0023] In order to solve the problem of low initial efficiency of hard carbon negative electrode materials for sodium ion batteries in the prior art, the present invention provides a method for preparing a composite negative electrode material, which comprises the following steps:

[0024] S1: uniformly mixing alkali metal sulfide and hard carbon precursor powder in water to obtain a mixed solution;

[0025] S2: adding the polyoxometallic acid to the mixed solution under stirring conditions to obtain a solid-liquid mixture;

[0026] S3: separating the solid matter from the solid-liquid mixture, vacuum drying and grinding the solid matter to obtain a precursor composite material;

[0027] S4: calcining the precursor composite material under an inert gas atmosphere to obtain a composite negative electrode material.

[0028] Specifically, the preferred step S1 of the present invention includes: crushing the hard carbon precursor to obtain hard carbon precursor powder; using deionized water as a solvent, first adding the hard carbon precursor powder into the deionized water, and then adding alkali metal sulfide into the deionized water containing the hard carbon precursor powder, and stirring while adding to evenly mix the hard carbon precursor powder and the alkali metal sulfide to obtain a mixed solution.

[0029] Further, polyoxometalate is added into the mixed solution, and stirring is performed while adding, so that sodium sulfide and polyoxometalate are in full contact, and an acid-base neutralization reaction occurs after the two come into contact, generating polyoxometalate and hydrogen sulfide. Since polyoxometalate has strong oxidizing property and strong electron-withdrawing ability, and the hard carbon precursor contains abundant functional groups, the polyoxometalate generated by the reaction is in situ attached to the functional groups in the hard carbon precursor, so that the composite negative electrode material obtained after calcination includes hard carbon and polyoxometalate attached to the hard carbon. Since the polyoxometalate ions have a special three-dimensional pore structure, it helps to improve the porosity inside the negative electrode material, so that after the composite negative electrode material is used in a sodium ion battery, sodium ions can be transmitted not only in the hard carbon micropores, but also in the polyoxometalate ions, which is beneficial to the sodium ions being deintercalated in the composite negative electrode material, and helps to improve the initial efficiency of the hard carbon negative electrode material of the sodium ion battery.

[0030] The preparation method of the composite negative electrode material provided by the present invention generates polyoxometalates in situ in a mixed solution containing hard carbon precursor powder through an acid-base neutralization reaction, so that the polyoxometalates are attached to functional groups in the hard carbon precursor powder, and then utilizes the special three-dimensional pore structure of the polyoxometalate ions to facilitate the embedding and deintercalation of sodium ions in the composite negative electrode material, thereby improving the initial efficiency of the composite negative electrode material.

[0031] Furthermore, the polyoxometallic acid of the present invention is preferably selected from H3XY 12 O 40 、H4XY 12 O 40 At least one of; wherein X is selected from any one of P and Si; Y is selected from any one of Mo and W, so that polymetallic acid ions are introduced into the composite negative electrode material through acid-base neutralization reaction to improve the initial efficiency of the composite negative electrode material, and rich heteroatoms can be introduced into the hard carbon to provide active sites to accelerate the reaction kinetics of the material, so that it has good physical and chemical properties and excellent conductivity.

[0032] In addition, the above-mentioned polyoxometallic acid has a stable structure and abundant resources, which can also help reduce the production cost of composite negative electrode materials.

[0033] At present, there are also schemes to introduce heteroatoms into hard carbon to increase active sites, but the existing preparation method is usually to immerse the hard carbon precursor in a solution containing a dopant and then dry it, so that the heteroatoms are added to the hard carbon. However, this preparation method directly introduces heteroatoms into the pores inside the hard carbon, which is bound to cause a certain blockage to the pores inside the hard carbon, thereby reducing the porosity inside the hard carbon, which is not conducive to the deintercalation of sodium ions therein, and inevitably affects the initial efficiency. The technical solution provided by the present invention, in the mixed solution where the hard carbon precursor powder exists, introduces abundant heteroatoms in situ in the form of polyoxometalates through an acid-base neutralization reaction in the hard carbon precursor powder, and utilizes the special three-dimensional pore structure of the polyoxometalate ions. It can provide active sites through heteroatoms while increasing the porosity inside the composite negative electrode material, which is conducive to the deintercalation of sodium ions. Compared with the prior art, it can improve the active sites of the composite negative electrode material on the basis of improving the initial efficiency.

[0034] Furthermore, the present invention prefers that the alkali metal sulfide is sodium sulfide, so that the generated polyoxometalate is sodium polyoxometalate. Therefore, the prepared composite negative electrode material includes hard carbon, and sodium polyoxometalate attached to the hard carbon functional group. Sodium ions are transported inside the polyoxometalate roots and in the hard carbon micropores. Before the composite negative electrode material is charged and discharged, a portion of sodium ions have entered the composite negative electrode material as "pre-sodium", thereby increasing the total amount of sodium ions in the battery, and having a certain supplementary effect on the sodium ions lost in the process of forming the SEI film, thereby helping to further improve the initial efficiency of the composite negative electrode material.

[0035] The preferred hard carbon precursor of the present invention is selected from at least one of bamboo, coconut shell, starch, walnut shell, anthracite, asphalt, and phenolic resin; wherein the preferred starch is selected from at least one of potato starch, corn starch, wheat starch, cassava starch, pea starch, and sweet potato starch.

[0036] In order to take into account both the initial efficiency and the conductive performance of the composite negative electrode material, the present invention preferably has a molar ratio of alkali metal sulfide to polymetallic acid of 1: (2-3) to ensure an excess of polymetallic acid; the mass ratio of alkali metal sulfide to hard carbon precursor powder is preferably 1: (8-10), and is further preferably 1:9.

[0037] Furthermore, the present invention preferably calcines the precursor composite material under an inert gas atmosphere, including: calcining the precursor composite material at 100-300° C. for 3-6 hours, and then calcining at 850-1400° C. for 4-6 hours under an inert gas atmosphere.

[0038] Another object of the present invention is to provide a composite negative electrode material, which is prepared by the method for preparing the composite negative electrode material as described above.

[0039] The composite negative electrode material provided by the present invention generates sodium polyoxometalate and hydrogen sulfide through acid-base neutralization reaction during the preparation process. Since polyoxometalate has strong oxidizing property and strong electron-withdrawing ability, and the hard carbon precursor contains abundant functional groups, the polyoxometalate generated in situ in the mixed solution containing hard carbon precursor powder is attached to the functional groups in the hard carbon precursor powder, and then the special three-dimensional pore structure of polyoxometalate ions is utilized to facilitate the embedding and de-embedding of sodium ions in the composite negative electrode material, thereby improving the initial efficiency of the composite negative electrode material.

[0040] Another object of the present invention is to provide a sodium ion battery, which comprises the composite negative electrode material as described above.

[0041] The sodium ion battery provided by the present invention adopts the composite negative electrode material as described above. During its preparation process, polyoxometalates are generated in situ in a mixed solution containing hard carbon precursor powder through an acid-base neutralization reaction, so that the polyoxometalates are attached to the functional groups in the hard carbon precursor powder. The special three-dimensional pore structure of the polyoxometalate ions is then utilized to facilitate the embedding and deintercalation of sodium ions in the composite negative electrode material, thereby improving the initial efficiency of the composite negative electrode material and further improving the initial efficiency of the sodium ion battery.

[0042] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below.

[0043] Example 1

[0044] This embodiment provides a method for preparing a composite negative electrode material, the preparation method comprising the following steps:

[0045] S1: Using deionized water as solvent, add 200 g corn starch into 2000 mL deionized water, then add 22 g (0.28 mol) sodium sulfide into the deionized water containing corn starch, stirring while adding to evenly mix the sodium sulfide and corn starch to obtain a mixed solution;

[0046] S2: 1624 g (0.56 mol) of polyoxometallic acid H3PW 12 O 40 Add to the mixture, stirring while adding, to make the polyoxometalate H3PW 12 O 40 Fully react with sodium sulfide to obtain a solid-liquid mixture. The reaction process is as follows:

[0047] 2H3P 12 O 40 + 3Na2S = 2Na3PW 12 O 40 + 3H2S;

[0048] S3: The solid-liquid mixture is centrifuged to separate the solid matter in the solid-liquid mixture, and the solid matter is vacuum dried at 85°C to remove the hydrogen sulfide and other substances generated by the reaction, and then ground to obtain Na3PW 12 O 40 Precursor composite materials;

[0049] S4: The ground Na3PW 12 O 40The precursor composite material was placed in a tube furnace and calcined at 160 ° C for 5 h in a nitrogen atmosphere to remove excess hydrogen sulfide and other substances inside the precursor. The resulting composite material was then placed in a box furnace and calcined at 1400 ° C for 5 h in a nitrogen atmosphere to obtain Na3PW, a hard carbon negative electrode material for sodium ion batteries with high coulombic efficiency. 12 O 40 -Hard carbon, i.e. composite negative electrode material.

[0050] Example 2

[0051] This embodiment provides a method for preparing a composite negative electrode material, the preparation method comprising the following steps:

[0052] S1: pulverizing coconut shell to obtain coconut shell powder; using deionized water as solvent, adding 200 g of coconut shell powder into 2000 mL of deionized water, and then adding 22 g (0.28 mol) of sodium sulfide into the deionized water containing the coconut shell powder, stirring while adding, so that the sodium sulfide and the coconut shell powder are evenly mixed to obtain a mixed solution;

[0053] S2: 1531 g (0.84 mol) of polyoxometalate H3PMo 12 O 40 Add to the mixture, stirring while adding, to make the polyoxometalate H3PMo 12 O 40 Fully react with sodium sulfide to obtain a solid-liquid mixture. The reaction process is as follows:

[0054] 2H3PMo 12 O 40 + 3Na2S = 2Na3PMo 12 O 40 + 3H2S;

[0055] S3: The solid-liquid mixture is centrifuged to separate the solid matter in the solid-liquid mixture, and the solid matter is vacuum dried at 85°C to remove the hydrogen sulfide and other substances generated by the reaction, and then ground to obtain Na3PMo 12 O 40 Precursor composite materials;

[0056] S4: The ground Na3PMo 12 O 40 The precursor composite material was placed in a tube furnace and calcined at 300°C for 3 hours in a nitrogen atmosphere to remove excess hydrogen sulfide and other substances inside the precursor. The resulting composite material was then placed in a box furnace and calcined at 1400°C for 6 hours in a nitrogen atmosphere to obtain Na3PMo, a hard carbon negative electrode material for sodium ion batteries with high coulombic efficiency. 12 O 40 -Hard carbon, i.e. composite negative electrode material.

[0057] Example 3

[0058] This embodiment provides a method for preparing a composite negative electrode material, the preparation method comprising the following steps:

[0059] S1: grinding the phenolic resin to obtain phenolic resin powder; using deionized water as a solvent, adding 200 g of the phenolic resin powder into 2000 mL of deionized water, and then adding 22 g (0.28 mol) of sodium sulfide into the deionized water containing the phenolic resin powder, stirring while adding, so that the sodium sulfide and the phenolic resin powder are evenly mixed to obtain a mixed solution;

[0060] S2: 1021 g (0.56 mol) of polyoxometalate H4SiMo 12 O 40 Add to the mixture, stirring while adding, to make the polyoxometalate H4SiMo 12 O 40 Fully react with sodium sulfide to obtain a solid-liquid mixture. The reaction process is as follows:

[0061] H4SiMo 12 O 40 + 2Na2S = Na4SiMo 12 O 40 + 2H2S;

[0062] S3: The solid-liquid mixture is centrifuged to separate the solid matter in the solid-liquid mixture, and the solid matter is vacuum dried at 85°C to remove the hydrogen sulfide and other substances generated by the reaction, and then ground to obtain Na4SiMo 12 O 40 Precursor composite materials;

[0063] S4: The ground Na4SiMo 12 O 40 The precursor composite material was placed in a tube furnace and calcined at 200°C for 5 hours in a nitrogen atmosphere to remove excess hydrogen sulfide and other substances inside the precursor. The resulting composite material was then placed in a box furnace and calcined at 1100°C for 5 hours in a nitrogen atmosphere to obtain Na4SiMo, a hard carbon negative electrode material for sodium ion batteries with high coulombic efficiency. 12 O 40 -Hard carbon, i.e. composite negative electrode material.

[0064] Example 4

[0065] This embodiment provides a method for preparing a composite negative electrode material, the preparation method comprising the following steps:

[0066] S1: Using deionized water as solvent, add 200 g corn starch into 2000 mL deionized water, then add 22 g (0.28 mol) sodium sulfide into the deionized water containing corn starch, stirring while adding to evenly mix the sodium sulfide and corn starch to obtain a mixed solution;

[0067] S2: 1611 g (0.56 mol) of polyoxometalate H4SiW 12 O 40 Add to the mixture, stirring while adding, to make the polyoxometalate H4SiW 12 O 40 Fully react with sodium sulfide to obtain a solid-liquid mixture. The reaction process is as follows:

[0068] HkDJ 12 O 40 + 2Na2S = Na4SiW 12 O 40 + 2H2S;

[0069] S3: The solid-liquid mixture is centrifuged to separate the solid matter in the solid-liquid mixture, and the solid matter is vacuum dried at 85°C to remove the hydrogen sulfide and other substances generated by the reaction, and then ground to obtain Na4SiW 12 O 40 Precursor composite materials;

[0070] S4: The ground Na4SiW 12 O 40 The precursor composite material was placed in a tube furnace and calcined at 100 ° C for 6 hours in a nitrogen atmosphere to remove excess hydrogen sulfide and other substances inside the precursor. The resulting composite material was then placed in a box furnace and calcined at 850 ° C for 6 hours in a nitrogen atmosphere to obtain Na4SiW, a hard carbon negative electrode material for sodium ion batteries with high coulombic efficiency. 12 O 40 -Hard carbon, i.e. composite negative electrode material.

[0071] Comparative Example 1

[0072] The corn starch was placed in a tube furnace without any treatment and calcined at 160°C for 5 hours in a nitrogen atmosphere. The resulting composite material was then placed in a box furnace and calcined at 1400°C for 5 hours in a nitrogen atmosphere to obtain a hard carbon negative electrode material for a sodium ion battery.

[0073] Comparative Example 2

[0074] This comparative example provides a method for preparing a composite negative electrode material, which comprises the following steps:

[0075] S1: Add 22 g (0.28 mol) of sodium sulfide into 2000 mL of deionized water, stir and mix well to obtain a mixed solution;

[0076] S2: 1624 g (0.56 mol) of polyoxometallic acid H3PW 12 O 40 Add to the mixture, stirring while adding, to make the polyoxometalate H3PW 12 O 40 Fully reacting with sodium sulfide to obtain a first solid-liquid mixture;

[0077] S3: adding 200 g corn starch to the solid-liquid mixture, stirring and mixing evenly to obtain a second solid-liquid mixture;

[0078] S3: The second solid-liquid mixture is centrifuged to separate the solid matter in the solid-liquid mixture, and the solid matter is vacuum dried at 85°C to remove the hydrogen sulfide and other substances generated by the reaction, and then ground to obtain a mixture of Na3PW 12 O 40 Precursor composite materials;

[0079] S4: The ground mixture is mixed with Na3PW 12 O 40 The precursor composite material is placed in a tubular furnace and calcined at 160°C for 5 hours in a nitrogen atmosphere to remove excess hydrogen sulfide and other substances inside the precursor. The resulting composite material is then placed in a box furnace and calcined at 1400°C for 5 hours in a nitrogen atmosphere to obtain a composite negative electrode material.

[0080] Comparative Example 3

[0081] This comparative example provides a method for preparing a composite negative electrode material, which comprises the following steps:

[0082] S1: Using deionized water as solvent, add 200 g corn starch into 2000 mL deionized water, then add 22 g (0.28 mol) sodium sulfide into the deionized water containing corn starch, stirring while adding to evenly mix the sodium sulfide and corn starch to obtain a mixed solution;

[0083] S2: Add 54.88 g (0.56 mol) of H3PO4 to the mixed solution, stirring while adding, so that H3PO4 and sodium sulfide react fully to obtain a solid-liquid mixture;

[0084] S3: centrifuging the solid-liquid mixture to separate the solid matter in the solid-liquid mixture, vacuum drying the solid matter at 85° C. to remove the hydrogen sulfide and other substances generated by the reaction, and then grinding to obtain a precursor composite material containing NaH2PO4;

[0085] S4: The ground NaH2PO4-containing precursor composite material is placed in a tubular furnace and calcined at 160°C for 5 hours in a nitrogen atmosphere to remove excess hydrogen sulfide and other substances inside the precursor. The resulting composite material is then placed in a box furnace and calcined at 1400°C for 5 hours in a nitrogen atmosphere to obtain a composite negative electrode material.

[0086] The composite negative electrode materials prepared in each embodiment and comparative example were used as negative electrode active materials, and were uniformly mixed with polyvinylidene fluoride (PVDF) (dissolved in N-methylpyrrolidone) and conductive carbon black in a mass ratio of 90:5:5, coated into an electrode film, and dried in a vacuum drying oven at 120°C for 12 hours. After rolling and punching, a hard carbon negative electrode sheet was obtained; a metal sodium sheet was used as a counter electrode, 1 mol / L NaPF6 (EC-DEC=1:1) was used as an electrolyte, and the hard carbon negative electrode sheets obtained above were assembled into 2430 button batteries in a glove box, and the current size was 0.5 mA / cm 2 , and tested its electrochemical performance. The test results are shown in Table 1:

[0087] Table 1

[0088] Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Gram capacity (mAh / g) 263.5 260.2 271.5 286.9 268.4 265.6 264.7 First coulombic efficiency 89.3% 88.5% 89.7% 88.5% 82.2% 85.9% 81.3%

[0089] It can be seen from the data in the above table that compared with the solution in Example 1 in which no treatment is performed on the corn starch, the gram capacity and the first coulombic efficiency of the technical solution provided by the present invention are significantly improved; although Example 2 also introduces polymetallic acid ions by reacting sodium sulfide with polymetallic oxoacids, because the polymetallic acid salts are generated separately during the preparation process and then mixed with the hard carbon precursor powder, the polymetallic acid ions are difficult to adhere to the inside of the hard carbon, resulting in a low first coulombic efficiency of the prepared composite negative electrode material; in Example 3, dihydrogen phosphate ions are introduced by in-situ reaction of sodium sulfide and phosphoric acid in the presence of hard carbon precursor powder. After calcination, although phosphorus element is introduced into the composite negative electrode material, phosphorus element itself does not have the ability of polymetallic oxoacids and cannot fix sodium ions, so its first coulombic efficiency is not ideal.

[0090] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A method for preparing a composite negative electrode material, characterized in that: The steps include: S1: uniformly mixing alkali metal sulfide and hard carbon precursor powder in water to obtain a mixed solution; S2: adding polyoxometallic acid to the mixed solution under stirring conditions to obtain a solid-liquid mixture; S3: separating the solid matter from the solid-liquid mixture, vacuum drying and grinding the solid matter to obtain a precursor composite material; S4: calcining the precursor composite material under an inert gas atmosphere to obtain a composite negative electrode material; The alkali metal sulfide is sodium sulfide; The hard carbon precursor is selected from at least one of bamboo, coconut shell, starch, walnut shell, anthracite, asphalt, and phenolic resin; The molar ratio of the alkali metal sulfide to the polyoxometallic acid is 1:(2-3); The mass ratio of the alkali metal sulfide to the hard carbon precursor powder is 1:(8-10).

2. The method for preparing a composite negative electrode material according to claim 1, characterized in that: The polyoxometallic acid is selected from H3XY 12 O 40 、H4XY 12 O 40 At least one of; wherein X is selected from any one of P and Si; Y is selected from any one of Mo and W.

3. The method for preparing the composite negative electrode material according to claim 1, characterized in that: The starch is selected from at least one of potato starch, corn starch, wheat starch, tapioca starch, pea starch and sweet potato starch.

4. The method for preparing a composite negative electrode material according to any one of claims 1 to 3, characterized in that: The step of calcining the precursor composite material under an inert gas atmosphere includes: calcining the precursor composite material at 100-300° C. for 3-6 hours, and then calcining at 850-1400° C. for 4-6 hours under an inert gas atmosphere.

5. A composite negative electrode material, characterized in that: The composite negative electrode material is prepared by the method for preparing the composite negative electrode material according to any one of claims 1 to 4.

6. A sodium ion battery, characterized in that: Comprising the composite negative electrode material as claimed in claim 5.